Polypropylene-based foamed particles, polypropylene
By using polypropylene-based resin with specific MI values and melting points and expansion flame retardant, the problem of insufficient flame retardancy of the polypropylene-based foamed molded body in the prior art is solved, and efficient The flame retardancy is improved and meets the strict standards of electrical components.
Patent Information
- Application Number
- CN202380028484.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-06
- Publication Date
- 2024-11-12
AI Technical Summary
The flame retardancy of the existing polypropylene-based foamed molded body has not yet met the high requirements for the peripheral components of the electrical components, and there is room for further improvement.
Polypropylene-based foamed particles containing polypropylene-based resins and expansion-based flame retardants with MI values and melting points within a specific range are used to produce foamed particles through dispersion and release processes, and flame retardant is obtained by in-mold foaming molding. Excellent polypropylene foam molded body.
It provides a polypropylene foam molded body with significantly improved flame retardancy, which can meet the high standards of UL94V vertical combustion test and is suitable for electrical components and other fields.
Smart Images

Figure BDA0005048626610000101 
Figure BDA0005048626610000111 
Figure BDA0005048626610000112
Abstract
Description
Technical Field
[0001] The present invention relates to polypropylene foamed particles and polypropylene foamed molded products, and methods for producing the same. Background Art
[0002] Molded articles (foamed articles) formed by molding polypropylene foam particles have been widely used as automotive interior materials and cushioning materials. Recently, in the process of transition to electric vehicles, there is an increasing demand for the use of polypropylene foamed articles in peripheral components of electrical parts.
[0003] Polypropylene-based foamed molded products used as peripheral members of electrical components are required to have higher flame retardancy, and a technique for imparting flame retardancy to polypropylene-based foamed molded products has been proposed (for example, Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2016 / 052739 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] However, from the viewpoint of the flame retardancy of the obtained foamed molded article, the above-mentioned conventional techniques have room for further improvement.
[0009] In view of the above circumstances, an object of one embodiment of the present invention is to provide polypropylene foamed particles capable of providing a polypropylene foamed molded product having excellent flame retardancy.
[0010] Solutions for solving problems
[0011] The present inventors have conducted intensive studies to solve the above-mentioned problems and have completed the present invention.
[0012] That is, the polypropylene foamed particles involved in one embodiment of the present invention are polypropylene foamed particles obtained by foaming polypropylene resin particles, wherein the polypropylene resin particles contain a base resin and an expandable flame retardant, and the base resin contains: a polypropylene resin (a) having an MI of 4.00 g / 10 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C., and a polypropylene resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135° C. to 155° C.
[0013] In addition, a method for producing polypropylene foamed particles according to one embodiment of the present invention includes: a dispersion step of dispersing polypropylene resin particles, an aqueous dispersion medium, and a foaming agent in a container; and a release step of releasing the dispersion obtained in the aforementioned dispersion step to a region where the pressure is lower than the pressure in the aforementioned container, wherein the aforementioned polypropylene resin particles contain a base resin and an expandable flame retardant, and the base resin contains: a polypropylene resin (a) having an MI of 4.00 g / 10.00 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C., and a polypropylene resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135° C. to 155° C.
[0014] Effects of the Invention
[0015] According to one embodiment of the present invention, the following effect is achieved: polypropylene foamed particles capable of providing a polypropylene foamed molded article having excellent flame retardancy can be provided. DETAILED DESCRIPTION
[0016] The following is a description of one embodiment of the present invention, but the present invention is not limited thereto. The present invention is not limited to the various structures described below, and various changes can be made within the scope indicated in the claims. In addition, embodiments or embodiments obtained by combining the technical means respectively disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, by combining the technical means respectively disclosed in each embodiment, new technical features can be formed. It should be noted that all academic literature and patent documents recorded in this specification are cited in this specification as references. In addition, in this specification, unless otherwise specified, "A to B" indicating a numerical range means "above A (including A and greater than A) and below B (including B and less than B)".
[0017] In this specification, a structural unit derived from X monomer contained in a polymer or a copolymer may be referred to as "X unit".
[0018] In this specification, unless otherwise specified, X 1 Unit, X 2 Unit, ... and X n A copolymer having a unit (n is an integer greater than 2) as a structural unit is referred to as "X 1 / X 2 / …… / X n Copolymer". As X 1 / X 2 / …… / X nThe copolymer is not particularly limited in the polymerization method unless otherwise specified, and may be a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer.
[0019] [1. Polypropylene foam particles]
[0020] The polypropylene foamed particles involved in one embodiment of the present invention are foamed particles obtained by foaming polypropylene resin particles, wherein the polypropylene resin particles contain a base resin and an expandable flame retardant, and the base resin contains: a polypropylene resin (a) having an MI of 4.00 g / 10.00 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C., and a polypropylene resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135° C. to 155° C.
[0021] The foamed beads have the above-mentioned structure, and therefore have the advantage of being able to provide a polypropylene foamed molded product having excellent flame retardancy. The foamed beads according to one embodiment of the present invention can also be said to be foamed beads using the polypropylene resin particles according to one embodiment of the present invention as a raw material.
[0022] The polypropylene foamed molded article can be provided by subjecting the polypropylene foamed particles according to one embodiment of the present invention to in-mold foam molding by a known method.
[0023] In this specification, “polypropylene resin particles” are sometimes referred to as “resin particles”, “polypropylene resin particles involved in one embodiment of the present invention” are sometimes referred to as “present resin particles”, “polypropylene foamed particles” are sometimes referred to as “foamed particles”, “polypropylene foamed particles involved in one embodiment of the present invention” are sometimes referred to as “present foamed particles”, and “polypropylene foamed molded article” is sometimes referred to as “foamed molded article”.
[0024] Hereinafter, each component which may be contained in the present resin particles which are the raw materials of the present foamed beads will be described.
[0025] <Base resin>
[0026] The present resin particles include a base resin, which includes a polypropylene resin (a) having an MI of 4.00 g / 10 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C., and a polypropylene resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135° C. to 155° C. In the present specification, the “base resin” refers to a resin component that substantially constitutes the present resin particles.
[0027] The base resin preferably contains 20 to 95 weight % of the polypropylene resin (a) in 100 weight % of the base resin, more preferably 30 to 90 weight % and even more preferably 35 to 75 weight %. The foamed particles obtained by foaming the resin particles containing the base resin satisfying this constitution have the advantage of being able to provide a foamed molded article having excellent surface properties.
[0028] In 100 wt % of the base resin, the base resin preferably contains 5 wt % to 80 wt % of the polypropylene resin (b), more preferably 10 wt % to 70 wt %, and further preferably 25 wt % to 65 wt %. The foamed particles formed by foaming the resin particles containing the base resin satisfying this constitution have the following advantages: a foamed molded article having excellent flame retardancy can be provided, which can satisfy the standard of the UL94V vertical combustion test which is an indicator of high flame retardancy.
[0029] Relative to the total amount of 100% by weight of the resin particles, the present resin particles preferably include more than 70.0% by weight of the substrate resin, more preferably more than 75.0% by weight, and more preferably more than 77.0% by weight. In the case where the resin particles include (i) more than 70.0% by weight of the substrate resin, a foaming molded body having no shrinkage and excellent strength (e.g., compressive strength) can be obtained. The upper limit of the content of the substrate resin in the present foaming resin is not particularly limited, but for example, relative to the total amount of 100% by weight of the resin particles, it can be 89.0% by weight or less, preferably 85.0% by weight, and more preferably 80.0% by weight or less.
[0030] (Polypropylene resin)
[0031] The base resin contained in the present resin particles includes two polypropylene resins (polypropylene resin (a) and polypropylene resin (b)). In the following description, unless otherwise specified, the description of "polypropylene resin" applies to any of "polypropylene resin (a)" and "polypropylene resin (b)".
[0032] In the present specification, the "polypropylene-based resin" refers to a resin containing 50 mol% or more of propylene units in 100 mol% of all structural units constituting the polypropylene-based resin.
[0033] In this specification, a "structural unit derived from a propylene monomer" may be referred to as a "propylene unit".
[0034] The polypropylene resin may be (i) a homopolymer of propylene, (ii) a block copolymer, alternating copolymer, random copolymer or graft copolymer of propylene and a monomer other than propylene, or (iii) a mixture of two or more thereof.
[0035] Among them, the polypropylene resin is preferably a random copolymer of propylene and a monomer other than propylene from the viewpoint of having the advantage of being able to process the resin particles and foamed particles at a low heating temperature in the foaming step and in-mold foam molding step described later.
[0036] In one embodiment of the present invention, from the viewpoint of excellent heat resistance, impact absorption and chemical resistance of the obtained foamed molded product, it is preferred that the polypropylene resin (a) and / or the polypropylene resin (b) are random copolymers, and it is more preferred that the polypropylene resin (a) and the polypropylene resin (b) are random copolymers.
[0037] The polypropylene resin may have one or more structural units derived from monomers other than the propylene monomer in addition to the propylene unit, or may have one or more types. The "monomers other than the propylene monomer" used in the production of the polypropylene resin is sometimes referred to as a "comonomer". The "structural unit derived from monomers other than the propylene monomer" contained in the polypropylene resin is sometimes referred to as a "comonomer unit".
[0038] Examples of the comonomer include α-olefins having 2 or 4 to 12 carbon atoms, such as ethylene, 1-butene, isobutylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, 1-octene and 1-decene.
[0039] Specific examples of polypropylene resins include polypropylene homopolymers, ethylene / propylene random copolymers, 1-butene / propylene random copolymers, 1-butene / ethylene / propylene random copolymers, ethylene / propylene block copolymers, 1-butene / propylene block copolymers, propylene / vinyl chloride copolymers, propylene / maleic anhydride copolymers, and styrene-modified polypropylene resins.
