Decorative sheet and method for manufacturing decorative sheet
By optimizing the concave and convex shape and material structure of the surface protective layer and using ionizing radiation curable resin, the problem of reducing fingerprint resistance and injury resistance caused by excessive addition of gloss regulators in the prior art is solved, and low gloss and high Durable decorative sheets have good processability and pollution resistance.
Patent Information
- Application Number
- CN202380030434.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-12
AI Technical Summary
When the existing decorative sheets pursue low gloss and high durability, excessive addition of gloss regulators leads to difficult removal of fingerprint dirt, reduced damage resistance, poor bending processability, and the surface protective layer is too hard and easy to break.
By optimizing the concave and convex shape and material structure of the surface protective layer, using ionizing radiation curable resin as the main material to form a surface protective layer of the ridge and core. The Martensite hardness is above 20N/mm2 and below 200N/mm2 and RSm/Ra Between 10 and 300 or less, the gloss is ensured, and the fingerprint resistance, pollution resistance and processability are achieved.
Decorative sheets with a gloss of less than 15 have excellent fingerprint resistance, high durability and good processability, and avoid cracking problems caused by the hard surface protective layer.
Smart Images

Figure CN118946459A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a decorative sheet used for interior and exterior decoration of buildings, surface decoration of doors and windows, furniture, construction materials, floor materials, etc., and a method for manufacturing the decorative sheet. Background Art
[0002] In the above-mentioned buildings, in order to give the surface of the decorative sheet design and durability, it is generally made into a decorative board by sticking it on the surface of wood, wooden board, metal board, non-combustible board, paper substrate or resin substrate through an adhesive, and is widely used.
[0003] Regarding the design, we can choose from various printing methods to create patterns such as wood grain or stone grain, or plain color surfaces without patterns, depending on the requirements and use. Similarly, the glossiness of the surface is also an important factor in design, and we can choose from high gloss like a mirror surface to low gloss without any reflection, depending on the requirements and use.
[0004] In addition, as mentioned above, the function of the decorative sheet that is equally important as the design is to impart durability. Durability is a comprehensive evaluation of scratch resistance and stain resistance, and whether these properties can be ensured continuously for a long time. The requirements vary depending on the environment and conditions in which the decorative sheet is used, but a decorative sheet with high performance is always required.
[0005] In order to impart durability, a surface protection layer is generally formed on the outermost surface of the decorative sheet. In addition, in order to adjust the glossiness, especially to achieve low glossiness, a gloss adjuster (matt additive) is generally added to the surface protection layer.
[0006] Furthermore, since the decorative sheet is generally subjected to processing such as cutting and bending in order to form a decorative plate or a decorative material, it is preferable that the decorative sheet has processability that can withstand such processing.
[0007] As described above, as a decorative sheet that takes design properties (low gloss), scratch resistance, and stain resistance into consideration, there is a decorative sheet described in Patent Document 1, for example.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2019-119138 Summary of the invention
[0011] Problems to be solved by the invention
[0012] In recent years, as the use of decorative plates using decorative sheets has expanded and consumers have become more aware of quality, glossiness of 15 or less and fingerprint resistance, scratch resistance, stain resistance, and processability are required.
[0013] In response to the above requirements, there is a method of adding a gloss regulator to roughen the surface for gloss adjustment. However, due to the large amount of addition, the following undesirable conditions will occur. (1) Fingerprint dirt is difficult to remove, and fingerprint resistance is reduced. (2) The gloss regulator is detached during the scratch resistance test, and the scratch resistance is reduced. (3) Dirt is difficult to remove, and the stain resistance is reduced. (4) During bending, whitening occurs due to the gloss regulator, and the bending processability is reduced. In particular, with regard to processability, in order to improve scratch resistance, by increasing the crosslinking density of the resin used in the surface protection layer, (5) the sheet curls significantly due to curing shrinkage, and tends to be difficult to laminate to the substrate. In addition, (6) the surface protection layer becomes too hard, so the decorative sheet tends to crack.
[0014] In order to solve the above problems, the purpose of the present invention is to provide a decorative sheet and a method for producing the same which has low gloss, i.e., excellent design, fingerprint resistance, high durability (especially scratch resistance and stain resistance), and processability (easy to laminate to a substrate and difficult to crack).
[0015] Means for solving problems
[0016] The inventors have found that by optimizing the concavo-convex shape of the surface protective layer and further repeatedly experimenting with the materials used for the surface protective layer to find the necessary structural elements, it is possible to provide a decorative sheet with a glossiness of 15 or less and exhibiting fingerprint resistance, high durability (especially scratch resistance and stain resistance) and processability (easy to laminate to a substrate and difficult to crack).
[0017] In order to solve the problem, the gist of the decorative sheet involved in one embodiment of the present invention is that it has a raw material layer and a surface protective layer arranged on one surface of the raw material layer, the glossiness of the surface protective layer is less than 15, the surface protective layer has a ridge portion arranged in a ridge-like protrusion on its surface, and is formed with a concave-convex shape, the main material of the surface protective layer is an ionizing radiation curable resin, the main component of the ionizing radiation curable resin is a tetrafunctional acrylic resin containing a repeating structure, the number of repetitions of the repeating structure is 12 or more, and the Martens hardness of the surface protective layer is 20N / mm 2 Above 200N / mm 2 In the following range, RSm / Ra of the concavo-convex shape of the surface protection layer is in the range of 10 or more and 300 or less.
[0018] Effects of the Invention
[0019] According to one embodiment of the present invention, a decorative sheet having a glossiness of 15 or less and having fingerprint resistance, scratch resistance, stain resistance, and processability can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] [ Figure 1 ] is a schematic cross-sectional view illustrating the structure of the decorative sheet involved in an embodiment of the present invention.
[0021] [ Figure 2 ] is a schematic cross-sectional view illustrating a structure of a surface protection layer of a decorative sheet involved in an embodiment of the present invention.
[0022] [ Figure 3 ] is a plan photograph showing a structural example of the surface of the surface protection layer of the decorative sheet involved in an embodiment of the present invention.
[0023] [ Figure 4 ] is a schematic cross-sectional view illustrating the cross-sectional shape of the ridge portion involved in an embodiment of the present invention.
[0024] [ Figure 5 ] is a schematic diagram illustrating the temporal variation of the irradiation light amount of each irradiation light in the manufacturing process of the decorative sheet involved in an embodiment of the present invention.
[0025] [ Figure 6 ] is a schematic cross-sectional view illustrating the measurement method of the curling test. DETAILED DESCRIPTION
[0026] Hereinafter, the configuration of a decorative sheet according to an embodiment of the present invention will be described with reference to the drawings.
[0027] Here, the drawings are schematic, and the relationship between thickness and plane size, the ratio of thickness of each layer, etc. are different from the actual situation. In addition, the embodiments shown below illustrate the configuration for concretizing the technical idea of the present invention, and the technical idea of the present invention can be variously modified within the technical scope specified by the claim items recorded in the claims.
[0028] (constitute)
[0029] like Figure 1 As shown, the decorative sheet 1 of this embodiment is composed of a pattern layer 3, an adhesive layer 7 (thermosensitive adhesive layer, anchor coating, dry lamination adhesive layer), a transparent resin layer 4 and a surface protection layer 5 stacked in sequence on one side, i.e., the surface side, of the raw material layer (base material layer) 2. In addition, a concealing layer 8 and a primer layer 6 are provided on the other side, i.e., the back side, of the raw material layer 2. The pattern layer 3, the adhesive layer 7, the transparent resin layer 4, the concealing layer 8 and the primer layer 6 may also be omitted.
