Flame retardant copolyester composition

By using additives such as metal phosphinates and drip inhibitors in copolyesters, combined with impact modifiers and compatibilizers, the problem of flame retardants affecting impact resistance and glass transition temperature is solved, and the problem of flame retardants affecting impact resistance and glass transition temperature is achieved. Copolyester compositions with efficient flame retardancy and impact resistance.

CN118946633APending Publication Date: 2024-11-12EASTMAN (CHINA) INVESTMENT MANAGEMENT CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202280093827.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When existing copolyesters meet fire resistance standards, the use of flame retardant will affect their impact resistance and glass transition temperature, and traditional halogen compounds have bioaccumulation problems or cause material embrittlement.

Method used

Combining the impact modifier and A copolyester composition with good flame retardancy and impact resistance was prepared.

Benefits of technology

It achieves the high impact strength and glass transition temperature while meeting the UL94 V-0 level, avoiding the embrittlement problem of traditional flame retardants, and improving the durability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005048904700000281
    Figure BDA0005048904700000281
  • Figure BDA0005048904700000291
    Figure BDA0005048904700000291
  • Figure BDA0005048904700000292
    Figure BDA0005048904700000292
Patent Text Reader

Abstract

The present invention relates to the combination of certain flame retardant additives in copolyesters to improve the flame retardant properties of copolyester compositions while maintaining thermal and impact properties, as well as to methods of making the copolyester compositions and articles made from the copolyester compositions. More specifically, the present invention relates to the use of metal phosphinate flame retardant compounds in copolyester compositions to improve flame retardant properties while surprisingly maintaining glass transition temperature and impact properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the use of certain combinations of additives in copolyesters to improve the flame retardant properties of the copolyester composition while having high impact properties. More specifically, the present invention relates to the use of non-halogenated flame retardants in copolyesters to improve the flame retardant properties while having acceptable impact resistance and glass transition temperature. Background Art

[0002] Flame retardant materials are added to some polymers to improve flame retardancy, especially to meet specific fire standards such as UL94V-2. However, adding flame retardant materials in amounts sufficient to meet fire standards may have a deleterious effect on the impact resistance and glass transition temperature of copolyesters containing effective amounts of flame retardant materials. Furthermore, adding many flame retardant materials will not meet UL94V-0 or better fire standards, let alone maintain the necessary physical properties of the polymer composition, no matter how much is used.

[0003] Copolyesters can be made flame retardant in a variety of ways, but these methods have some disadvantages. Certain halogen compounds such as Dechlorane Decabromodiphenyl oxide or decabromodiphenyl ether can be effective flame retardants, but may be objectionable in the market due to potential problems regarding bioaccumulation. Other halogen compounds may not have the same disadvantages, but may cause embrittlement when used in an amount sufficient to flame retard the copolyester. Liquid phosphorus compounds such as triphenyl phosphite or triphenyl phosphate can make the copolyester flame retardant, but at effective amounts, they plasticize and soften the copolyester, thereby reducing heat deformation resistance. Melamine and phosphorus solid flame retardants can also be used alone, but in the past, reaching the concentration required for flame retardancy made the copolyester brittle or reduced tensile strength characteristics. Plastics used in many applications, such as electronic applications, housings of handheld and fixed appliances, and housings or shells of handheld and fixed power tools, all have flammability requirements specified in various specifications or standards. In addition to flammability requirements, these applications also have durability or physical property requirements.

[0004] There is a need for improved copolyester compositions comprising effective flame retardants that exhibit good flame retardancy and good impact resistance. Summary of the invention

[0005] Applicants have unexpectedly discovered an improved copolyester composition comprising an effective amount of certain non-halogenated flame retardants useful for making articles such as films, sheets, molded parts or profiles that exhibit good flame retardancy while maintaining glass transition temperature and impact resistance.

[0006] In one aspect, a copolyester composition is provided, comprising:

[0007] (a) from about 50 wt % to about 95 wt % of a copolyester comprising:

[0008] (i) a diacid component comprising

[0009] 70 mol % to 100 mol % of terephthalic acid residues,

[0010] 0-30 mol% of a modified aromatic diacid residue having 8 to 12 carbon atoms, and

[0011] 0-10 mol% of aliphatic dicarboxylic acid residues; and

[0012] (ii) a diol component comprising

[0013] 45 mol% to 95 mol% of cyclohexanedimethanol (CHDM) residues

[0014] 5 mol% to 65 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues, and

[0015] 0 to 10 mol % of a modifying diol having 2 to 20 carbon atoms;

[0016] The copolyesters have an inherent viscosity of about 0.5 to 1.2 dL / g, as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C.