[0040] As polypropylene resin, one of the above-mentioned specific examples can be used alone, or two or more can be used in combination. In the above-mentioned specific examples, from the viewpoint that the obtained resin particles have good foamability and the viewpoint that the obtained foamed particles have good formability, it is suitable to be ethylene / propylene random copolymer and 1-butene / ethylene / propylene random copolymer.
[0041] As a polypropylene resin, the case of using an ethylene / propylene random copolymer (referred to as case A) is considered. In case A, the ethylene content in the ethylene / propylene random copolymer is preferably 0.2% by weight to 15.0% by weight, more preferably 0.5% by weight to 10.0% by weight, and further preferably 0.5% by weight to 4.0% by weight in 100% by weight of each copolymer. The ethylene content can also be referred to as the content of structural units (ethylene units) derived from ethylene. When the content of ethylene units in the ethylene / propylene random copolymer is (i) 0.2% by weight or more, there is a tendency that the foamability of the resin particles in the process of manufacturing the present foamed particles and / or the moldability of the obtained foamed particles become good, and when it is (ii) 15.0% by weight or less, there is no need to worry about the reduction of the mechanical properties of the foamed molded body obtained from the present foamed particles.
[0042] The melting point of the polypropylene resin (a) is preferably 135° C. to 155° C., more preferably 136° C. to 154° C., more preferably 137° C. to 153° C., more preferably 138° C. to 152° C., further preferably 139° C. to 151° C., and particularly preferably 140° C. to 150° C. When the melting point of the polypropylene resin is (i) 135° C. or higher, a foamed molded article having excellent dimensional stability at high temperatures tends to be easily obtained, and when it is (ii) 155° C. or lower, a foamed molded article can be molded by in-mold foaming at a low water vapor pressure.
[0043] The melting point of the polypropylene resin (b) is preferably 135° C. to 155° C., more preferably 136° C. to 154° C., more preferably 137° C. to 153° C., more preferably 138° C. to 152° C., further preferably 139° C. to 151° C., and particularly preferably 140° C. to 150° C. When the melting point of the polypropylene resin (b) is (i) 135° C. or higher, a foamed molded article having excellent dimensional stability at high temperatures tends to be easily obtained, and when it is (ii) 155° C. or lower, a foamed molded article having excellent surface properties can be obtained by in-mold foam molding at a low water vapor pressure.
[0044] The resin particles contain a polypropylene resin (a) and a polypropylene resin (b) having a melting point of 135°C to 155°C as base resins, and thus tend to easily produce a foamed molded product having better dimensional stability at high temperatures. In addition, the foamed molded product can be molded by in-mold foaming at a lower water vapor pressure.
[0045] In this specification, the melting point of a polypropylene resin is a value determined by differential scanning calorimetry (hereinafter referred to as "DSC method"). The specific operation steps are as follows: (1) the temperature of 5 mg to 6 mg of a polypropylene resin is increased from 40.0°C to 220.0°C at a heating rate of 10.0°C / min, thereby melting the polypropylene resin; (2) then, the temperature of the melted polypropylene resin is decreased from 220.0°C to 40.0°C at a cooling rate of 10.0°C / min, thereby crystallizing the polypropylene resin; (3) then, the temperature of the crystallized polypropylene resin is further increased from 40.0°C to 220.0°C at a heating rate of 10°C / min. The temperature of the peak (melting peak) of the DSC curve of the polypropylene resin obtained at the second heating (i.e., at (3)) can be determined as the melting point of the polypropylene resin. It should be noted that when there are multiple peaks (melting peaks) in the DSC curve of the polypropylene resin obtained by the above method at the second temperature increase, the temperature of the peak (melting peak) with the largest heat of fusion is taken as the melting point of the polypropylene resin. As a differential scanning calorimeter, for example, DSC6200 model made by Seiko Instruments Inc. can be used.
[0046] The melt index (MI) of the polypropylene resin (a) at 230°C is 4.00 g / 10 min to 15.00 g / 10 min, preferably 5.00 g / 10 min to 15.00 g / 10 min, more preferably 5.50 g / 10 min to 12.00 g / 10 min, further preferably 6.00 g / 10 min to 10.00 g / 10 min, and further preferably 6.50 g / 10 min to 8.00 g / 10 min. MI is sometimes referred to as "melt flow rate (MFR)".
[0047] When the MI of the polypropylene resin (a) is 4.00 g / 10 minutes or more, the polypropylene resin has good fluidity during foaming and is easy to foam. In addition, when the MI of the polypropylene resin (a) is 15.00 g / 10 minutes or less, the polypropylene resin has moderate fluidity, and therefore, foamed particles with a high foaming ratio can be obtained. In particular, if the MI of the polypropylene resin (a) is 4.00 g / 10 minutes to 8.00 g / 10 minutes, foamed particles that can appropriately provide a relatively high density foamed molded body can be efficiently manufactured, and therefore it is preferred.
[0048] The melt index (MI) of the polypropylene resin (b) at 230°C is 0.05 to 3.00 g / 10 min, preferably 0.10 to 2.00 g / 10 min, more preferably 0.30 to 1.00 g / 10 min, further preferably 0.40 to 0.60 g / 10 min.
[0049] When the MI of the polypropylene resin (b) is 0.05 g / 10 minutes or more, when kneading with the polypropylene resin (a) in the granulation step described later, it is not easy to produce non-dispersion and can be mixed more evenly. In addition, when the MI of the polypropylene resin (b) is 3.00 g / 10 minutes or less, foamed particles that can provide a foamed molded body with excellent flame retardancy can be obtained. It should be noted that the determination method of the MI of the polypropylene resin is as described in the examples.
[0050] The weight average molecular weight (Mw) of the polypropylene resin (a) is not particularly limited, but is preferably 1×10 4 Above and less than 80×10 4 , more preferably 5×10 4 ~75×10 4 , more preferably 10×10 4 ~50×10 4 .
[0051] The weight average molecular weight (Mw) of the polypropylene resin (b) is not particularly limited, but is preferably 80×10 4 More preferably, 100×10 4 More preferably, 110×10 4 As the polypropylene resin (b), by using a 100×10 4 A resin having a larger Mw than 10×10-10 can provide a foamed molded product having excellent flame retardancy that meets a high flame retardancy standard (UL94V) even when the resin is relatively light (low density) or thin (sample thickness). The upper limit of the Mw of the polypropylene resin (b) is not particularly limited, but may be, for example, 200×10 4 the following.
[0052] In this specification, the Mw of a polypropylene resin refers to a value measured as a polystyrene-equivalent value by gel permeation chromatography (GPC). An example of the measurement conditions of GPC in the measurement of the Mw of a polypropylene resin is as follows.
[0053] (Measurement conditions)
[0054] Sample pretreatment: 30 mg of a sample (polypropylene resin) was completely dissolved in 20 mL of o-dichlorobenzene at 145° C., and the solution was filtered through a sintered filter with a pore size of 1.0 μm. The filtrate obtained was used as an analysis sample.
[0055] Measuring device: Gel permeation chromatograph Alliance GPC 2000 (manufactured by Waters Corporation)
[0056] Analytical apparatus: Data processing software Empower Professional (manufactured by Waters) Columns: 2 TSKgelGMH6-HT, 2 TSKgel GMH6-HTL (dimensions of each column: inner diameter 7.5 mm × length 300 mm, manufactured by Tosoh Corporation) Mobile phase: o-dichlorobenzene (containing 0.025% BHT)
[0057] Column temperature: 140°C
[0058] Detector: Differential refractometer
[0059] Flow rate: 1.0mL / min.
[0060] The molecular structures of the polypropylene resin (a) and the polypropylene resin (b) are not particularly limited, but may be linear structures or branched structures. Among them, from the viewpoint of obtaining a molded body with few interparticle gaps and excellent surface properties, the polypropylene resin (b) is preferably a linear structure, and more preferably both the polypropylene resin (a) and the polypropylene resin (b) are linear structures.
[0061] The polypropylene resin can be obtained by a known method. The polymerization catalyst used in the synthesis of the polypropylene resin is not particularly limited, and a Ziegler catalyst, a metallocene catalyst, and the like can be used.
[0062] <Intumescent flame retardants>
[0063] The resin particles contain an expansion flame retardant. In this specification, an expansion flame retardant refers to a substance that contains phosphorus and nitrogen in its constituent components and can impart flame retardancy to an object (e.g., a foamed molded body) containing the expansion flame retardant. When the foamed molded body containing the expansion flame retardant is burned, the foamed molded body is heated by combustion, and a foaming expansion layer containing a foam-like coating is formed on the surface of the foamed molded body, thereby (i) suppressing the heat from the burning part of the foamed molded body surface from being transferred to the inside of the foamed molded body (heat insulation), suppressing the thermal decomposition of the resin, and (ii) blocking the oxygen supply to the inside of the foaming expansion layer to suppress the oxidation reaction, thereby being able to exert excellent flame retardancy. It can also be said that the expansion flame retardant is a substance that has the function of forming a foaming expansion layer containing such a foam-like coating when the foamed molded body containing the expansion flame retardant is burned.