[0030] Then, if Figure 1 As shown, the decorative sheet 1 of this embodiment is attached to a substrate B to form a decorative material 11. The substrate B is not particularly limited, and may be made of, for example, a wooden board, an inorganic board, a metal board, or a composite board made of a plurality of materials.
[0031] <Raw material layer 2>
[0032] As the raw material layer 2, for example, a material selected arbitrarily from paper, synthetic resin, or synthetic resin foam, rubber, non-woven fabric, synthetic paper, metal foil, etc. can be used. As paper, thin leaf paper, titanium paper, resin-impregnated paper, etc. can be exemplified. As synthetic resin, polyethylene, polypropylene, polybutene, polystyrene, polycarbonate, polyester, polyamide, ethylene-vinyl acetate copolymer, polyvinyl alcohol, acrylic acid, etc. can be exemplified. As rubber, ethylene-propylene copolymer rubber, ethylene-propylene-diene copolymer rubber, styrene-butadiene copolymer rubber, styrene-isoprene-styrene block copolymer rubber, styrene-butadiene-styrene block copolymer rubber, polyurethane, etc. can be exemplified. As non-woven fabric, organic or inorganic non-woven fabric can be used. As metal of metal foil, aluminum, iron, gold, silver, etc. can be exemplified.
[0033] When an olefin resin is used as the raw material layer 2, since the surface of the raw material layer 2 is mostly inert, it is preferred to provide a primer layer 6 between the raw material layer 2 and the substrate B. In addition, in order to improve the adhesion between the raw material layer 2 composed of an olefin material and the substrate B, the raw material layer 2 may be subjected to surface modification treatments such as corona treatment, plasma treatment, ozone treatment, electron beam treatment, ultraviolet treatment, and dichromic acid treatment.
[0034] As the primer layer 6, the same material as the pattern layer 3 described later can be used. Since the primer layer 6 is applied to the back side of the decorative sheet 1, when the decorative sheet 1 is wound in a web shape, in order to avoid sticking and improve the adhesion with the adhesive, an inorganic filler can be added to the primer layer 6. Examples of the inorganic filler include silicon dioxide, aluminum oxide, magnesium oxide, titanium oxide, barium sulfate, and the like.
[0035] Taking printing workability, cost, and the like into consideration, the thickness of the original material layer 2 is preferably within a range of 20 μm to 250 μm.
[0036] <Pattern layer 3>
[0037] The pattern layer 3 is a pattern printing layer obtained by applying ink to the raw material layer 2. As a binder for the ink, for example, it can be appropriately selected and used from each or each modified substance such as nitrocellulose, cellulose, vinyl chloride-vinyl acetate copolymer, polyvinyl butyral, polyurethane, acrylic, polyester, etc. The binder can be any of water-based, solvent-based, and emulsion-based, and can also be a one-component type or a two-component type using a curing agent. In addition, a method of using a curable ink and curing the ink by irradiation with ultraviolet rays or electron beams can also be adopted. Among them, the most common method is a method of using a carbamate-based ink and curing it by isocyanate. For the pattern layer 3, in addition to the binder, for example, colorants such as pigments and dyes contained in ordinary inks, body pigments, solvents, various additives, etc. can be added. As pigments with high versatility, for example, pearl pigments such as condensed azo, insoluble azo, quinacridone, isoindoline, anthraquinone, imidazolones, cobalt, phthalocyanine, carbon, titanium oxide, iron oxide, and mica can be listed.
[0038] In addition to ink coating, the pattern layer 3 can also be designed by vapor deposition or sputtering of various metals. In particular, it is preferable to add a light stabilizer to the ink, thereby suppressing the degradation of the decorative sheet 1 itself caused by light degradation of the ink and extending the life of the decorative sheet 1.
[0039] <Adhesive layer 7>
[0040] The adhesive layer 7 is also called a heat-sensitive adhesive layer, an anchor coating layer, or a dry lamination adhesive layer.
[0041] The resin material of the adhesive layer 7 is not particularly limited, and for example, it can be appropriately selected and used from resin materials such as acrylic acid, polyester, polyurethane, and epoxy. In addition, as the resin material of the adhesive layer 7, for example, an ethylene-vinyl acetate copolymer resin adhesive can also be used. The coating method can be appropriately selected according to the viscosity of the adhesive, etc., and a gravure coater is usually used. After being coated on the pattern layer 3 by the gravure coater, it is laminated with the transparent resin layer 4. It should be noted that, when the bonding strength between the transparent resin layer 4 and the pattern layer 3 is fully obtained, the adhesive layer 7 can be omitted.
[0042] <Transparent resin layer 4>
[0043] As the resin material of the transparent resin layer 4, an olefin resin is preferably used. As the olefin resin, for example, in addition to polypropylene, polyethylene, polybutene, etc., alpha olefins (for example, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1 Polymers obtained by homopolymerization of ethylene-1-olefins or copolymerization of two or more monomers such as ethylene-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, 12-ethyl-1-tetradecene, etc.; copolymers obtained by copolymerizing ethylene or α-olefins with other monomers such as ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, ethylene-methyl methacrylate copolymers, ethylene-ethyl methacrylate copolymers, ethylene-butyl methacrylate copolymers, ethylene-methyl acrylate copolymers, ethylene-ethyl acrylate copolymers, and ethylene-butyl acrylate copolymers.
[0044] In addition, in order to improve the surface strength of the decorative sheet 1, highly crystalline polypropylene is preferably used as the resin of the transparent resin layer 4. It should be noted that various additives such as (for example) heat stabilizers, light stabilizers, anti-blocking agents, catalyst scavengers, colorants, light scattering agents, and gloss regulators may be added to the transparent resin layer 4 as needed. As heat stabilizers, phenolic, sulfur, phosphorus, hydrazine, etc. are generally added in any combination, and as light stabilizers, hindered amines, etc. are generally added in any combination.
[0045] <Surface protection layer 5>
[0046] The surface protection layer 5 has a core portion 5A and a ridge portion 5B provided to protrude in a ridge shape from one surface of the core portion 5A. Thus, a concavo-convex shape is formed on the surface of the surface protection layer 5.
[0047] Here, in the decorative sheet 1 according to the present embodiment, "ridge" refers to a shape that is slenderly raised and connected in a linear shape in a plan view. The ridge portion 5B may be curved or linear in a plan view, but is preferably curved from the viewpoint of the anti-fingerprint property of the surface of the decorative sheet 1. In the present disclosure, the ridge portion 5B is, for example, a portion from the lowest part to the top of the concave-convex shape provided on the surface of the surface protection layer 5, and the core portion 5A refers to the portion of the surface protection layer 5 other than the ridge portion 5B.
[0048] Figure 22 is a cross-sectional view schematically showing a cross section of a ridge portion 5B of the surface protection layer 5 (a cross section in the thickness direction of the surface protection layer 5 ). Figure 3 : is a plan view showing the structure of the surface of the surface protection layer 5. Here, Figure 3 This is a plane photograph obtained using a laser microscope (OLS-4000 manufactured by Olympus Corporation).
[0049] like Figure 3 As shown in the plan view of FIG. 1 , the ridge 5B is a shape that is elongated and connected in a linear manner in a plan view. As described later, the ridge 5B is formed by irradiating the surface of the ionizing radiation curing resin with light of a specific wavelength to shrink the surface of the ionizing radiation curing resin.