[0017] wherein wt% is based on the weight of the copolyester, and

[0018] wherein the total mol% of the dicarboxylic acid components is 100 mol%, and the total mol% of the diol components is 100 mol%;

[0019] (b) from about 10 wt % to about 20 wt % of a flame retardant additive comprising a metal phosphinate compound; and

[0020] (c) from about 0.05 wt % to about 0.5 wt % of a drip suppressant additive;

[0021] wherein the copolyester composition has a UL 94 V-0 rating or better; and

[0022] The copolyester composition has a notched Izod impact strength of 60 Joules / m or more measured according to ASTM D256.

[0023] In an embodiment, the copolyester composition further comprises: (d) about 1 wt% to about 10 wt% of an impact modifier component. In certain embodiments, the impact modifier component comprises an ethylene acrylate glycidyl methacrylate (EA-GMA) impact modifier.

[0024] In an embodiment, the copolyester composition further comprises: (e) about 0.1 wt% to about 5 wt% of a compatibilizer. In an embodiment, the compatibilizer comprises a silicone compatibilizer, such as a phenyl silicone resin. In an embodiment, the phenyl silicone resin is a liquid at 25°C.

[0025] In certain embodiments, the copolyester composition comprises an impact modifier component comprising an EA-GMA impact modifier and a liquid silicone compatibilizer.

[0026] In an embodiment, the diol component comprises 60 mol% to 95 mol% of cyclohexanedimethanol residues and 5 mol% to 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues. In certain embodiments, the diol component comprises 70 mol% to 95 mol% of cyclohexanedimethanol residues and 5 mol% to 30 mol%, or 10 mol% to 30 mol%, or 15 mol% to 30 mol%, or 20 mol% to 30 mol%, or 15 mol% to 25 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues. In certain embodiments, the diol component comprises 60 mol% to 75 mol% of cyclohexanedimethanol residues and 25 mol% to 40 mol%, or 30 mol% to 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues.

[0027] In embodiments, the copolyester has an inherent viscosity of 0.55 to 0.85, or 0.55 to 0.65, or 0.65 to 0.80, or 0.65 to 0.75 dL / g.

[0028] In embodiments, the flame retardant additive is present in an amount of 10 wt % to 20 wt %, or 10 wt % to 18 wt %, or 10 wt % to 15 wt % of the copolyester composition.

[0029] In an embodiment, the flame retardant additive comprises a compound containing aluminum phosphinate. In certain embodiments, the flame retardant additive is aluminum diethylphosphinate.

[0030] In an embodiment, the copolyester composition comprises a drip suppressant additive in an amount of 0.05 wt% to 0.4 wt%, or 0.05 wt% to 0.25 wt%, or 0.1 wt% to 0.2 wt%. The drip suppressant may comprise a fluoropolymer. The fluoropolymer may include, but is not limited to, polytetrafluoroethylene (PTFE), such as Teflon TM Polytetrafluoroethylene.

[0031] In an embodiment, the copolyester composition further comprises an impact modifier component in an amount of 2 wt% to 10 wt%, or 3 wt% to 9 wt%, or 4 wt% to 8 wt%. In an embodiment, the impact modifier component comprises an impact modifier selected from a reactive acrylic impact modifier, a non-reactive MBS impact modifier, an epoxide functionalized impact modifier, or a mixture thereof. In an embodiment, the impact modifier comprises or is an ethylene-methyl acrylate-glycidyl methacrylate terpolymer. In an embodiment, the copolyester composition further comprises a chain extender. In certain embodiments, the chain extender comprises a multifunctional epoxide chain extender.

[0032] In an embodiment, the copolyester composition has a notched Izod impact strength of 60, or 70, or 80, or 90, or 100, or 120, or 130, or 140, or 150, or 175, or 200, or 225, or 250, or 275, or 300 Joules / m or more measured according to ASTM D256. In an embodiment, the copolyester composition exhibits 100% ductile behavior when tested according to ASTM D256.