[0064] In 100% by weight of the resin particles, the present resin particles preferably contain an expansion flame retardant greater than 4.0% by weight and less than 30.0% by weight, more preferably 6.0% by weight to 25.0% by weight, further preferably 11.0% by weight to 23.0% by weight, and further preferably 15.0% by weight to 21.0% by weight. In the case where the resin particles contain (i) an expansion flame retardant greater than 4.0% by weight, a foamed molded product with excellent flame retardancy can be provided, and in the case where the resin particles contain (ii) less than 30.0% by weight, a foamed molded product with no shrinkage and excellent strength (e.g., compression strength) can be provided. It should be noted that, in the case of using a combination of multiple compounds as the expansion flame retardant, the content of the expansion flame retardant in the present resin particles refers to the total amount of the aforementioned multiple compounds.
[0065] The intumescent flame retardant according to one embodiment of the present invention (hereinafter sometimes referred to as "the present intumescent flame retardant") may be (i) a compound containing both a phosphorus atom and a nitrogen atom in the molecule, (ii) a combination of a compound containing a phosphorus atom in the molecule and a compound containing a nitrogen atom in the molecule, or (iii) a combination of two or more thereof. Among them, the present intumescent flame retardant is preferably a combination of a compound containing a phosphorus atom in the molecule and a compound containing a nitrogen atom in the molecule, because it has the advantages of being difficult to be thermally modified during foaming of resin particles and during molding of foamed particles, having good dispersibility in the base resin, and being easy to exert the flame retardant effect caused by the formed foamed layer.
[0066] Examples of the intumescent flame retardant that can be included in the resin pellets include compounds containing both phosphorus atoms and nitrogen atoms in the molecule, such as ammonium polyphosphate, melamine polyphosphate, melamine phosphate, and phosphate ester amide; and pyrophosphates such as piperazine pyrophosphate and melamine pyrophosphate. One of these may be used alone, or two or more of them may be used in combination.
[0067] In the case where the present expansion flame retardant is a combination of a compound containing a phosphorus atom in the molecule and a compound containing a nitrogen atom in the molecule, as the compound containing the phosphorus atom, organic phosphorus compounds, red phosphorus, etc. can be listed. In addition, as the compound containing the nitrogen atom in the molecule, hindered amines, melamine, ammonium borate, ammonium carbonate, etc. can be listed. Among them, from the advantage of being able to provide foamed particles that can provide a foamed molded body with excellent surface aesthetics and productivity on the basis of flame retardancy, as the compound containing the phosphorus atom, an organic phosphorus compound is preferably used, and as the compound containing the nitrogen atom in the molecule, a hindered amine is preferably used. That is, the present resin particles preferably contain organic phosphorus compounds and hindered amines as expansion flame retardants, and more preferably only contain organic phosphorus compounds and hindered amines. It should be noted that compounds containing phosphorus atoms and nitrogen atoms are not regarded as "compounds containing phosphorus atoms" in this specification, and compounds containing nitrogen atoms and phosphorus atoms are not regarded as "compounds containing nitrogen atoms" in this specification.
[0068] (Organophosphorus compounds)
[0069] Examples of the organic phosphorus compound include phosphonates, organic phosphites, organic phosphinites, metal salts of phosphinic acid, metal salts of diphosphinic acid, phosphinates, and polyol phosphate alcohols.
[0070] Among the above-mentioned organic phosphorus compounds, phosphonic acid esters are preferred from the viewpoint of providing a foamed molded product having more excellent non-ignition property and self-extinguishing property.
[0071] (Phosphonate)
[0072] Phosphonates are esters containing M-PO(OH)2 groups and / or M-PO(OM 1 )2 group (herein, M is a monovalent hydrocarbon group (for example, methyl, benzyl, aryl, alkynyl, propadienyl, vinyl or substituted vinyl, etc.), M 1 Esters and partial esters of hydrocarbon groups (eg, alkyl groups or aryl groups, etc.), and salts thereof.
[0073] Examples of the phosphonic acid ester include alkylphosphonic acid, arylphosphonic acid, and esters thereof; monophosphonic acid ester; acyclic diphosphonic acid ester; and cyclic phosphonic acid ester.
[0074] Among the phosphonates, cyclic phosphonates are preferred, and cyclic bisphosphonates are particularly preferred.
[0075] Examples of the cyclic phosphonate include compounds represented by the following structural formula (i):
[0076]
[0077] In the above structural formula (i), R 1 and R 2 Independently for C 1-4 Alkyl, R 3 H or C 1-4 Alkyl, R 4 C 9-22 Alkyl, C 9-22 Cycloalkyl, C 9-22 Aryl or C 9-22 Aralkyl, and n is 0 or 1.
[0078] The cyclic phosphonate represented by the above structural formula (i) is disclosed in detail in French Patent Application Publication No. 1503429.
[0079] As the cyclic phosphonate, a compound represented by the following structural formula (ii), i.e., a cyclic bisphosphonate, such as pentaerythritol diphosphonate can also be suitably used:
[0080]
[0081] In the above structural formula (ii), A 1 and A 2 Independently for C 1-10 Alkyl, C 2-10 alkenyl, benzyl, phenylethyl, phenyl or naphthyl.
[0082] Cyclic bisphosphonates are disclosed in more detail in US Pat. No. 4,174,343 and UK Patent Application Publication No. 1,515,223.
[0083] From the viewpoint of obtaining a foamed molded article having excellent heat-resistant dimensional stability, among the cyclic bisphosphonates, pentaerythritol diphosphonate represented by the following structural formula (iii) is particularly preferred (for example, AFLAMMIT (registered trademark) PCO 900 (phosphorus content 24%) manufactured by Thor GmbH). Specifically, as the pentaerythritol diphosphonate, 3,9-dimethyl-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane-3,9-dioxide is particularly preferred.
[0084]
[0085] As other cyclic phosphoric acid esters, compounds disclosed in French Patent Application Publication No. 1503429 can be used.
[0086] As the organic phosphorus compound, an organic phosphorus compound having its surface coated (for example, a surface-coated phosphonate or the like) may be used.
[0087] (Hindered Amine)
[0088] In this specification, "hindered amine" refers to a hindered amine having an OR group (here, R is a saturated or unsaturated monovalent hydrocarbon group) directly substituted on the N atom (hereinafter sometimes referred to as an N-substituted hindered amine). The hindered amine is not particularly limited as long as it is a hindered amine having an OR group directly substituted on the N atom, and a known hindered amine can be used. As the hindered amine, one hindered amine may be used alone, or two or more hindered amines may be used in combination.
[0089] In this specification, hindered amines that do not have an OR group substituted directly on the N atom are not considered hindered amines.
[0090] From the viewpoint of being able to exert a flame retardant effect in a wide temperature range, the hindered amine is preferably an N-substituted hindered amine containing a triazine component (hereinafter sometimes referred to as a "triazine skeleton-containing hindered amine"). The hindered amine containing a triazine skeleton is not particularly limited, but preferably (i) a compound with a CAS number of 191680-81-6 ((i-1) a reaction product of a reaction product of peroxidized N-butyl-2,2,6,6-tetramethyl-4-piperidinamine and 2,4,6-trichloro-1,3,5-triazine and cyclohexane and N,N'-bis(3-aminopropyl)ethylenediamine, also referred to as (i-2) a reaction product of 2,4-bis((1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)butylamino)-6-chloro-s-triazine and N,N'-bis(3-aminopropyl)ethylenediamine) The product is also referred to as (i-3) N,N',N"'-tri{2,4-bis[(1-hydrocarbyloxy-2,2,6,6-tetramethylpiperidin-4-yl)alkylamino]-s-triazine-6-yl}-3,3'-ethylenediiminodipropylamine), and / or (ii) bis(1-undecanyloxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate. In addition, isomers of the above-mentioned hindered amine containing a triazine skeleton and derivatives of the above-mentioned hindered amine containing a triazine skeleton by cross-linking can also be used. Regarding the hindered amine containing a triazine skeleton, in more detail, it has been disclosed on page 2, line 32 to page 4, line 6 of the specification of European Patent No. 0889085.
[0091] As the hindered amine containing a triazine skeleton, commercially available products can also be used appropriately. Commercially available products of the hindered amine containing a triazine skeleton include: BASF's FLAMSTAB (registered trademark) NOR116 (a compound with a CAS number of 191680-81-6), CLARIANT's HOSTAVIN (registered trademark) NOW XP, ADEKASTAB LA-81 (bis(1-undecyloxy-2,2,6,6-tetramethylpiperidin-4-yl) carbonate) and the like.
[0092] (Content of organic phosphorus compounds and hindered amines)
[0093] When the present resin particles contain an organic phosphorus compound and a hindered amine as an intumescent flame retardant, the present resin particles contain 3.0 to 20.0% by weight of the organic phosphorus compound, preferably 5.0 to 19.0% by weight, more preferably 7.0 to 18.0% by weight, further preferably 10.0 to 17.0% by weight, and further preferably 13.0 to 16.0% by weight, based on 100% by weight of the total amount of the resin particles. When the resin particles contain (i) 3.0% by weight or more of the organic phosphorus compound, a foamed molded article having excellent flame retardancy can be stably provided, and when the resin particles contain (ii) 20.0% by weight or less, a foamed molded article having no sink mark and excellent strength (e.g., compressive strength) can be provided.
[0094] In addition, the present resin particles preferably contain 1.0 to 10.0% by weight of the hindered amine, more preferably 2.0 to 8.0% by weight, further preferably 2.5 to 7.0% by weight, and further preferably 3.0 to 6.0% by weight, based on 100% by weight of the total amount of the resin particles. When the present resin particles contain (i) more than 1.0% by weight of the hindered amine, a foamed molded article having excellent non-ignition property and self-extinguishing property can be obtained, and when the present resin particles contain (ii) 10.0% by weight or less, adhesion (blocking) between the resin particles can be suppressed in the foaming step described later.