[0050] The shape of the ridge 5B can be determined by the lateral direction (the plane direction of the surface protection layer 5). Figure 2 The surface roughness index RSm (μm) of the longitudinal direction (the depth direction of the ridge 5B, the thickness direction of the surface protection layer 5) is Figure 2 The ratio of the surface roughness index Ra (μm) (in the vertical direction) RSm / Ra is expressed, and RSm / Ra is 10 to 300. More preferably, it is 50 to 300. When RSm / Ra is less than 10, it is difficult to wipe off dirt because the shape of the ridge 5B is too fine, and the contamination resistance is deteriorated. When RSm / Ra is greater than 300, the ridge interval is too wide, so it does not have low gloss.
[0051] In addition, RSm / Ra is more preferably 100 to 300. When RSm / Ra is within this numerical range, the intervals between the ridges are appropriately wide, so the affinity for water or detergent (water containing a surfactant or alcohol) is improved. Therefore, when the decorative sheet has RSm / Ra within this numerical range, even if the surface of the decorative sheet is contaminated, it is easy to wipe the dirt with water or detergent.
[0052] RSm / Ra is most preferably 100 to 250. When RSm / Ra is within this numerical range, a general commercial cleaning sponge can easily enter between the ridges, and even when the surface of the decorative sheet is contaminated, the dirt can be easily wiped off with the general commercial cleaning sponge.
[0053] In addition, RSm (μm) can be 50 to 400, preferably 80 to 300. If RSm (μm) is within this numerical range, the intervals between the ridges are appropriately wide, so the affinity for water or detergent (water containing a surfactant or alcohol) is improved. Therefore, if the decorative sheet has RSm (μm) within this numerical range, even if the surface of the decorative sheet is contaminated, it is easy to wipe the dirt with water or detergent.
[0054] In addition, Ra (μm) may be 0.3 to 10, preferably 0.5 to 10, and more preferably 0.8 to 5. If Ra (μm) is within this numerical range, a general commercially available cleaning sponge can easily enter between the ridges, and even if the surface of the decorative sheet is contaminated, it is easy to wipe the dirt with a general commercially available cleaning sponge.
[0055] Here, Ra and RSm are measured values when measured using a line roughness meter (in accordance with JIS B0601).
[0056] The cross-sectional shape of the surface protection layer 5 in the thickness direction of the ridge portion 5B may be a sinusoidal wave shape.
[0057] Here, if Figure 4 As shown in FIG. 1 , the “sine wave shape” means that the shape of a line from the lowest position C to the highest position (apex) D of the ridge portion 5B can be expressed by a sine wave.
[0058] Next, the mechanism of forming the ridge portion 5B will be described.
[0059] When acrylate is irradiated with light having a wavelength of 200 nm or less as the first irradiation light, acrylate can be self-excited. Therefore, by irradiating acrylate with light having a wavelength of 200 nm or less, acrylate can be cross-linked. Light having a wavelength of 200 nm or less reaches a depth of about tens to hundreds of nm in acrylate. Therefore, only the surface is cross-linked, and the portion below it still has fluidity, thus generating fine concavo-convex shapes connected in a wave shape like folded folds.
[0060] In the surface protection layer 5 formed in this way, there is no interface between the core portion 5A and the ridge portion 5B, and the core portion 5A and the ridge portion 5B are formed in a state of being integrally continuous.
[0061] Light below 200 nm is absorbed by oxygen in the atmosphere and is greatly attenuated. Therefore, when processing acrylate, it is necessary to introduce nitrogen to control the reaction atmosphere. The residual oxygen concentration in the reaction atmosphere is preferably suppressed to less than 2000 ppm. The residual oxygen concentration in the reaction atmosphere is more preferably less than 1000 ppm.
[0062] In order to generate the concavoconvex shape by using the light with a wavelength of 200 nm or less as the first irradiation light, the integrated light amount of the first irradiation light is preferably set to 0.5 mJ / cm 2 Above 200mJ / cm 2 The cumulative light intensity is more preferably 1 mJ / cm 2 Above 100mJ / cm 2 The cumulative light intensity is more preferably 3 mJ / cm 2 Above 50mJ / cm 2 The most preferred cumulative light intensity is 5 mJ / cm 2 Above 30mJ / cm 2 When the accumulated light intensity is less than 0.5mJ / cm 2 In the case of , the curing shrinkage reaction is weak and the concavo-convex shape cannot be fully formed, so the gloss will not be reduced. 2 In this case, the curing shrinkage reaction becomes too strong and the surface condition deteriorates.
[0063] Light below 200nm can be extracted from excimer VUV light. Excimer VUV light can be generated by a lamp of a rare gas or a rare gas halide. When electrons with high energy are applied from the outside to a lamp enclosing a gas of a rare gas or a rare gas halide, a large amount of discharge plasma (dielectric barrier discharge) is generated. Through this plasma discharge, the atoms of the discharge gas (rare gas) are excited and instantly become an excimer state. When returning to the ground state from the excimer state, light of a wavelength region unique to the excimer is emitted.
[0064] The gas used for the excimer lamp can be any gas used in the past as long as it emits light below 200nm. As the gas, rare gases such as Xe, Ar, and Kr, and mixed gases of rare gases such as ArBr and ArF and halogen gases can be used. The wavelength (center wavelength) of the excimer lamp varies depending on the gas, for example, it has a wavelength of about 172nm (Xe), about 126nm (Ar), about 146nm (Kr), about 165nm (ArBr), about 193nm (ArF), etc.
[0065] However, considering the size of the photon energy obtained, the difference in wavelength and the binding energy of the organic matter, it is preferred to use a xenon lamp as a light source that emits excimer light with a central wavelength of 172nm. In addition, if the cost and material acquisition etc. spent on equipment maintenance are also considered, it is preferred to use a xenon lamp as a light source.
[0066] Since the light with a wavelength of 200 nm or less as the first irradiation light can only reach a depth of about tens to hundreds of nm from the outermost surface in the acrylic, the inside of the surface protection layer 5 having the ridge 5B formed by irradiation with light of 200 nm or less still has fluidity, and a curing reaction must be further performed. In order to cure the surface protection layer 5 after irradiation with light of 200 nm or less, ionizing radiation or UV light with a longer wavelength than the first irradiation light, i.e., light with a wavelength of 200 nm or less, can be used as the second irradiation light.
[0067] It should be noted that in the present embodiment, for example, after the irradiation of the second irradiation light, ionizing radiation of a different type from the second irradiation light or UV light having a longer wavelength than the second irradiation light may be irradiated as the third irradiation light, but it is preferred that the surface protection layer 5 having the ridge portion 5B is formed by irradiating only the first irradiation light and the second irradiation light. It should be noted that the third irradiation light may be irradiated in the case where the strength of the surface protection layer 5 is insufficient when only the second irradiation light is irradiated.
[0068] In order to cure the entire surface protection layer 5 by irradiating the second irradiation light, the integrated light amount of the second irradiation light is preferably set to 10 mJ / cm 2 Above 500mJ / cm 2 The cumulative light intensity is more preferably 50 mJ / cm 2 Above 400mJ / cm 2 The cumulative light intensity is more preferably 100 mJ / cm 2 Above 300mJ / cm 2 When the accumulated light intensity is less than 10mJ / cm 2 In the case of , the curing reaction is weak and sufficient strength cannot be given to the entire surface protection layer 5, so the scratch resistance tends to decrease. In addition, when the cumulative light amount is greater than 500mJ / cm 2 In the case of , the curing reaction becomes too strong and the surface state tends to deteriorate.