[0033] In another aspect, an article is provided, comprising a copolyester composition according to one or more embodiments or a combination of any embodiments described herein. In an embodiment, the article is in the form of a film, a sheet, a molded part, or a profile. DETAILED DESCRIPTION

[0034] The present invention may be more readily understood by reference to the following detailed description and working examples of certain embodiments of the invention.

[0035] According to the purpose of the present invention, some embodiments of the present invention are described in the summary of the invention and further described below. In addition, other embodiments of the present invention are also described herein.

[0036] The present invention provides a copolyester composition comprising a copolyester and a flame retardant additive, wherein the copolyester composition exhibits good flame retardancy, good toughness, articles prepared therefrom, and methods for preparing the composition and articles. The present invention relates to the use of a certain class of flame retardant additives to improve flame retardant properties while maintaining impact properties. The flame retardant additive comprises a phosphite compound of a metal such as aluminum. When the flame retardant is added with the copolyester at an appropriate concentration, the flame retardant composition has a notched Izod impact strength of greater than about 60 joules / m, or 70, or 80, or 90, or 100 joules / m or more according to ASTM D256, while achieving a UL94 V-0 rating or better. In one embodiment, when tested according to ASTM D256, the copolyester composition can exhibit 100% ductile behavior while achieving a UL94 V-0 rating or better.

[0037] In an embodiment, the metal phosphinate compound comprises a metal selected from calcium, magnesium, aluminum and / or zinc. In an embodiment, the metal phosphinate compound is aluminum phosphite. In an embodiment, the metal phosphinate is a metal dialkyl phosphinate. In an embodiment, the metal phosphinate is aluminum dialkyl phosphinate. In an embodiment, the aluminum dialkyl phosphinate compound is aluminum diethyl phosphinate. In an embodiment, the metal phosphinate compound, such as aluminum diethyl phosphinate, is present in an amount of 10 wt % to 20 wt %, or 10 wt % to 18 wt %, or 10 wt % to 15 wt % of the copolyester composition.

[0038] In certain embodiments, the aluminum phosphinate compound may be a commercially available product, such as OP 1240 (available from Clariant).

[0039] In embodiments, the copolyester composition also includes a small amount of a drip inhibitor additive (as discussed herein), but less than 1 wt%, or less than 0.5 wt%, or less than 0.25 wt%, or less than 0.1 wt%, or less than 0.05 wt%, or contains no flame retardant synergist additive.

[0040] In an embodiment, a flame retardant synergist may be used. In an embodiment, the flame retardant synergist additive may include a phosphorus-containing compound selected from a compound containing phosphorus, nitrogen and / or sulfur; a phosphazene compound; an oligomeric phosphate; or a combination thereof. Some examples of synergists may include melamine polyphosphate (MPP), liquid phosphorus compounds such as PhireGuard RDP and PhireGuard BDP, or other organophosphorus compounds, such as organophosphorus compounds containing phosphorus (V) with a double bond between P and N. In an embodiment, the flame retardant synergist additive may include antimony.

[0041] Regarding component (d) impact modifier, this compound is generally an elastomeric compound or polymer for absorbing or dissipating impact kinetic energy. A wide range of known materials can be used in component (d). Various impact modifiers can be used to implement the present invention. In an embodiment, the impact modifier is in the dispersed phase, and the copolyester is included in the continuous phase of the entire copolyester composition. Examples of suitable impact modifiers include, but are not limited to, various known graft copolymers, core-shell polymers, and block copolymers. These polymers may include at least one monomer selected from olefins, dienes, aromatics, acrylates, and alcohols. (See, for example, EP 1,694,771B1). An example includes a core-shell polymer, wherein the core is composed of a rubbery polymer and the shell is composed of a styrene copolymer (e.g., see U.S. Patent No. 5,321,056, which is incorporated herein by reference). Other examples include core-shell and functional polyolefins, such as those described in US2014 / 0256848 A1, which are incorporated herein by reference. See also EP 2139948 B1.

[0042] Examples of impact modifiers that can be used include, but are not limited to, ethylene / propylene terpolymers; functionalized polyolefins, such as those containing methyl acrylate and / or glycidyl methacrylate; styrene-based block copolymer impact modifiers and various acrylic core / shell impact modifiers. Residues of these additives are also contemplated as part of the polyester composition.