[0095] In order to have the above advantages, the present resin particles preferably contain 3.0 to 20.0 wt % of an organic phosphorus compound and 1.0 to 10.0 wt % of a hindered amine in 100 wt % of the total amount of the resin particles.
[0096] <Other additives>
[0097] The resin particles may optionally contain other additives in addition to the base resin and the intumescent flame retardant as long as the effects of the present invention are not impaired. Other additives include: other flame retardants (except the intumescent flame retardant), UV protection agents (e.g., Tinuvin 622 manufactured by BASF), peroxide scavengers, nucleating agents, antistatic agents, antioxidants (e.g., Irgafos 168, Irganox 1010 manufactured by BASF), light stabilizers, conductive agents, lubricants, fillers, carbon black, powdered activated carbon, etc.
[0098] As other flame retardants, for example, brominated bisphenol A flame retardants, brominated bisphenol S flame retardants, brominated butadiene-styrene block copolymer flame retardants, brominated polyphenylene ether flame retardants, etc. can be included as bromine-based flame retardants, and melamine-based flame retardants can be listed as melamine sulfate, melamine polyphosphate, melamine cyanurate, melamine pyrophosphate, melamine hydrogen bromide, etc. These other flame retardants can be used alone or in combination of two or more.
[0099] The content of other flame retardants in the present resin particles is preferably greater than 0% by weight to 1.00% by weight, more preferably 0.05% by weight to 0.75% by weight, and further preferably 0.10% by weight to 0.50% by weight, in the total amount of 100% by weight of the polypropylene resin particles. It should be noted that the present resin particles contain an expansion flame retardant as an essential component, so even if these other flame retardants are not included, foamed particles that can provide a foamed molded body with excellent flame retardancy can be provided. That is, the content of other flame retardants in the present resin particles can be 0% by weight.
[0100] (Melting point of resin particles)
[0101] The melting point of the resin particles is not particularly limited, but is preferably 122.0°C to 159.0°C, for example.
[0102] <Physical properties of polypropylene foamed particles>
[0103] (Average bubble diameter)
[0104] The average bubble diameter of the present foamed particles is not particularly limited, but is preferably 100 μm to 600 μm, more preferably 150 μm to 450 μm or less, and further preferably 200 μm to 400 μm or less. When the average bubble diameter of the present foamed particles is (i) 100 μm or more, a foamed molded product with excellent surface aesthetics can be obtained. In addition, when (ii) 600 μm or less, the secondary foaming property of the foamed particles during in-mold foaming molding becomes good, and a foamed molded product with excellent surface aesthetics can be obtained. It can also be said that the average bubble diameter of the foamed particles is the unit diameter of the foamed particles. It should be noted that in this specification, the method for determining the average bubble diameter of the foamed particles is as described in the examples.
[0105] (Heat of fusion of foamed particles at high temperature side)
[0106] The high temperature side fusion heat of the present foamed particles is preferably 5.0 J / g to 25.0 J / g, more preferably 8.0 J / g to 20.0 J / g, and further preferably 10.0 J / g to 15.0 J / g. When the high temperature side fusion heat of the foamed particles is (i) 5.0 J / g or more, the generation of shrinkage marks and the shrinkage of the size of the obtained foamed molded body at the surface of the foamed molded body during in-mold foam molding can be suppressed. When it is below 25.0 J / g, a foamed molded body with excellent internal fusion properties and a smooth surface can be obtained. It can also be said that the high temperature side fusion heat is the high temperature side melting peak heat. It should be noted that in this specification, the method for determining the high temperature side fusion heat of the foamed particles is as described in the examples.
[0107] In addition, from the viewpoint of having the advantage of not generating shrinkage marks and surface irregularities due to shrinkage and being able to provide a foamed molded product with excellent surface properties, the foamed particles preferably have at least two melting peaks in the DSC curve obtained by measurement based on the differential scanning calorimeter method. That is, the foamed particles preferably have at least two melting peaks in the DSC curve obtained by measurement based on the differential scanning calorimeter method, and the high temperature side heat of fusion is 5.0 J / g to 25.0 J / g.
[0108] (Density of foamed particles)
[0109] The volume density of the present foamed particles (bulk density of foamed particles) is not particularly limited, but is preferably 15 g / L to 400 g / L, more preferably 60 g / L to 300 g / L, further preferably 70 g / L to 250 g / L, further preferably 80 g / L to 250 g / L, and particularly preferably 90 g / L to 250 g / L. When the volume density of the present foamed particles is (i) 15 g / L or more, there is an advantage that the internal pressure required for molding the foamed particles becomes lower. In addition, when (ii) 400 g / L or less, there is an advantage that a foamed molded product with excellent lightness can be obtained. It should be noted that in this specification, the method for determining the volume density of the foamed particles is as described in the examples.
[0110] In addition, when the present foamed beads are impregnated with air (internal pressure is applied) during molding, the density of the foamed beads means the bulk density of the foamed beads before impregnation with air (before internal pressure is applied).
[0111] [2. Method for producing foamed particles]
[0112] A method for producing foamed beads as one embodiment of the present invention preferably includes: a dispersing step of dispersing polypropylene resin particles, an aqueous dispersion medium and a foaming agent in a container; and a releasing step of releasing the dispersion obtained in the aforementioned dispersing step to a region where the pressure is lower than the pressure in the aforementioned container, wherein the aforementioned polypropylene resin particles contain a base resin and an intumescent flame retardant, and the base resin contains: a polypropylene resin (a) having an MI of 4.00 g / 10.00 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C., and a polypropylene resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135° C. to 155° C.
[0113] In this specification, "the method for producing foamed beads according to one embodiment of the present invention" may be referred to as "the present production method".
[0114] Regarding the resin particles used in the present production method, the description of the above-mentioned [1. Polypropylene-based foamed particles] can be appropriately cited.
[0115] (Granulation process)
[0116] The present production method preferably includes a granulation step of preparing resin particles before the foaming step.
[0117] The granulation step in the present manufacturing method is not particularly limited as long as resin pellets can be obtained, and a known method can be used. As an example of the granulation step, the following methods (S1) to (S3) can be listed: (S1) melt-kneading a specified amount of polypropylene resin (a), polypropylene resin (b) and intumescent flame retardant and other additives as required using an extruder to prepare a melt-kneaded product; (S2) extruding the melt-kneaded product from a die provided in the extruder; (S3) chopping the extruded melt-kneaded product into a desired shape (e.g., cylindrical and spherical) to obtain resin pellets.
[0118] In the above (S1), a predetermined amount of polypropylene resin (a), polypropylene resin (b) and intumescent flame retardant and other additives as required may be blended in advance to prepare a blend. The blend may be supplied to an extruder and melt-kneaded to prepare a melt-kneaded product.
[0119] In the above (S3), before the melt-kneaded product is cut into pieces, the extruded melt-kneaded product may be cooled using a cooling medium such as water to be solidified.
[0120] (Dispersion process)
[0121] The dispersing step can also be said to be a step of preparing a dispersion in which the present resin particles, a foaming agent, and, if necessary, a dispersant and / or a dispersing aid are dispersed in an aqueous dispersion medium.
[0122] The container used in the dispersion step is not particularly limited, but is preferably a container that can withstand the foaming temperature and foaming pressure described below. As the container, for example, a pressure-resistant container is preferred, and an autoclave-type pressure-resistant container is more preferred. The container may be equipped with a stirrer inside the container.
[0123] The aqueous dispersion medium is not particularly limited as long as it can uniformly disperse the resin particles, the foaming agent, and the like.
[0124] Examples of the aqueous dispersion medium include: (a) a dispersion medium obtained by adding methanol, ethanol, ethylene glycol, glycerol, or the like to water; (b) water such as tap water and industrial water; and (c) a solution (aqueous solution) containing a salt such as sodium chloride or sodium sulfate.
[0125] Examples of the foaming agent include: (a) (a-1) inorganic gases such as nitrogen, carbon dioxide, and air (a mixture of oxygen, nitrogen, and carbon dioxide); and (a-2) inorganic foaming agents such as water; and (b) (b-1) saturated hydrocarbons having 3 to 5 carbon atoms such as propane, n-butane, isobutane, n-pentane, isopentane, and neopentane; (b-2) ethers such as dimethyl ether, diethyl ether, and methyl ethyl ether; and (b-3) organic foaming agents such as halogenated hydrocarbons such as monochloromethane, ethyl chloride, and hydrofluoroolefins.
[0126] Among them, the foaming agent is preferably water and / or carbon dioxide from the viewpoint of low environmental load and excellent economic efficiency and safety.
[0127] In the method for producing the foamed particles, it is preferred to use a dispersant (e.g., an inorganic substance such as tricalcium phosphate and kaolin) and a dispersing aid (e.g., an anionic surfactant such as sodium dodecylbenzenesulfonate). According to this configuration, the aggregation (sometimes referred to as adhesion) of the resin particles can be reduced, and the stability of the dispersion in the container can be improved. As a result, there is an advantage that the foamed particles can be produced stably.
[0128] The aqueous dispersion medium and the foaming agent may be used alone or in combination of two or more.
[0129] (Temperature-pressure increase step and holding step)
[0130] In the present production method, preferably, after the dispersion step and before the release step, the following steps are further included: (i) a temperature increase-pressure increase step of increasing the temperature in the container to a certain temperature and increasing the pressure in the container to a certain pressure, and (ii) a holding step of maintaining the temperature and pressure in the container at a certain temperature and a certain pressure. The holding step is preferably implemented after the temperature increase-pressure increase step. In this specification, (a) the certain temperature in the temperature increase-pressure increase step and the holding step is sometimes referred to as the foaming temperature, and (b) the certain pressure is sometimes referred to as the foaming pressure.