[0069] In addition, the cumulative light amount of the second irradiation light is preferably greater than the cumulative light amount of the first irradiation light. The cumulative light amount of the second irradiation light is preferably 1.1 times or more and 50.0 times or less of the cumulative light amount of the first irradiation light, and more preferably 5.0 times or more and 30.0 times or less. When the cumulative light amount of the second irradiation light is less than 1.1 times the cumulative light amount of the first irradiation light, the curing reaction is weak and sufficient strength may not be given to the entire surface protection layer 5. In addition, when the cumulative light amount of the second irradiation light exceeds 50.0 times the cumulative light amount of the first irradiation light, the curing reaction of the entire surface protection layer 5 becomes too strong, and the shape of the ridge 5B may be deformed.
[0070] Below, refer to Figure 5The temporal change in the irradiation light amount of the first irradiation light and the temporal change in the irradiation light amount of the second irradiation light will be described.
[0071] Figure 5 It is a diagram schematically showing the time change of the irradiation light amount of the first irradiation light and the time change of the irradiation light amount of the second irradiation light.
[0072] Figure 5 (a), (c), (e), (g), and (i) are diagrams schematically showing the temporal change in the irradiation light amount of the first irradiation light. Figure 5 (b), (d), (f), (h), and (j) are diagrams schematically showing the temporal change in the irradiation light amount of the second irradiation light.
[0073] like Figure 5 As shown in (a), the irradiation light intensity of the first irradiation light may gradually increase as the irradiation time elapses, and then gradually decrease as the irradiation time elapses. Figure 5 As shown in (c), the irradiation light intensity of the first irradiation light may also gradually decrease as the irradiation time elapses. Figure 5 As shown in (e), the irradiation light intensity of the first irradiation light may also gradually increase as the irradiation time elapses. Figure 5 As shown in (g), the irradiation light intensity of the first irradiation light may gradually decrease as the irradiation time elapses, and then gradually increase as the irradiation time elapses. Figure 5 As shown in (i), the irradiation light amount of the first irradiation light may be constant from the start of irradiation to the end of irradiation.
[0074] like Figure 5 As shown in (b), the irradiation light intensity of the second irradiation light may gradually increase as the irradiation time elapses, and then gradually decrease as the irradiation time elapses. Figure 5 As shown in (d), the irradiation light intensity of the second irradiation light may also gradually decrease as the irradiation time elapses. Figure 5 As shown in (f), the irradiation light intensity of the second irradiation light may also gradually increase as the irradiation time elapses. Figure 5 As shown in (h), the irradiation light intensity of the second irradiation light may gradually decrease as the irradiation time elapses, and then gradually increase as the irradiation time elapses. Figure 5 As shown in (j), the irradiation light amount of the second irradiation light may be constant from the start of irradiation to the end of irradiation.
[0075] In addition, in this embodiment, Figure 5 The irradiation mode of the first irradiation light shown in (a), (c), (e), (g) and (i) is the same as Figure 5The irradiation methods of the second irradiation light shown in (b), (d), (f), (h) and (j) may be used in combination as appropriate. Figure 5 (a) The irradiation mode of the first irradiation light and Figure 5 (f) The second irradiation light irradiation method shown in FIG. Figure 5 (g) The irradiation mode of the first irradiation light and Figure 5 It should be noted that when the value of RSm / Ra is set to 10 or more and 300 or less, it is more preferable to set Figure 5 (c) The irradiation mode of the first irradiation light and Figure 5 The irradiation method of the second irradiation light shown in (f) is used in combination.
[0076] As described above, the ridge 5B formed by irradiating light with a wavelength of 200 nm or less has a fine structure compared to the concavo-convex shape formed by mechanical processing such as embossing on the surface of the surface protection layer 5. By forming such a fine concavo-convex shape on the surface of the surface protection layer 5, the anti-fingerprint property can be improved while maintaining the matte feeling of the surface of the decorative sheet 1.
[0077] The surface protection layer 5 has a Martens hardness of 20N / mm 2 Above 200N / mm 2 The resin layer is preferably 50N / mm 2 Above 150N / mm 2 Below, more preferably 80N / mm 2 Above 150N / mm 2 The Martens hardness of the surface protection layer 5 is less than 20 N / mm 2 In the case of, the scratch resistance is reduced, so it is not preferred. In addition, the Martens hardness of the surface protection layer 5 is greater than 200N / mm 2 In the case of a coating that is too hard, the sheet will curl up significantly due to shrinkage during curing, making it difficult to laminate to the substrate during processing; or the coating will harden, causing the decorative sheet to break when pasted and transported during processing, resulting in a decrease in yield, which is not preferred. In addition, the coating will harden and the scratch resistance based on the Hoffman scratch test will also deteriorate, which is not preferred. Here, the above-mentioned Martens hardness may also be the Martens hardness of the ionizing radiation curing resin constituting the surface protection layer 5. That is, as the ionizing radiation curing resin constituting the surface protection layer 5, it is preferred to use a Martens hardness of 20N / mm 2 Above 200N / mm 2 The following resins are more preferably used 50N / mm 2 Above 150N / mm 2 The following resins are preferably used: 80 N / mm 2Above 150N / mm 2 Specifically, as the resin constituting the surface protection layer 5, for example, a tetrafunctional acrylic resin containing any one of ethylene oxide, propylene oxide and ε-caprolactone as a repeating structure is used, and the Martens hardness of the surface protection layer 5 is preferably 20N / mm 2 Above 200N / mm 2 Below, more preferably 50N / mm 2 Above 150N / mm 2 Below, more preferably 80N / mm 2 Above 150N / mm 2 the following.
[0078] The Martens hardness value can be arbitrarily adjusted by selecting the type or molecular weight of the ionizing radiation curable resin constituting the surface protection layer 5. When the surface protection layer 5 is composed of a plurality of resins, the Martens hardness value can be arbitrarily adjusted by adjusting the content ratio of the constituent resins.
[0079] In addition, when the surface protection layer 5 is formed of multiple layers, the Martens hardness of the uppermost layer of the surface protection layer 5 may be set within the above numerical range, or the Martens hardness of the lowermost layer of the surface protection layer 5 may be set within the above numerical range. Alternatively, the Martens hardness value may gradually decrease or increase from the uppermost layer toward the lowermost layer of the surface protection layer 5.
[0080] It should be noted that the Martens hardness specified in the present embodiment is a value measured according to the method of ISO 14577. In addition, the Martens hardness specified in the present embodiment is an average value of values measured at 10 randomly determined locations in the same sample.
[0081] The thickness of the surface protection layer 5 is preferably set within a range of 2 μm to 20 μm. The thickness of the surface protection layer 5 is more preferably within a range of 3 μm to 20 μm. The thickness of the surface protection layer 5 is further preferably within a range of 5 μm to 15 μm. The thickness of the surface protection layer 5 is most preferably within a range of 5 μm to 12 μm. When the thickness of the surface protection layer 5 is set to less than 2 μm, deep forming cannot be performed by shaping with vacuum ultraviolet light, and low gloss cannot be achieved. In addition, when the thickness of the surface protection layer 5 is set to greater than 20 μm, processability is reduced and whitening occurs during bending.
[0082] The thickness of the surface protection layer 5 is preferably set so that the ratio of the thickness of the ridge portion 5B to the thickness of the core portion 5A (thickness of the ridge portion 5B / thickness of the core portion 5A) is greater than 0.01 and less than 2.0, and more preferably greater than 0.1 and less than 1.0.