[0043] Commercially available examples include:

[0044] Obtained from Nippon Oil & Fat Corporation 4300 and 4400; Kaneka Americas Holding, Inc. M300; Kane acquired from Kaneka America Holdings B564; Kane acquired from Kaneka America Holdings ECO 1000; obtained from Arkema 8900.

[0045] The impact modifiers used as component (d) above are generally present in an amount of about 1 wt% to about 10 wt%. In other embodiments, they are present in an amount of about 2 wt% to 10 wt%, or 3 wt% to 9 wt%, or 4 wt% to 8 wt%.

[0046] In an embodiment, the compatibilizer used as the above component (e) includes phenyl, alkyl or alkyl-phenyl silicone resin. In an embodiment, the silicone resin can be a phenyl silicone resin. In an embodiment, the silicone resin is a liquid at 25°C. In an embodiment, the silicone resin is a phenyl silicone resin that is liquid at 25°C. In an embodiment, the silicone resin, such as a phenyl silicone resin, has 1 to 10,000 cps, or 1 to 8000 cps, or 1 to 6000 cps, or 1 to 5000 cps, or 1 to 3000 cps, or 1 to 2000 cps, or 1 to 1000 cps, or 1 to 800 cps, or 1 to 600 cps, or 1 to 500 cps, or 1 to 300 cps, or 1 to 100 cps, or 1 to 50 cps, or 1 to 25 cps, or 1 to 20 cps, or 20 to 10,000 cps, or 20 to 8000 cps, or 20 to 6000 cps, or 20 to 5000 cps. s, or 20 to 3000cps, or 20 to 2000cps, or 20 to 1000cps, or 20 to 800cps, or 20 to 600cps, or 20 to 500cps, or 20 to 300cps, or 50 to 10,000cps, or 50 to 8000cps, or 50 to 6000cps, or 50 to 5000cps, or 50 to 3000cps, or 50 to 2000cps, or 50 to 1000cps, or 50 to 800cps, or 50 to 600cps, or 50 to 500cps, or 50 to 300cps, or 100 to 10,000cps cps, or 100 to 8000cps, or 100 to 6000cps, or 100 to 5000cps, or 100 to 3000cps, or 100 to 2000cps, or 100 to 1000cps, or 100 to 800cps, or 100 to 600cps, or 100 to 500cps, or 100 to 300cps, or 300 to 10,000cps, or 300 to 8000cps, or 300 to 6000cps, or 300 to 5000cps, or 300 to 3000cps, or 300 to 2000cps, or 300 to 1000cps, or 300 to 800cps, or 300 to 600cps, or 300 to 500cps, or 500 to 10,000cps, or 500 to 8000cps, or 500 to 6000cps, or 500 to 5000cps, or 500 to 3000cps, or 500 to 2000cps, or 500 to 1000cps, or 1000 to 10,000cps, or 1000 to 8000cps, or 1000 to 6000cps, or 1000 to 5000cps, or 1000 to 3000cps, or 1000 to 2000cps, or 2000 to 10,000cps, or 2000 to 8000cps, or 2000 to 6000cps, or 2000 to 5000cps, or 2000 to 3000cps, or 3000 to 10,000cps, or 3000 to 8000cps, or 3000 to 6000cps, or 3000 to 5000cps, which can be measured at 25°C using a digital rotational viscometer NDJ-8T, for viscosities of 1 to 100cps, the #0 spindle and 6 to 60rpm can be used for measurement; for viscosities above 100 to 5,000cps, the #1 or #2 spindle and 1.5 to 60rpm can be used for measurement. ,