[0131] The foaming temperature varies depending on the type of the base resin and the intumescent flame retardant contained in the resin particles, the type of the foaming agent, etc., and therefore cannot be generalized. The foaming temperature is preferably (i) the melting point of the mixture of the base resin and the intumescent flame retardant, (b) the polypropylene resin composition, or (c) the resin particles -20.0°C to the melting point +20.0°C, more preferably (ii) the melting point of the mixture of the base resin and the intumescent flame retardant, (b) the polypropylene resin composition, or (c) the resin particles -10.0°C to the melting point +15.0°C, and further preferably (iii) the melting point of the mixture of the base resin and the intumescent flame retardant, (b) the polypropylene resin composition, or (c) the resin particles -5.0°C to the melting point +13.0°C.
[0132] The foaming pressure is preferably 0.5 MPa (gauge pressure) to 10.0 MPa (gauge pressure), more preferably 0.6 MPa (gauge pressure) to 5.0 MPa (gauge pressure), and more preferably 0.6 MPa (gauge pressure) to 2.5 MPa (gauge pressure). When the foaming pressure is 0.5 MPa (gauge pressure) or more, foamed particles having an appropriate density can be obtained.
[0133] In the holding step, the time (holding time) for holding the dispersion in the container at a temperature near the foaming temperature and the foaming pressure is not particularly limited. The holding time is preferably 10 to 60 minutes, more preferably 12 to 50 minutes, and even more preferably 15 to 40 minutes.
[0134] (Release process)
[0135] The releasing step can be used to foam the resin particles, thereby obtaining foamed particles. The releasing step can also be said to be a step of opening one end of the container and releasing the dispersion in the container to a region (space) where the pressure is lower than the foaming pressure (i.e., the pressure in the container).
[0136] In the release process, "region with a pressure lower than the foaming pressure" means "region under a pressure lower than the foaming pressure" or "space under a pressure lower than the foaming pressure", and can also be said to be "under an atmosphere with a pressure lower than the foaming pressure". The region with a pressure lower than the foaming pressure is not particularly limited as long as it is lower than the foaming pressure, and may be, for example, a region under atmospheric pressure.
[0137] (Foaming process)
[0138] Sometimes, the process from the dispersion process to the release process is called the foaming process. In addition, the process of producing foamed particles from resin particles is called the "primary foaming process", and the obtained foamed particles are called "primary foamed particles".
[0139] (Two-stage foaming process)
[0140] In order to obtain foamed particles with a high expansion ratio, the first-stage foamed particles obtained in the first-stage foaming process can be foamed again. The process of increasing the expansion ratio of the first-stage foamed particles is called a "second-stage foaming process", and the polypropylene foamed particles obtained by the second-stage foaming process are called "second-stage foamed particles". The specific method of the second-stage foaming process is not particularly limited, but a known method can be used.
[0141] [3. Polypropylene foamed product]
[0142] The polypropylene foamed molded article involved in one embodiment of the present invention is a foamed molded article formed by molding the present foamed particles (for example, in-mold foaming molding). In this specification, "the polypropylene foamed molded article involved in one embodiment of the present invention" is sometimes referred to as "the present foamed molded article". It can also be said that the present foamed molded article is formed by molding polypropylene foamed particles, and the polypropylene foamed particles are formed by foaming polypropylene resin particles, and the polypropylene resin particles contain a base resin and an expansion flame retardant, and the base resin contains: a polypropylene resin (a) having an MI of 4.00 g / 10 minutes to 15.00 g / 10 minutes and a melting point of 135°C to 155°C, and a polypropylene resin (b) having an MI of 0.05 g / 10 minutes to 3.00 g / 10 minutes and a melting point of 135°C to 155°C.
[0143] Since the present foamed molded product has the above-mentioned structure, it is excellent in flame retardancy.
[0144] (Flame retardancy of foamed molded article)
[0145] In this specification, the flame retardancy of the foamed molded article can be evaluated by UL94V "Vertical Burning Foam Material Test" (UL94V test). The test method and evaluation criteria of UL94V "Vertical Burning Foam Material Test" are as described in the Examples.
[0146] The present foamed molded product preferably satisfies at least standard V-2 in the UL94V test, more preferably satisfies standard V-1, and particularly preferably satisfies standard V-0. Compared with a foamed molded product that is NG, a foamed molded product that satisfies standard V-2 can be said to be a foamed molded product with excellent flame retardancy, compared with a foamed molded product that only satisfies standard V-2, a foamed molded product that satisfies standard V-1 can be said to be a foamed molded product with more excellent flame retardancy, and compared with a foamed molded product that only satisfies V-2 and / or V-1 or is NG, a foamed molded product that satisfies standard V-0 can be said to be a molded product with particularly excellent flame retardancy.
[0147] In the UL94V test, the foamed molded body that meets the standard V-0 does not continue to burn for more than 10 seconds when it comes into contact with flames, and the cotton wool placed under the test sample does not catch fire due to the particles of the falling test sample. In other words, it can be said that the foamed molded body has excellent self-extinguishing properties: on the basis of further suppressing the combustion of the foamed molded body, even if flammable particles are generated (melted and dripped) during combustion, the fire will be extinguished before reaching the cotton wool (combustible material).
[0148] In the UL94V test, the thickness of the test sample is one of the factors that affect the evaluation result. Even if the test sample is obtained from the same foaming molded body, the thinner the thickness of the test sample, the greater the ratio of the surface area to the volume of the test sample, that is, the ratio of the burning area during combustion increases, and the evaluation of flame retardancy tends to deteriorate. In other words, a foaming molded body that meets the standard of excellent flame retardancy even under the condition that the thickness of the test sample is thinner (e.g., 8mm or 5mm) can be said to be a foaming molded body with more excellent flame retardancy. Therefore, from the viewpoint of providing a foamed molded product having more excellent flame retardancy as the present foamed molded product, in the UL94V test, it is preferred that the standard V-0 be satisfied when the thickness of the test sample is 13 mm and 8 mm, and the standard V-2 be satisfied when the thickness of the test sample is 5 mm. It is more preferred that the standard V-0 be satisfied when the thickness of the test sample is 13 mm and 8 mm, and the standard V-1 be satisfied when the thickness of the test sample is 5 mm. It is particularly preferred that the standard V-0 be satisfied when the thickness of the test sample is 13 mm, 8 mm and 5 mm.
[0149] (Residual weight ratio of foamed molded article)
[0150] In this specification, the flame retardancy of the foamed molded article can also be evaluated by the residual weight ratio of the foamed molded article after the UL94V test. In this specification, the residual weight ratio of the foamed molded article is the weight of the test sample after the UL94V test (after the second combustion) (the weight after combustion), and the residual weight ratio of the foamed molded article can be calculated based on the following formula: Residual weight ratio of foamed molded article (%) = (weight of the test sample after combustion (after UL94V test) / weight of the test sample before combustion (before UL94V test)) × 100.
[0151] The residual weight ratio of foam molding is higher, and it can be said that this foam molding is a foam molding with more excellent flame retardancy.It should be noted that the residual weight ratio of foam molding and the evaluation of UL94V test are equally affected by the thickness of the test specimen.Even if it is the test specimen obtained by the same foam molding, the thickness of the test specimen is thinner, and the residual weight ratio has a lower tendency.
[0152] Therefore, from the viewpoint of providing a foamed molded product having more excellent flame retardancy, the residual weight ratio of the present foamed molded product is (i) preferably 70% or more, more preferably 80% or more, further preferably 85% or more, further preferably 90% or more, and particularly preferably 95% or more when the thickness of the test sample is 13 mm, (ii) preferably 50% or more, more preferably 60% or more, further preferably 70% or more, further preferably 75% or more, and particularly preferably 80% or more when the thickness of the test sample is 8 mm, and (iii) preferably 40% or more, more preferably 50% or more, further preferably 60% or more, further preferably 70% or more, and particularly preferably 75% or more when the thickness of the test sample is 5 mm.
[0153] About the flame retardancy of foaming molding, the density of foaming molding is also one of the factors that the test result of UL94V test and the measurement result of residual weight ratio are affected. The density of foaming molding is less, and the amount of the component (base resin and flame retardant) of the foamed particles contained in this foaming molding is less, and it becomes difficult to enjoy the reasons such as the flame retardancy improvement effect brought by the composition of these base resins and the use of flame retardant, and the evaluation of flame retardancy has a tendency to deteriorate. Therefore, between the foaming moldings with greatly different densities, it is impossible to simply compare the test result of UL94V test and the measurement result of residual weight ratio. Therefore, for this foaming molding, "excellent flame retardancy" refers to compared with the foaming molding (not satisfying the foaming molding of one embodiment of the present invention) with equal density, with more excellent flame retardancy.
[0154] (Density of foamed molded article)
[0155] The density of this foaming molded product is preferably 15g / L~400g / L, preferably 50g / L~300g / L, and preferably 98g / L~200g / L. If the density of the foaming molded product is above 15g / L, the surface of the foaming molded product is smooth and has no shrink marks, and a foaming molded product with more excellent surface aesthetics can be obtained. When it is below 400g / L, a foaming molded product with sufficient light weight can be obtained. In addition, especially when the density of the foaming molded product is above 98g / L, in the UL94V test, even when the thickness of the test sample is 5mm, a foaming molded product with more excellent flame retardancy that can meet the V-0 standard can be provided, so it is preferred. It should be noted that in this specification, the method for measuring the density of the foaming molded product is as described in the examples.