[0083] Here, the pattern layer 3 and the surface protection layer 5 can be formed by various printing methods such as gravure printing, offset printing, screen printing, electrostatic printing, inkjet printing, etc. In addition, since the surface protection layer 5 covers the entire surface side of the raw material layer 2, it can also be formed by various coating methods such as roller coating, blade coating, micro gravure coating, die coating, etc. These printing methods or coating methods can be selected separately according to the layers to be formed, or the same method can be selected for processing.
[0084] From the viewpoint of design, the pattern layer 3 and the surface protection layer 5 can be synchronized. In the case of synchronization, the surface protection layer 5 needs to be formed together after the pattern layer 3 is formed, so it is preferable to use the gravure printing method. In addition, since the gravure printing method can be printed at a relatively high speed, it is also advantageous in terms of cost and is preferred. Here, synchronization means that more than 50%, preferably more than 70%, and most preferably more than 90% of the portion where the surface protection layer 5 is formed overlaps with the pattern portion of the pattern layer 3 in a plan view.
[0085] In order to adjust the thickness of the surface protection layer 5, the coating amount can be adjusted in the above-mentioned printing method and coating method. In various printing methods and coating methods, the coating amount can be calculated based on the quality difference between the decorative sheet formed with the surface protection layer and the decorative sheet without the surface protection layer on the substrate (raw material layer).
[0086] The main material of the surface protection layer 5 is an ionizing radiation curable resin. Here, the main material refers to: relative to 100 parts by mass of the surface protection layer, it contains 60 parts by mass or more, more preferably 70 parts by mass or more, and most preferably 80 parts by mass or more of the material. As the ionizing radiation curable resin constituting the surface protection layer 5, various monomers or commercially available oligomers and other known resins can be used, for example, (meth) acrylic resins, silicone resins, polyester resins, carbamate resins, amide resins, epoxy resins can be used. The ionizing radiation curable resin can be any of a water-based resin or a non-aqueous (organic solvent-based) resin.
[0087] The main component of the ionizing radiation curable resin constituting the surface protection layer 5 is a tetrafunctional acrylate resin containing a repeating structure. As a tetrafunctional acrylate resin, for example, pentaerythritol tetraacrylate or the like can be used. Here, the main component refers to: relative to 100 parts by mass of the constituent resin components, it contains more than 60 parts by mass, more preferably more than 70 parts by mass, and most preferably more than 80 parts by mass. In the case of an acrylate resin with less than 3 functions, the degree of crosslinking is insufficient and the scratch resistance is reduced, so it is not preferred. In the case of an acrylate resin with more than 5 functions, the degree of crosslinking becomes too high and the processability is reduced, so it is not preferred.
[0088] When gravure printing is used as the coating method, the preferred viscosity range of the ionizing radiation curable resin is 10 to 500 mPa·s, and the optimal viscosity range is 50 to 300 mPa·s. In order to adjust the viscosity, an organic solvent or a low-viscosity bifunctional acrylate resin can be added. However, from the perspective of environmental load, it is preferred not to use an organic solvent. When the amount of bifunctional acrylate resin added is large, the scratch resistance decreases, so it is not preferred. Therefore, when the bifunctional acrylate resin is added to the quadrifunctional acrylate resin and used, the content of the bifunctional acrylate resin is preferably in the range of 10% to 30% by mass of the content (mass) of the quadrifunctional acrylate resin, and more preferably in the range of 15% to 20% by mass.
[0089] The viscosity of the ionizing radiation curable resin may be in the range of 10 to 80 mPa·s, preferably 10 to 50 mPa·s. If the viscosity of the ionizing radiation curable resin is in this numerical range, the versatility of the coating method is improved.
[0090] The viscosity of the ionizing radiation curable resin may be in the range of 200 to 250 mPa·s, preferably 220 to 250 mPa·s. When the viscosity of the ionizing radiation curable resin is in this numerical range, fine concavo-convex shapes can be easily formed.
[0091] The above-mentioned repeating structure is preferably any one of an ethylene oxide (EO) structure, a propylene oxide (PO) structure, and an ε-caprolactone (CL) structure. The repeating structure is more preferably ethylene oxide or propylene oxide. The ethylene oxide structure, the propylene oxide structure, and the ε-caprolactone structure are preferred because the molecules can rotate freely and have high flexibility, so the molecules are easily folded by light below 200nm and easily form fine concave-convex shapes. In addition, the number of repetitions of the repeating structure is set to be greater than 12. It is more preferably greater than 12 and less than 50, and most preferably greater than 20 and less than 50. When the number of repetitions is less than 11, when irradiated with vacuum ultraviolet light (VUV light), the ionizing radiation curing resin constituting the surface protection layer 5 does not shrink sufficiently, and the surface protection layer 5 will not become low gloss. When the number of repetitions is greater than 50, the crosslinking density decreases and the scratch resistance of the surface protection layer 5 deteriorates.
[0092] The number of repetitions of the above-mentioned repeating structure can be analyzed by using MALDI-TOF-MS. The ionizing radiation curable resin may have a molecular weight distribution. In the case of having a molecular weight distribution, the number of repetitions is set to the number of repetitions corresponding to the molecular weight having the strongest peak in the MALDI-TOF-MS mass spectrum.
[0093] The surface protection layer 5 may contain particles. By adding particles with an optimal particle size and an optimal content, a uniform surface can be formed. As particles, for example, organic materials such as PE wax, PP wax, resin beads, or inorganic materials such as silica, glass, aluminum oxide, titanium dioxide, zirconium oxide, calcium carbonate, and barium sulfate can be used. The average particle size (D50) of the particles is preferably 10 μm or less. More preferably, it is 1 μm to 8 μm, further preferably 2 μm to 6 μm, and most preferably 3 μm to 5 μm. In the case of more than 10 μm, the scratch resistance is reduced due to the shedding of particles, so it is not preferred. In the case of less than 1 μm, the effect of making the surface uniform is small, so it is not preferred.
[0094] In addition, the amount of particles added is preferably 0.5 to 10 parts by mass relative to 100 parts by mass of the ionizing radiation curable resin. The amount of particles added is more preferably 2 to 8 parts by mass, further preferably 2 to 6 parts by mass, and most preferably 4 to 5 parts by mass. The surface protection layer 5 is preferably formed into a uniform surface state by containing the above-mentioned amount of particles.
[0095] Here, "particle size (average particle size)" may be a value (average value) obtained by measuring the particle size distribution of the particles used; or it may be a value obtained by observing the cross section of the obtained decorative material, measuring the particle sizes of multiple particles and averaging them. The two measurement methods are different from each other, but the obtained particle size values are substantially the same. For example, the average particle size of the particles added to the surface protection layer 5 may be the median particle size (D50) measured by a laser diffraction / scattering particle size distribution measuring device.
[0096] When the entire surface protection layer 5 is cured by UV light, a photoinitiator needs to be added to the surface protection layer 5. The photoinitiator is not particularly limited, and examples thereof include benzophenone-based, acetophenone-based, benzoin ether-based, and thioxanthone-based photoinitiators.
[0097] In order to impart the required functions, functional additives such as antibacterial agents and mildewproof agents may be added to the surface protection layer 5. In addition, ultraviolet absorbers and light stabilizers may be added to the surface protection layer 5 as required. As ultraviolet absorbers, for example, benzotriazole series, benzoate series, benzophenone series, triazine series, etc. are usually added in any combination, and as light stabilizers, for example, hindered amine series, etc. are usually added in any combination.