[0047] In an embodiment, the phenyl silicone resin is an alkylphenyl silicone resin, such as methylphenyl silicone resin or octylphenyl silicone resin. In an embodiment, the liquid methylphenyl silicone resin has 0.1 / 1.0 to 2.0 / 1.0, or 0.1 / 1.0 to 1.8 / 1.0, or 0.1 / 1.0 to 1.6 / 1.0, or 0.1 / 1.0 to 1.4 / 1.0, or 0.1 / 1.0 to 1.2 / 1.0, or 0.1 / 1.0 to 1.1 / 1.0, or 0.1 / 1.0 to 1.0 / 1.0, or 0.1 / 1.0 to 0.8 / 1.0, or 0.1 / 1.0 to 0.6 / 1.0, or 0.1 / 1.0 to 0.4 / 1.0, or 0.1 / 1.0 to 0.2 / 1.0, or 0. 2 / 1.0 to 2.0 / 1.0, or 0.2 / 1.0 to 1.8 / 1.0, or 0.2 / 1.0 to 1.6 / 1.0, or 0.2 / 1.0 to 1.4 / 1.0, or 0.2 / 1.0 to 1.2 / 1.0, or 0.2 / 1.0 to 1.1 / 1.0, or 0.2 / 1.0 to 1.0 / 1.0, or 0.2 / 1.0 to 0.8 / 1.0, or 0.2 / 1.0 to 0.6 / 1.0, or 0.2 / 1.0 to 0.4 / 1.0, or 0.5 / 1.0 to 2.0 / 1.0, or 0.5 / 1.0 to 1.8 / 1.0, or 0.5 / 1.0 to 1.6 / 1.0, or 0.5 / 1.0 to 1.4 / 1.0, or 0.5 / 1.0 to 1.2 / 1.0, or 0.5 / 1.0 to 1.1 / 1.0, or 0.5 / 1.0 to 1.0 / 1.0, or 1.0 / 1.0 to 2.0 / 1.0, or 1.0 / 1.0 to 1.8 / 1.0, or 1.0 / 1.0 to 1.6 / 1.0, or 1.0 / 1.0 to 1.4 / 1.0, or 1.0 / 1.0 to 1.2 / 1.0, or 1.1 / 1.0 to 2.0 / 1.0, or 1.1 / 1.0 to 1.8 / 1.0, or 1.1 / 1. In an embodiment, the liquid silicone resin has a phenyl / methyl molar ratio of 90% or more, or 95% or more. The solids content can be determined by the weight loss after heating to 120°C for 2 hours to remove the liquid.In an embodiment, the molecular weight (Mw) of the liquid silicone resin is 1000 to 50000, or 1000 to 40000, or 1000 to 30000, or 1000 to 20000, or 1000 to 10000, or 1000 to 5000, or 2000 to 5000, or 2000 to 40000, or 2000 to 30000, or 2000 to 20000, or 2000 to 10000, or 2000 to 5000, 4000 to 50000, or 4000 to 40000, or 4000 to 30000, or 4000 to 20000. The molecular weight can be determined by calculating the theoretical Mw based on the chemical composition.

[0048] The copolyesters useful in the present invention comprise the residues of an aromatic diacid and the residues of two or more diols.

[0049] The term "copolyester" as used herein is intended to include "polyester" and is understood to refer to a synthetic polymer prepared by the reaction of one or more difunctional carboxylic acids and / or polyfunctional carboxylic acids with one or more difunctional hydroxyl compounds and / or polyfunctional hydroxyl compounds. Typically, the difunctional carboxylic acid can be a dicarboxylic acid and the difunctional hydroxyl compound can be a diol, such as a glycol. In addition, as used in this application, the interchangeable terms "diacid" or "dicarboxylic acid" include polyfunctional acids, such as branching agents. The term "glycol" used in this application includes, but is not limited to, glycols, diols and / or polyfunctional hydroxyl compounds. Alternatively, the difunctional carboxylic acid can be a hydroxycarboxylic acid, such as p-hydroxybenzoic acid, and the difunctional hydroxyl compound can be an aromatic ring with 2 hydroxyl substituents, such as hydroquinone. As used herein, the term "residue" refers to any organic structure introduced into a polymer from the corresponding monomer by polycondensation and / or esterification. As used herein, the term "repeat unit" refers to an organic structure having a dicarboxylic acid residue and a diol residue bonded by a carbonyl group. Thus, for example, the dicarboxylic acid residue can be derived from a dicarboxylic acid monomer or its associated acyl halide, ester, salt, anhydride or mixture thereof. As used herein, the term "dicarboxylic acid" is intended to include dicarboxylic acids and any derivatives of dicarboxylic acids, including their associated acyl halide, ester, half ester, salt, half salt, anhydride, mixed anhydride or mixtures thereof, which can be used in a reaction process with a diol to prepare a polyester. As used herein, the term "terephthalic acid" is intended to include terephthalic acid itself and its residues and any derivatives of terephthalic acid, including their associated acyl halide, ester, half ester, salt, half salt, anhydride, mixed anhydride and / or mixtures thereof or their residues, which can be used in a reaction process with a diol to prepare a copolyester. The term "modified aromatic diacid" refers to an aromatic dicarboxylic acid other than terephthalic acid. The term "modified glycol" refers to a glycol other than cyclohexanedimethanol (CHDM) or 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD).