[0156] <Method for producing foamed molded article>
[0157] The method for producing the foamed molded article is not particularly limited as long as the foamed particles can be molded (preferably in-mold foaming) to obtain the foamed molded article, but known methods can be applied. As the method for producing the foamed molded article, for example, the method described in the <Method for producing a foamed molded article> of International Publication WO2022 / 149538 can be suitably adopted.
[0158] One embodiment of the present invention may include the following configurations.
[0159] [1] A polypropylene foamed particle obtained by foaming a polypropylene resin particle, wherein the polypropylene resin particle comprises a base resin and an intumescent flame retardant, wherein the base resin comprises: a polypropylene resin (a) having an MI of 4.00 g / 10 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C., and a polypropylene resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135° C. to 155° C.
[0160] [2] The polypropylene foamed beads according to [1], wherein the polypropylene resin (a) and the polypropylene resin (b) are random polypropylene resins.
[0161] [3] The polypropylene foamed particles according to [1] or [2], wherein the polypropylene resin (b) is contained in an amount of 5 to 80% by weight based on 100% by weight of the base resin.
[0162] [4] The polypropylene foamed beads according to any one of [1] to [3], wherein the expandable flame retardant comprises an organic phosphorus compound and a hindered amine.
[0163] [5] The polypropylene foamed particles according to [4], wherein the polypropylene resin particles contain 3.0 wt% to 20.0 wt% of an organic phosphorus compound and 1.0 wt% to 10.0 wt% of a hindered amine per 100 wt% of the polypropylene resin particles.
[0164] [6] The polypropylene foamed particles according to [4] or [5], wherein the organophosphorus compound is one or more selected from the group consisting of phosphonates, organophosphites, organophosphinites, metal salts of phosphinic acid, metal salts of diphosphinic acid, phosphite salts and polyol phosphate alcohols.
[0165] [7] The polypropylene foamed beads according to any one of [4] to [6], wherein the organic phosphorus compound is a cyclic phosphonate.
[0166] [8] The polypropylene foamed beads according to any one of [1] to [7], wherein the weight average molecular weight of the polypropylene resin (b) is 80×10 4 above.
[0167] [9] The polypropylene foamed beads according to any one of [1] to [8], wherein the polypropylene resin (b) is a linear polypropylene resin.
[0168]
[10] The polypropylene foamed particles according to any one of [1] to [9], wherein the bulk density is 15.0 g / L to 400.0 g / L.
[0169]
[11] The polypropylene foamed particles according to any one of [1] to
[10] , which have at least two melting peaks in a DSC curve measured by a differential scanning calorimeter method, and a high temperature side heat of fusion of 5.0 J / g to 25.0 J / g.
[0170]
[12] The polypropylene foamed beads according to any one of [1] to
[11] , wherein the polypropylene resin (a) and / or the polypropylene resin (b) is an ethylene / propylene random copolymer.
[0171]
[13] The polypropylene foamed beads according to any one of [1] to
[12] , wherein the average cell diameter is 100 μm to 600 μm.
[0172]
[14] The polypropylene foamed beads according to any one of [1] to
[13] , wherein the polypropylene resin (a) is contained in an amount of 20 to 95% by weight in 100% by weight of the base resin.
[0173]
[15] A polypropylene foamed molded product obtained by in-mold foaming of the polypropylene foamed particles described in any one of [1] to
[14] .
[0174]
[16] The polypropylene foamed molded product according to
[15] , which has a bulk density of 15.0 g / L to 400.0 g / L.
[0175]
[17] The polypropylene foam molded product according to
[15] or
[16] , which satisfies standard V-2 in the UL94V test.
[0176]
[18] The polypropylene foam molded product according to any one of
[15] to
[17] , which satisfies standard V-1 in the UL94V test.
[0177]
[19] The polypropylene foam molded product according to any one of
[15] to
[18] , which satisfies standard V-0 in the UL94V test.
[0178]
[20] A method for producing polypropylene foamed particles, comprising: a dispersion step of dispersing polypropylene resin particles, an aqueous dispersion medium and a foaming agent in a container; and a release step of releasing the dispersion obtained in the aforementioned dispersion step to a region where the pressure is lower than the pressure in the aforementioned container, the aforementioned polypropylene resin particles comprising a base resin and an expandable flame retardant, the base resin comprising: a polypropylene resin (a) having an MI of 4.00 g / 10.00 min to 15.00 g / 10 min and a melting point of 135°C to 155°C, and a polypropylene resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135°C to 155°C.
[0179]
[21] The method for producing polypropylene foamed beads according to
[20] , wherein the polypropylene resin (a) and the polypropylene resin (b) are random polypropylene resins.
[0180]
[22] The method for producing polypropylene foamed particles according to
[20] or
[21] , wherein the polypropylene resin (b) is contained in an amount of 5 to 80% by weight in 100% by weight of the base resin.
[0181]
[23] The method for producing polypropylene foamed beads according to any one of
[20] to
[22] , wherein the intumescent flame retardant comprises an organic phosphorus compound and a hindered amine.
[0182]
[24] The method for producing polypropylene foamed particles according to
[23] , wherein the polypropylene resin particles contain 3.0 wt% to 20.0 wt% of an organic phosphorus compound and 1.0 wt% to 10.0 wt% of a hindered amine in 100 wt% of the polypropylene resin particles.
[0183]
[25] The method for producing polypropylene foamed particles according to
[23] or
[24] , wherein the aforementioned organic phosphorus compound is one or more selected from the group consisting of phosphonates, organic phosphites, organic hypophosphites, metal salts of hypophosphinic acid, metal salts of diphosphinic acid, phosphites and polyol phosphate alcohols.
[0184]
[26] The method for producing polypropylene foamed beads according to any one of
[23] to
[25] , wherein the organic phosphorus compound is a cyclic phosphonate.
[0185]
[27] The method for producing polypropylene foamed beads according to any one of
[20] to
[26] , wherein the weight average molecular weight of the polypropylene resin (b) is 80×10 4 above.
[0186]
[28] The method for producing polypropylene foamed beads according to any one of
[20] to
[27] , wherein the polypropylene resin (b) is a linear polypropylene resin.
[0187]
[29] The method for producing polypropylene foamed particles according to any one of
[20] to
[28] , wherein the polypropylene resin (a) and / or the polypropylene resin (b) is an ethylene / propylene random copolymer.
[0188]
[30] The method for producing polypropylene foamed beads according to any one of
[20] to
[29] , wherein the polypropylene resin (a) is contained in an amount of 20% to 95% by weight in 100% by weight of the base resin.
[0189]
[31] The method for producing polypropylene foamed particles according to any one of
[20] to
[30] , wherein the foaming agent is water and / or carbon dioxide.
[0190] Example
[0191] Hereinafter, the present invention will be specifically described by way of examples, but the technical scope of the present invention is not limited to these examples.
[0192] [Material]
[0193] The materials used in Examples and Comparative Examples are as follows.
[0194] <Base resin>
[0195] (Polypropylene resin (a))
[0196] Polypropylene (a1): linear ethylene / propylene random copolymer, MI = 7.00 g / 10 min, melting point 144°C, ethylene content 3.2%, Mw = 44 × 10 4
[0197] (Polypropylene resin (b))
[0198] Polypropylene (b1): linear ethylene / propylene random copolymer, MI = 0.48 g / 10 min, melting point 142 °C, ethylene content 3.5%, Mw = 121 × 10 4
[0199] Polypropylene (b2): linear ethylene / propylene random copolymer, MI = 0.51 g / 10 min, melting point 149 ° C, ethylene content 2.5%, Mw = 116 × 10 4
[0200] <Intumescent flame retardants>
[0201] (Organophosphorus compounds)
[0202] AFLAMMIT (registered trademark) PCO900 (cyclic phosphonate) manufactured by Thor GmbH
[0203] (Hindered Amine)
[0204] BASF FLAMESTAB (registered trademark) NOR116 (compound with CAS number 191680-81-6)
[0205] <Other additives>
[0206] (Nucleating Agent)
[0207] Talc powder PK-S manufactured by Lin Huacheng Co., Ltd.
[0208] (Antioxidant)
[0209] Irgafos 168 manufactured by BASF
[0210] Irganox 1010 manufactured by BASF
[0211] (UV protection agent)
[0212] Tinuvin 622 manufactured by BASF
[0213] <Foaming agent>
[0214] Carbon dioxide: Made by AIR WATER Co., Ltd.
[0215] <Dispersant>
[0216] BASF Kaolin ASP-170
[0217] Tricalcium phosphate produced by Taiping Chemical Company
[0218] <Dispersing aid>
[0219] DBS G-15 manufactured by Kao Corporation
[0220] It should be noted that the dispersant and the dispersing aid are added to the dispersion or the pressure-resistant sealed container in the dispersion step described later, so they will not remain in the resin particles and the foamed particles or only remain in a trace amount. In addition, the carbon dioxide used as the foaming agent will be emitted from the obtained foamed particles due to the high gas permeability of the foamed particles.
[0221] [Measurement method]
[0222] The evaluation methods performed in Examples and Comparative Examples are described below.
[0223] (MI of polypropylene resins (polypropylene resin (a) and polypropylene resin (b)))
[0224] The MI of the polypropylene resin was measured using the MI measuring instrument described in JIS K7210:1999, with an orifice diameter of The measurement was performed under the conditions of an orifice length of 8.000±0.025 mm, a load of 2160 g, and a temperature of 230±0.2°C.