[0098] Although such a decorative sheet 1 does not contain a gloss regulator (matting additive), the glossiness is 15 or less. In conventional decorative sheets, when the glossiness of a decorative sheet having a surface protective layer is 8 or less, the content of the gloss regulator in the surface protective layer is high, and the surface protective layer becomes turbid. Therefore, the color and pattern of the colored pattern layer may not be clearly expressed, or the design of the decorative sheet may be reduced. In addition, in the case of obtaining a decorative sheet with a glossiness close to 0, the content of the gloss regulator in the surface protective layer is further increased, so it is difficult to form a surface protective layer with a smooth surface without generating streaks, spots, etc. when forming the surface protective layer.
[0099] The decorative sheet 1 can obtain a decorative sheet having a glossiness of 15 or less while maintaining the same level of performance as a decorative sheet having a glossiness of 20 or more. Here, the "glossiness" is a value measured at an incident angle of 60 degrees using a gloss meter according to JIS Z8741.
[0100] <Hidden Layer 8>
[0101] In addition, when it is desired to provide concealment to the base material B in the decorative sheet 1, a coloring sheet may be used on the raw material layer 2 or an opaque concealing layer 8 may be provided. The concealing layer 8 may be basically made of the same material as the pattern layer 3, but since concealment is the purpose, it is preferred to use an opaque pigment, titanium oxide, iron oxide, etc. as the pigment. In addition, in order to improve concealment, metals such as gold, silver, copper, and aluminum may be added. Usually, aluminum in a thin sheet form is often added.
[0102] (Manufacturing method)
[0103] A production example of the decorative sheet 1 will be described.
[0104] A resin film is used as the raw material layer 2, and a surface protection layer 5 is formed on the raw material layer 2 by printing. For the surface protection layer 5, the surface of the coated ionizing radiation curable resin is irradiated with light having a wavelength of less than 200nm (the first irradiation light) to shrink the surface of the ionizing radiation curable resin. Then, in order to cure the shrunken ionizing radiation curable resin, ionizing radiation or UV light having a wavelength longer than the light having a wavelength of less than 200nm as the first irradiation light is irradiated. Thus, a decorative sheet 1 having a surface protection layer 5 is formed, the surface protection layer 5 having a core 5A and a ridge 5B provided to protrude in a ridge shape from one surface (the upper surface) of the core 5A.
[0105] (Other functions)
[0106] The decorative sheet 1 involved in this embodiment has a surface protection layer 5 with a concavo-convex shape formed on the surface. According to this structure, even if the surface protection layer does not contain a gloss regulator (matting additive), the gloss (glossiness) of the surface protection layer can be adjusted. The gloss regulator reduces the oleophobicity of the layer formed by the resin material, so fingerprints are easily attached. Since the surface protection layer 5 involved in this embodiment does not contain a gloss regulator, it does not absorb oil and the oleophobicity is relatively improved. Therefore, in various occasions such as on-site construction, furniture assembly, and daily life of residents, it is difficult to attach fingerprints to the decorative sheet 1 having the surface protection layer 5.
[0107] Furthermore, according to the configuration of the surface protection layer 5 having the uneven shape formed on the surface, the oil repellency of the surface protection layer 5 is improved, and it is possible to suppress the adsorption of oil stains and pollutants on the surface of the decorative sheet 1 .
[0108] Furthermore, since the surface protection layer 5 does not contain a gloss adjuster, when the surface of the decorative sheet 1 is scratched, the particles of the gloss adjuster do not fall off, and gloss changes and scratches on the surface of the decorative sheet 1 are unlikely to occur.
[0109] In addition, according to the Martens hardness of 20N / mm 2 Above 200N / mm 2 When the surface protection layer 5 is configured within the following range, the surface protection layer 5 itself has a certain hardness, and curling of the decorative sheet 1 caused by curing shrinkage of the surface protection layer 5 is reduced, thereby facilitating lamination to the base material.
[0110] In addition, according to the Martens hardness of 20N / mm 2 Above 200N / mm 2 The configuration of the surface protection layer 5 within the following range can provide appropriate flexibility to the surface protection layer 5 itself, so that the decorative sheet 1 is less likely to be broken (damage to the decorative sheet 1 is reduced).
[0111] In the present embodiment, the surface protection layer 5 is formed of one layer, but is not limited to such a configuration. For example, the surface protection layer 5 may be a multi-layer configuration. That is, the surface protection layer 5 may be laminated with multiple layers of the same ionizing radiation curing resin, or laminated with multiple layers of different ionizing radiation curing resins, and a concave-convex shape may be formed on the surface. In the case of laminating multiple layers of different ionizing radiation curing resins, for example, the Martens hardness of the outermost layer of the surface protection layer 5 is 20N / mm 2 Above 200N / mm 2Within the following range, the main material is an ionizing radiation curable resin, the main component of which is a tetrafunctional acrylic resin containing a repeating structure, the repeating structure is preferably any one of the structures of ethylene oxide, propylene oxide and ε-caprolactone, and the number of repetitions of the repeating structure is greater than 12. There is no particular limitation on the layer located on the side of the original material layer 2 of the surface protective layer 5 (i.e., the layer located below the outermost layer of the surface protective layer 5).
[0112] For example, the Martens hardness of the bottom layer of the surface protection layer 5 (the layer located on the original material layer 2 side of the surface protection layer 5) may be 20 N / mm 2 Above 200N / mm 2 Within the following range, the main material is an ionizing radiation curable resin, the main component of which is a tetrafunctional acrylic resin containing a repeating structure, the repeating structure is preferably any one of the structures of ethylene oxide, propylene oxide and ε-caprolactone, and the number of repetitions of the repeating structure is greater than 12, and there is no particular limitation on the outermost layer of the surface protection layer 5.
[0113] [Example]
[0114] Hereinafter, embodiments according to the present invention will be described.
[0115] <Example 1>
[0116] The unit area mass is 50g / m 2 The impregnated paper (GFR-506: manufactured by Kojin Co., Ltd.) was used as the raw material layer 2, and a pattern layer 3 was formed on one surface using an oily nitrocellulose resin gravure printing ink (PCNT (PCRNT) various colors: manufactured by Toyo Ink Co., Ltd.), and then the following surface protective layer coating liquid was applied. The layer thickness of the surface protective layer coating liquid was set to 5 μm. Then, the surface of the surface protective layer coating liquid was irradiated so that the accumulated light amount became 100 mJ / cm 2 The surface was irradiated with a Xe excimer lamp having a wavelength of 172 nm to shrink the surface. Then, the surface protective layer coating liquid was cured by irradiation with ionizing radiation to form a surface protective layer 5, thereby obtaining a decorative sheet of Example 1 having a total thickness of 60 μm.
[0117] (Surface protection layer coating liquid)
[0118] The surface protective layer coating liquid is composed of the following particles mixed with the following ionizing radiation curable resin.
[0119] ·Ionizing radiation curable resin
[0120] Type: Ethoxylated pentaerythritol tetraacrylate (EO35 molar addition)
[0121] Product name: NK Ester ATM-35E (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.)
[0122] Mixing: 100 parts by mass
[0123] ·particle
[0124] Product name: SYLYSIA 250N (manufactured by Fuji Silysia Chemical Ltd.)