[0225] (Measurement of average cell diameter of foamed particles)
[0226] The method for determining the average bubble diameter of the foamed particles is as described in the following (1) to (5): (1) using a razor (Hi-Stainless Double Edge Blade manufactured by FEATHER Co., Ltd.) to cut the foamed particles in a manner that passes through the center of the foamed particles; (2) using an optical microscope (VHX-5000 manufactured by KEYENCE Co., Ltd.) to observe the cross section of the obtained foamed particles at a magnification of 50 times; (3) in the image obtained by observation, draw a straight line passing through the center or approximately the center of the cross section of the foamed particles; (4) (4-1) determining the number of bubbles n existing on the straight line, (4-2) determining the length of the line segment cut from the straight line based on the intersection of the straight line and the surface of the foamed particles, as the foamed particle diameter L; (5) calculating the average bubble diameter of the foamed particles by the following formula:
[0227] Average bubble diameter (μm) = L / n.
[0228] (Heat of fusion of foamed particles at high temperature side)
[0229] The high temperature side fusion heat of the foamed particles is as described in the following (1) to (5): (1) about 5 mg of foamed particles are measured; (2) the temperature of the measured foamed particles is increased from 10°C to 190°C at a heating rate of 10°C / min in a measurement using a differential scanning calorimeter method to melt the foamed particles; (3) in the DSC curve of the foamed particles obtained by the process of the above (2), a straight line is connected to form a baseline by connecting the point indicating the temperature before the start of melting and the point indicating the temperature after the end of melting; (4) a straight line is drawn in a direction perpendicular to the X-axis through the maximum point between the melting peak on the high temperature side or the highest temperature melting peak and the adjacent melting peak; (5) the heat (J / g) calculated from the area on the high temperature side surrounded by the baseline, the straight line passing through the maximum point and the DSC curve is taken as the high temperature side fusion heat of the foamed particles.
[0230] (Volume density of foamed particles)
[0231] The bulk density of the foamed beads is determined by the following methods (1) to (3): (1) The foamed beads are placed in a volume V (cm 3 ) container until the foamed particles overflow from the container; (2) scraping the powder surface (upper end) of the container and measuring the weight W (g) of the foamed particles in the container; (3) calculating the volume density of the foamed particles by the following formula: Volume density of foamed particles (g / L) = weight W (g) of foamed particles / {volume V (cm 3 ) / 1000}.
[0232] (Density of foamed molded article)
[0233] The method for measuring the density of the foamed molded article is as described in the following (1) to (3); (1) measuring the length (mm), width (mm) and thickness (mm) of the foamed molded article, and calculating the volume V (L) of the foamed molded article; (2) measuring the weight W (g) of the foamed molded article; (3) calculating the density of the foamed molded article based on the following formula:
[0234] Density of foamed molded article (g / L)=W / V.
[0235] (Surface properties of foamed molded article)
[0236] The obtained foamed molded body was visually observed, and the surface properties of the foamed molded body were evaluated according to the following criteria:
[0237] Good (○): There is almost no intergranular gap (gaps between foamed particles) in the foamed body as a whole, and the surface is not conspicuous and has no wrinkles or shrinkage;
[0238] Slightly poor (△): A small amount of intergranular gaps, surface irregularities, wrinkles and / or shrinkage can be seen on the entire foamed product;
[0239] Poor (×): The foamed molded product has a large number of intergranular gaps, surface irregularities, wrinkles, and / or shrinkage evident throughout the foamed molded product.
[0240] (Flame retardancy and residual weight ratio of foamed molded article)
[0241] The flame retardancy of the foamed molded article was measured and evaluated by the UL94V "vertical burning test" and the residual weight ratio.
[0242] (UL94V "vertical burning test")
[0243] The test method of the UL94V "vertical combustion test" is as follows (1) to (5): (1) A test sample having a specific size (length 125±5 mm×width 13±0.5 mm) and a specific thickness (thickness (t) of the test sample = 13 mm, 8 mm, or 5 mm) is cut out from the foam molded product; (2) The upper part of the cut test sample is fixed by a fixing fixture, the test sample is held vertically, and absorbent cotton is placed directly below it; (2) The lower end of the held test sample is brought into contact with the flame of a gas burner for 10 seconds to cause it to burn (first combustion); (3) The burning time and red-hot time of the test sample are measured, and if the burning stops within 30 seconds, the lower end of the test sample is brought into contact with the flame of a gas burner for 10 seconds to cause it to burn (second combustion); (4) The burning time and red-hot time of the test sample are measured again; (5) The test sample is changed, and the operations of (1) to (4) are repeated a total of 5 times, and the flame retardancy is evaluated according to the following evaluation criteria.
[0244] Evaluation Criteria
[0245] [NG (failure)]: During the first or second combustion, the sample continues to burn for more than 30 seconds, or there is a sample that burns to the position of the fixing fixture;
[0246] [V-2]: The sample does not continue to burn for more than 30 seconds after the first contact with the flame.
[0247] The total burning time of 5 samples after 10 exposures to flame is less than 250 seconds.
[0248] The sample that has not burned to the position of the fixing fixture,
[0249] After the second exposure to flame, no sample has a sum of burning time and red-hot time of more than 250 seconds, and
[0250] There are samples where the absorbent cotton placed under the test sample is ignited due to particles of the test sample falling during combustion;
[0251] [V-1]: The sample did not continue to burn for more than 30 seconds after the first and second flame exposure.
[0252] The total burning time of 5 samples after 10 exposures to flame is less than 250 seconds.
[0253] The sample that has not burned to the position of the fixing fixture,
[0254] After the second exposure to flame, no sample has a sum of burning time and red-hot time of more than 250 seconds, and
[0255] The sample in which the absorbent cotton placed under the test sample does not catch fire due to the particles of the fallen test sample during any burning;
[0256] [V-0]: The sample does not continue to burn for more than 10 seconds after the first and second flame exposure.
[0257] The total burning time of 5 samples after 10 times of exposure to flame is less than 50 seconds.
[0258] The sample that has not burned to the position of the fixing fixture,
[0259] After the second exposure to flame, no sample has a sum of burning time and red-hot time of more than 30 seconds, and
[0260] In any of the burning cases, there was no case where the absorbent cotton placed under the test specimen caught fire due to the fallen particles of the test specimen.
[0261] (Residual weight ratio)
[0262] For the test sample after the UL94V test (after the second combustion), the weight of the test sample (weight after combustion) was measured, and the residual weight ratio of the foamed molded article was calculated based on the following formula:
[0263] Remaining weight ratio (%) of the foamed article=(weight of the test sample after combustion (after UL94V test) / weight of the test sample before combustion (before UL94V test))×100.
[0264] [Example 1]
[0265] (Production of polypropylene resin pellets)
[0266] The components are dry-blended in such a manner that, in 100 wt % of the blend, as base resin, the polypropylene resin (a1) accounts for 29.6 wt %, and the polypropylene resin (b1) accounts for 50.0 wt %; as intumescent flame retardants, the organic phosphorus compound accounts for 15.0 wt %, and the hindered amine accounts for 5.0 wt %; as other additives, the talcum powder PK-S as a nucleating agent accounts for 0.1 wt %, the Irgafos 168 as an antioxidant accounts for 0.133 wt %, the Irganox 1010 accounts for 0.067 wt %, and the Tinuvin 622 as a UV inhibitor accounts for 0.1 wt % (the other additives account for a total of 0.4 wt %).
[0267] The obtained blend was put into a twin-screw extruder [TEM26SX manufactured by Shibaura Machinery] and melt-kneaded at a resin temperature of 200° C. The melt-kneaded polypropylene resin composition was extruded into a strand shape through a die having a circular hole installed at the front end of the extruder. The extruded polypropylene resin composition was water-cooled and then cut with a cutter to obtain resin pellets (granulation step).
[0268] (Production of polypropylene foam particles)
[0269] 100 parts by weight of the obtained resin particles, 442 parts by weight of pure water, 1.1 parts by weight of tricalcium phosphate as a dispersant, 0.22 parts by weight of kaolin ASP-170 and 0.027 parts by weight of DBS as a dispersing aid are placed in a pressure-resistant sealed container. Then, while stirring the raw materials in the pressure-resistant sealed container, 2.1 parts by weight of carbon dioxide as a foaming agent is introduced into the aforementioned pressure-resistant sealed container to prepare a dispersion (dispersion process). Next, the temperature in the pressure-resistant sealed container is heated to a foaming temperature of 150.2°C. Then, additional carbon dioxide is pressurized into the pressure-resistant sealed container to increase the pressure in the pressure-resistant sealed container to a foaming pressure of 1.1 MPa (gauge pressure) (temperature-pressure increase process). Next, after the pressure-resistant sealed container is kept at the aforementioned foaming temperature and foaming pressure for 20 minutes (maintaining process), the valve at the bottom of the sealed container is opened, and the dispersion is released through an orifice with a diameter of 3.6 mm to the foaming tube under atmospheric pressure to obtain foamed particles (releasing process). At this time, during the release of the dispersion, in order to make the pressure in the pressure-resistant sealed container not lower than the foaming pressure, additional carbon dioxide is pressed into the pressure-resistant sealed container to maintain the pressure in the pressure-resistant sealed container at 1.1 MPa (gauge pressure). After the obtained foamed particles are dried at 60°C for 6 hours, the average bubble diameter, the heat of fusion on the high temperature side and the bulk density (bulk density of foamed particles) are measured. The results are shown in Table 1. It should be noted that the obtained foamed particles contain 15.0% by weight of organic phosphorus compounds and 5.0% by weight of hindered amines relative to the total amount of the foamed particles (100% by weight).