[0125] Particle size: 5μm
[0126] Mixing: 0.5 parts by mass
[0127] <Example 2>
[0128] A decorative sheet of Example 2 was obtained in the same manner as in Example 1 except that the ionizing radiation curable resin of Example 1 was replaced with the following resin.
[0129] ·Ionizing radiation curable resin
[0130] Type: Ethoxylated pentaerythritol tetraacrylate (EO50 molar addition)
[0131] <Example 3>
[0132] A decorative sheet of Example 3 was obtained in the same manner as in Example 1 except that the ionizing radiation curable resin of Example 1 was replaced with the following resin.
[0133] ·Ionizing radiation curable resin
[0134] Type: Ethoxylated pentaerythritol tetraacrylate (EO20 molar addition)
[0135] <Example 4>
[0136] A decorative sheet of Example 4 was obtained in the same manner as in Example 1 except that the ionizing radiation curable resin of Example 1 was replaced with the following resin.
[0137] ·Ionizing radiation curable resin
[0138] Type: Propoxylated pentaerythritol tetraacrylate (PO35 molar addition)
[0139] <Example 5>
[0140] A decorative sheet of Example 5 was obtained in the same manner as in Example 1 except that the ionizing radiation curable resin of Example 1 was replaced with the following resin.
[0141] ·Ionizing radiation curable resin
[0142] Type: Caprolactone modified pentaerythritol tetraacrylate (caprolactone (CL) 30 mole addition)
[0143] <Example 6>
[0144] A decorative sheet of Example 6 having a total thickness of 56 μm was obtained in the same manner as in Example 1 except that the layer thickness of the surface protection layer coating liquid of Example 1 was 1 μm.
[0145] <Example 7>
[0146] A decorative sheet of Example 7 having a total thickness of 57 μm was obtained in the same manner as in Example 1 except that the layer thickness of the surface protection layer coating liquid of Example 1 was 2 μm.
[0147] <Example 8>
[0148] A decorative sheet of Example 8 having a total thickness of 75 μm was obtained in the same manner as in Example 1 except that the layer thickness of the surface protection layer coating liquid of Example 1 was 20 μm.
[0149] <Example 9>
[0150] A decorative sheet of Example 9 having a total thickness of 80 μm was obtained in the same manner as in Example 1 except that the layer thickness of the surface protection layer coating liquid of Example 1 was 25 μm.
[0151] <Example 10>
[0152] A decorative sheet of Example 10 was obtained in the same manner as in Example 9 except that the particles of Example 9 were not blended.
[0153] <Example 11>
[0154] A decorative sheet of Example 11 was obtained in the same manner as in Example 3 except that the particles of Example 3 were not blended.
[0155] <Example 12>
[0156] A decorative sheet of Example 12 was obtained in the same manner as in Example 1 except that the particles of Example 1 were replaced with the following particles.
[0157] ·particle
[0158] Product name: SYLYSIA 450 (manufactured by Fuji Silysia Chemical Ltd.)
[0159] Particle size: 8.0 μm
[0160] Mixing: 0.5 parts by mass
[0161] <Example 13>
[0162] A decorative sheet of Example 13 was obtained in the same manner as in Example 1 except that the particles of Example 1 were replaced with the following particles.
[0163] ·particle
[0164] Product name: SYLYSIA 780 (manufactured by Fuji Silysia Chemical Ltd.)
[0165] Particle size: 11.3 μm
[0166] Mixing: 0.5 parts by mass
[0167] <Example 14>
[0168] A decorative sheet of Example 14 was obtained in the same manner as in Example 1 except that the blending amount of the particles of Example 1 was changed to 10 parts by mass.
[0169] <Example 15>
[0170] A decorative sheet of Example 15 was obtained in the same manner as in Example 1 except that the blending amount of the particles of Example 1 was changed to 11 parts by mass.
[0171] <Example 16>
[0172] A decorative sheet of Example 16 having a total thickness of 56 μm was obtained in the same manner as in Example 1 except that the layer thickness of the surface protection layer coating liquid of Example 1 was 1 μm and no particles were present.
[0173] <Example 17>
[0174] A decorative sheet of Example 17 was obtained in the same manner as in Example 1 except that the ionizing radiation curable resin of Example 1 was replaced with the following resin.
[0175] ·Ionizing radiation curable resin
[0176] Type: Ethoxylated pentaerythritol tetraacrylate (EO12 molar addition)
[0177] <Example 18>
[0178] A decorative sheet of Example 18 having a total thickness of 80 μm was obtained in the same manner as in Example 2 except that the layer thickness of the surface protection layer coating liquid of Example 2 was 25 μm.
[0179] <Example 19>
[0180] A decorative sheet of Example 19 was obtained in the same manner as in Example 1 except that the ionizing radiation curable resin of Example 1 was replaced with the following resin.
[0181] ·Ionizing radiation curable resin 1 (main component)
[0182] Type: Ethoxylated pentaerythritol tetraacrylate (EO35 molar addition)
[0183] Product name: NK Ester ATM-35E (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.)
[0184] Mixing: 60 parts by mass
[0185] ·Ionizing radiation curable resin 2
[0186] Type: Dipentaerythritol hexaacrylate
[0187] Product name: Miramer M600 (made by Miwon)
[0188] Mixing: 40 parts by mass
[0189] <Comparative Example 1>
[0190] A decorative sheet of Comparative Example 1 was obtained in the same manner as in Example 1 except that the excimer lamp irradiation of Example 1 was not performed and the amount of particles added was changed to 15 parts by mass.
[0191] <Comparative Example 2>
[0192] A decorative sheet of Comparative Example 2 was obtained in the same manner as in Example 1 except that the ionizing radiation curable resin in Example 1 was replaced with the following resin.
[0193] ·Ionizing radiation curable resin
[0194] Type: Trimethylolpropane EO modified triacrylate (EO6 molar addition)
[0195] Product name: Miramer M3160 (made by Miwon)
[0196] <Comparative Example 3>
[0197] A decorative sheet of Comparative Example 3 was obtained in the same manner as in Example 1 except that the ionizing radiation curable resin in Example 1 was replaced with the following resin.
[0198] ·Ionizing radiation curable resin
[0199] Type: Ethoxylated dipentaerythritol polyacrylate (EO12 molar addition)
[0200] Product name: NK Ester A-DPH-12E (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.)
[0201] <Comparative Example 4>
[0202] A decorative sheet of Comparative Example 4 was obtained in the same manner as in Example 1 except that the ionizing radiation curable resin in Example 1 was replaced with the following resin.
[0203] ·Ionizing radiation curable resin
[0204] Type: Pentaerythritol tetraacrylate
[0205] Product name: NK Ester A-TMMT (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.)
[0206] (evaluate)
[0207] The decorative sheets of Examples 1 to 19 and Comparative Examples 1 to 4 obtained by the above method were evaluated.
[0208] In the present example, if the evaluation is "○" or "△", there is no problem in actual use, and thus it is regarded as passing.
[0209] <Surface Condition>
[0210] As for the surface state, the surface uniformity was evaluated by visual inspection.
[0211] The evaluation criteria are as follows.
[0212] 0:Uniform surface condition
[0213] △: There is unevenness in some parts
[0214] ×: Surface condition that is uneven across the entire surface
[0215] <Glossiness>
[0216] The glossiness was measured at 60° glossiness using Rhopoint IQ (manufactured by KONICA MINOLTA, INC.) In Tables 1 and 2, the 60° glossiness is expressed as "60° glossiness value".
[0217] Note that if the glossiness is 15 or less, it is regarded as sufficiently low glossiness, and therefore, in this example, “15 or less” is regarded as passing.
[0218] <Martens hardness measurement method>
[0219] The method for measuring the Martens hardness is described. The Martens hardness of each decorative sheet is measured using a Martens hardness measuring device (FISCHERSCOPE HM 2000; manufactured by Fischer Instruments Co., Ltd.) according to ISO 14577. It should be noted that since the measurement is carried out from the cross section, for the sample, the decorative sheet 1 is embedded in a resin such as a cold-curing epoxy resin or a UV-curing resin and fully cured, then cut to expose the cross section of the decorative sheet 1, and mechanical grinding is performed to obtain the measuring surface. The specific measurement method is to press the indenter into the measuring surface of each sample, and calculate the Martens hardness based on the indentation depth and load. The measurement conditions are set to a test force of 10 mN, a test force load time of 10 seconds, and a test force holding time of 5 seconds, and the measurement is carried out.
[0220] <Anti-fingerprint property: Wiping property evaluation>
[0221] As the anti-fingerprint evaluation, the fingerprint wiping property evaluation was performed.
[0222] The 60-degree glossiness of the surface of each decorative sheet was measured as the "initial glossiness". Next, after the anti-fingerprint evaluation liquid was attached to the surface protection layer, the anti-fingerprint evaluation liquid attached to the surface of the decorative sheet was wiped off. Then, the 60-degree glossiness of the portion after the anti-fingerprint evaluation liquid was wiped off was measured as the "glossiness after wiping". Here, a higher fatty acid was used as the anti-fingerprint evaluation liquid.
[0223] The fingerprint wipe rate is calculated as follows.
[0224] Fingerprint wiping rate (%) = (gloss after wiping / initial gloss) × 100
[0225] The evaluation criteria are as follows.
[0226] ○: 70% or more and less than 250%
[0227] △: 50% or more and less than 70%, or 250% or more and less than 300%
[0228] ×: less than 50%, or more than 300%
[0229] <Pollution resistance>
[0230] As an evaluation of stain resistance, according to the stain A test specified in the Japanese Agricultural Standards (JAS), lines with a width of 10 mm were drawn with blue ink, black quick-drying ink and red crayon respectively. After leaving for 4 hours, the lines of blue ink, black quick-drying ink and red crayon were wiped with ethanol in a cloth to evaluate the stain resistance to ink.
[0231] The evaluation criteria are as follows.
[0232] ○: Can easily wipe the colored threads
[0233] △: You can wipe part of each color thread, but dirt will remain on some of them.
[0234] ×: Cannot wipe colored threads
[0235] <Scratch resistance test: Stainless steel wool friction test>
[0236] The obtained decorative sheet was attached to the wooden substrate B using a urethane adhesive, and then a stainless steel wool friction test was performed as a scratch resistance evaluation. A load of 100 g was applied to the stainless steel wool and rubbed back and forth 20 times, and the scratches and gloss changes on the decorative sheet surface were visually confirmed.
[0237] The evaluation criteria are as follows.
[0238] 0: No surface damage or gloss change
[0239] △: Slight damage or gloss change on the surface
[0240] ×: The surface has obvious damage or gloss changes
[0241] <Processability Test: Curl>
[0242] The obtained decorative sheet was cut into 10 cm squares and left to stand at 25°C and 50% RH for 48 hours. Then, the average distance between the four corners and the plane was calculated. Figure 6 As shown in FIG. 1 , in this curling test, the shortest distance d from the surface (plane) of the test stand on which the decorative sheet is placed to each corner of the decorative sheet is measured, and the values are averaged to evaluate the curling of the decorative sheet. It should be noted that the curling is used as an index of the ease of lamination to the substrate.
[0243] The evaluation criteria are as follows.
[0244] ○: 3cm or less
[0245] △: greater than 3cm and less than 5cm
[0246] ×: larger than 5cm
[0247] <Processability test: Wrapping processing (cracking)>
[0248] The obtained decorative sheet was packaged and the edges of the cut decorative sheet were visually observed to evaluate cracking.
[0249] The evaluation criteria are as follows.
[0250] ○: No rupture observed
[0251] △: Partial cracking was observed
[0252] ×: Cracks were observed on the entire surface
[0253] The evaluation results are shown in Tables 1 and 2.
[0254] [Table 1]
[0255]
[0256] [Table 2]
[0257]
[0258] As shown in Table 1, the decorative sheets of Examples 1 to 19 can provide decorative sheets having a glossiness of 15 or less and having fingerprint resistance, scratch resistance, stain resistance, and processability. In addition to the surface shape of the surface protective layer and the resin composition of the surface protective layer, the performance can be further improved by optimizing the layer thickness of the surface protective layer, the particle size of the particles to be mixed, and the amount of addition.
[0259] Explanation of symbols
[0260] 1 decorative sheet
[0261] 2 Raw material layer
[0262] 3 pattern layers
[0263] 4 Transparent resin layer
[0264] 5. Surface protection layer
[0265] 6 Primer coat
[0266] 7 Adhesive layer
[0267] 8 Hidden Layer
[0268] 11Decoration Materials
[0269] B substrate
Claims
1. A decorative sheet comprising a raw material layer and a surface protection layer provided on one surface of the raw material layer, characterized in that: The glossiness of the surface protection layer is below 15, The surface protection layer has a ridge portion provided on the surface thereof so as to protrude in a ridge shape and is formed with a concavo-convex shape. The Martens hardness of the surface protection layer is 20N / mm 2 Above 200N / mm 2 Within the following range, The main material of the surface protection layer is ionizing radiation curable resin. The main component of the ionizing radiation curable resin is a tetrafunctional acrylic resin having a repeating structure. The number of repetitions of the repeating structure is 12 or more, The RSm / Ra of the concavo-convex shape of the surface protection layer is in the range of 10 or more and 300 or less.
2. The decorative sheet according to claim 1, characterized in that: The repeating structure is any one of the structures of ethylene oxide, propylene oxide and ε-caprolactone.
3. The decorative sheet according to claim 1 or claim 2, characterized in that: The thickness of the surface protection layer is in the range of 2 μm to 20 μm.
4. The decorative sheet according to any one of claims 1 to 3, characterized in that: The surface protection layer includes particles having an average particle size of 10 μm or less.
5. The decorative sheet according to claim 4, characterized in that: The amount of the particles added is in a range of 0.5 parts by mass to 10 parts by mass, both inclusive, relative to 100 parts by mass of the ionizing radiation curable resin.
6. A method for manufacturing a decorative sheet, characterized in that: The surface of the applied ionizing radiation curable resin is irradiated with light having a wavelength of 200 nm or less, and then irradiated with ionizing radiation or UV light having a wavelength longer than the light having a wavelength of 200 nm or less. Thereby, a surface protection layer having ridge portions protruding in a ridge shape is formed.
7. The method for manufacturing a decorative sheet according to claim 6, characterized in that: The wavelength of the light with a wavelength of 200 nm or less is 172 nm.
8. The decorative sheet according to claim 1, characterized in that: The RSm / Ra of the concavo-convex shape of the surface protection layer is in the range of 50 or more and 300 or less.
9. The decorative sheet according to claim 1, characterized in that: The RSm / Ra of the concavo-convex shape of the surface protection layer is in the range of 100 or more and 300 or less.
Citation Information
Patent Citations
Ultraviolet-curable coating agent composition and laminate
JP2017171794A
Cured product
JP2020111715A
Dielectric composition and electronic component
KR1020200110244A