[0270] (Production of Polypropylene Foam Molded Article)
[0271] The obtained foamed particles are put into a pressure-resistant sealed container, and air is introduced into the pressure-resistant sealed container, so that the foamed particles in the pressure-resistant sealed container are impregnated with pressurized air, and the foamed particles are given an internal pressure (absolute pressure) of 0.25MPa (absolute pressure) of the foamed particles. Using a molding machine (a polypropylene in-mold foaming molding machine made by DAISEN Co., Ltd.), the foamed particles impregnated with air are heated and molded with water vapor of 0.32MPa (gauge pressure), thereby obtaining a foamed molded body. After the obtained foamed molded body is placed at room temperature for 1 hour, it is aged and dried for 12 hours in a constant temperature chamber of 75°C, and placed at room temperature again for 4 hours. Then, using the above method, the density, surface properties, flame retardancy and residual weight ratio of the obtained foamed molded body are measured / evaluated. The results are shown in Table 1.
[0272] [Examples 2 to 12, Comparative Examples 1 to 8]
[0273] Resin particles, foamed particles and foamed molded products were obtained in the same manner as in Example 1 except that the amounts of the components and / or the foaming conditions were changed as shown in Tables 1 to 4, and the physical properties were measured and evaluated. The results are shown in Tables 1 to 4.
[0274] It should be noted that in Examples 9 and 10, the obtained foamed beads were subjected to two-stage foaming according to the following steps, and the obtained two-stage foamed beads were molded to obtain a foamed molded article.
[0275] (Production of polypropylene foamed particles (two-stage foamed particles))
[0276] After drying the obtained foamed particles (one-stage foamed particles) at 60°C for 6 hours, put them into a pressure-resistant sealed container. Air is introduced into the pressure-resistant sealed container to impregnate the one-stage foamed particles in the pressure-resistant sealed container with pressurized air, and the one-stage foamed particles are given an internal pressure (absolute pressure) of 0.30MPa (absolute pressure). About 20L of the one-stage foamed particles impregnated with air (given an internal pressure of the foamed particles) are put into the foaming machine. Next, the one-stage foamed particles in the foaming machine are heated with water vapor of 0.10MPa (gauge pressure) for 30 seconds, so that the one-stage foamed particles are further foamed (two-stage foaming) to obtain foamed particles (two-stage foamed particles). The density of the obtained two-stage foamed particles is shown in Table 3.
[0277] In addition, in all Examples (Examples 1 to 12) and Comparative Examples (Comparative Examples 1 to 9), the obtained foamed beads had two melting peaks in the DSC curve obtained by the differential scanning calorimetry method (DSC method).
[0278] [Table 1]
[0279]
[0280] [Table 2]
[0281]
[0282] [Table 3]
[0283]
[0284] [Table 4]
[0285]
[0286] [Summarize]
[0287] According to Tables 1 to 4, in each embodiment / comparative example, by comparing the foamed molded products with the same density, it can be seen that the foamed molded products formed by in-mold foaming of the foamed particles have excellent flame retardancy. Specifically, as described in the following (1) to (4):
[0288] (1) According to the comparison between the foamed molded bodies of Examples 1 and 2 and the foamed molded body of Comparative Example 1, the foamed molded body of Comparative Example 1 was evaluated as NG when the thickness (t) of the test specimen was 5 mm. In contrast, the foamed molded body of Example 1, which was formed by in-mold foaming of the present foaming particles, met the standard V-0 even when t was 5 mm. In addition, although the amount of organic phosphorus compound added to the foamed molded body of Example 2 was a relatively small 13% by weight, it met the standard V-2 even when t was 5 mm. Furthermore, it can be seen that the foamed molded bodies of Examples 1 and 2 both have a high residual weight ratio and have excellent flame retardancy;
[0289] (2) According to the comparison between the foamed molded body of Example 3 and the foamed molded body of Comparative Example 2, the foamed molded body of Comparative Example 2 was evaluated as NG when the thickness (t) of the test sample was 5 mm. In contrast, although the foamed molded body density of Example 3 obtained by in-mold foaming of the present foamed particles was relatively light at 167 g / L, it satisfied the V-0 standard even when t was 5 mm, and the residual weight ratio was also high, indicating excellent flame retardancy.
[0290] (3) According to the comparison between the foamed molded bodies of Examples 4 and 5 and the foamed molded body of Comparative Example 3, the foamed molded body of Comparative Example 3 was evaluated as NG when t was 5 mm. On the other hand, the foamed molded bodies of Examples 4 and 5 obtained by in-mold foaming of the present foamed particles satisfied the standard V-2 or higher even when t was 5 mm, and also had a high residual weight ratio, showing excellent flame retardancy.
[0291] (4) According to the comparison between the foamed molded bodies of Examples 6 and 7 and the foamed molded bodies of Comparative Examples 4 and 5, it can be seen that the foamed molded bodies of Comparative Examples 4 and 5 were rated V-2 when t was 13 mm and 8 mm, and were rated NG when t was 5 mm. In contrast, the foamed molded bodies of Examples 6 and 7 obtained by in-mold foaming of the present foamed particles satisfied the standard of V-0 or higher when t was 13 mm and 8 mm, and also had a high residual weight ratio, showing excellent flame retardancy.
[0292] (5) According to the comparison between the foamed molded bodies of Examples 8 to 10 and the foamed molded bodies of Comparative Examples 6 and 7, the foamed molded bodies of Comparative Examples 6 and 7 were evaluated as NG even when t was 13 mm due to their low density. In contrast, although the foamed molded bodies of Examples 8 to 10 had a relatively low density of 80 g / L or less, they were able to satisfy the standard V-2 when t was 13 mm. This shows that the foamed molded body obtained by in-mold foaming of the present foamed particles can exhibit flame retardancy even at a relatively low density, which is generally difficult to impart flame retardancy to.
[0293] (6) According to the comparison between the foamed molded bodies of Examples 11 and 12 and the foamed molded bodies of Comparative Examples 8 and 9, the foamed molded bodies of Comparative Examples 8 and 9 were rated as V-2 when t was 13 mm, whereas the foamed molded bodies of Examples 11 and 12 were able to satisfy the standard V-0 when t was 13 mm. It can be seen from this that the foamed molded body formed by in-mold foaming of the present foamed particles can exhibit excellent flame retardancy even when the amount of flame retardant used is small.
[0294] Industrial Applicability
[0295] By performing in-mold foaming molding on the polypropylene foam particles according to one embodiment of the present invention, a polypropylene foam molded body having excellent flame retardancy can be provided. The polypropylene foam molded body having excellent flame retardancy can be used for various purposes such as cushioning packaging materials, logistics materials, heat insulation materials, civil engineering and construction components, and automobile components, and can be particularly suitably used in various fields such as transportation, buildings, structures, furniture, electrical equipment, and electronic equipment that require strict flame retardancy standards.
Claims
1. A polypropylene foamed particle, which is obtained by foaming a polypropylene resin particle, wherein the polypropylene resin particle comprises a base resin and an expansion flame retardant, The base resin comprises: a polypropylene resin (a) having an MI of 4.00 g / 10 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C., and A polypropylene resin (b) having an MI of 0.05 to 3.00 g / 10 minutes and a melting point of 135 to 155°C.
2. The polypropylene foamed particles according to claim 1, in, The polypropylene-based resin (a) and the polypropylene-based resin (b) are each a random copolymer.
3. The polypropylene foamed particles according to claim 1 or 2, in, The polypropylene resin (b) is contained in 100% by weight of the base resin in an amount of 5% to 80% by weight.
4. The polypropylene foamed particles according to any one of claims 1 to 3, in, The intumescent flame retardant includes an organic phosphorus compound and a hindered amine.
5. The polypropylene foamed particles according to claim 4, in, The polypropylene resin particles contain, in 100% by weight of the polypropylene resin particles: 3.0 wt% to 20.0 wt% of an organic phosphorus compound, and Hindered amine 1.0 wt% to 10.0 wt%.
6. The polypropylene foamed particles according to claim 4 or 5, in, The organic phosphorus compound is a cyclic phosphonate.
7. The polypropylene foamed particles according to any one of claims 1 to 6, in, The weight average molecular weight of the polypropylene resin (b) is 80×10 4 above.
8. The polypropylene foamed particles according to any one of claims 1 to 7, in, The polypropylene-based resin (b) is a linear polypropylene-based resin. 9 . The polypropylene foamed particles according to claim 1 , wherein the bulk density is 15 g / L to 400 g / L. The polypropylene foamed beads according to any one of claims 1 to 9, which have at least two melting peaks in a DSC curve measured by a differential scanning calorimeter method, and have a high temperature side heat of fusion of 5.0 J / g to 25.0 J / g.
11. The polypropylene foamed particles according to any one of claims 1 to 10, in, The polypropylene resin (a) and / or the polypropylene resin (b) is an ethylene / propylene random copolymer. 12 . The polypropylene foamed beads according to claim 1 , wherein the average cell diameter is 100 μm to 600 μm.
13. A polypropylene foamed molded product obtained by subjecting the polypropylene foamed particles according to any one of claims 1 to 12 to in-mold foaming. 14 . The polypropylene foamed molded product according to claim 13 , which has a bulk density of 15 g / L to 400 g / L.
15. A method for producing polypropylene foamed particles, wherein include: A dispersing step, in which polypropylene resin particles, an aqueous dispersion medium and a foaming agent are dispersed in a container; as well as a releasing step of releasing the dispersion obtained in the dispersing step to a region where the pressure is lower than the pressure in the container, The polypropylene resin particles include a base resin and an intumescent flame retardant. The base resin comprises: a polypropylene resin (a) having an MI of 4.00 g / 10.00 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C., and A polypropylene resin (b) having an MI of 0.05 to 3.00 g / 10 minutes and a melting point of 135 to 155°C.