[0050] In one embodiment, terephthalic acid can be used as a starting material. In another embodiment, dimethyl terephthalate can be used as a starting material. In another embodiment, a mixture of terephthalic acid and dimethyl terephthalate can be used as a starting material and / or an intermediate material.

[0051] The copolyesters used in the present invention can generally be prepared from dicarboxylic acids and diols, which react in substantially equal proportions and are introduced into the polyester polymer as their respective residues. Therefore, the copolyesters of the present invention can contain substantially equal molar proportions of acid residues (100 mol%) and diol (and / or multifunctional hydroxy compound) residues (100 mol%), such that the total mole number of repeating units is equal to 100 mol%. Therefore, the mole% provided in the present disclosure can be based on the total mole number of acid residues, the total mole number of diol residues, or the total mole number of repeating units. For example, based on the total acid residues, a copolyester containing 30 mol% of isophthalic acid means that the copolyester contains 30 mol% of isophthalic acid residues in a total of 100 mol% of acid residues. Therefore, there are 30 moles of isophthalic acid residues in every 100 moles of acid residues. In another example, a copolyester containing 30 mol% of 1,4-cyclohexanedimethanol based on total diol residues means that out of a total of 100 mol% of diol residues, the copolyester contains 30 mol% of 1,4-cyclohexanedimethanol residues. Thus, there are 30 moles of 1,4-cyclohexanedimethanol residues for every 100 moles of diol residues.

[0052] In an embodiment, the copolyester comprises 70 mol% to 100 mol% terephthalic acid (TPA). Alternatively, the copolyester comprises 80 mol% to 100 mol% TPA, or 90 mol% to 100 mol% TPA, or 95 mol% to 100 mol% TPA, or 100 mol% TPA. For the purposes of this disclosure, the terms "terephthalic acid" and "dimethyl terephthalate" are used interchangeably herein.

[0053] In addition to terephthalic acid, the dicarboxylic acid component that can be used for the copolyester of the present invention can include at most 30mol%, at most 20mol%, at most 10mol%, at most 5mol% or at most 1mol% of one or more modified aromatic dicarboxylic acids.Another embodiment contains 0mol% of modified aromatic dicarboxylic acid.Therefore, if present, it is expected that the amount of one or more modified aromatic dicarboxylic acids can be within the scope of any one of these aforementioned endpoint values, including, for example, 0.01mol% to 30mol%, 0.01mol% to 20mol%, 0.01mol% to 10mol%, 0.01mol% to 5mol% and 0.01mol% to 1mol%.In one embodiment, the modified aromatic dicarboxylic acids that can be used for the present invention include but are not limited to those with at most 20 carbon atoms, and it can be linear, para-oriented or symmetrical. Examples of modified aromatic dicarboxylic acids useful in the present invention include, but are not limited to, isophthalic acid, 4,4'-biphenyl dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, and trans-4,4'-stilbene dicarboxylic acid, and esters thereof. In one embodiment, the modified aromatic dicarboxylic acid is isophthalic acid.

[0054] The carboxylic acid component that can be used for the copolyester of the present invention can be further modified with up to 10mol%, for example up to 5mol% or up to 1mol% of one or more aliphatic dicarboxylic acids containing 2 to 16 carbon atoms, for example malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid and dodecanedioic acid dicarboxylic acid. Certain embodiments can also contain 0.01mol% or more mol%, for example 0.1mol% or more mol%, 1mol% or more mol%, 5mol% or more mol%, or 10mol% or more mol% of one or more modified aliphatic dicarboxylic acids. Another embodiment contains 0mol% of modified aliphatic dicarboxylic acids. Therefore, if present, it is expected that the amount of one or more modified dicarboxylic acids can be within the scope of any of these aforementioned endpoint values, including, for example, 0.01mol% to 10mol% and 0.1mol% to 10mol%. The total mol% of the dicarboxylic acid component is 100mol%.

[0055] The ester of terephthalic acid and other modified dicarboxylic acids or their corresponding ester and / or salt can replace dicarboxylic acid and use. Suitable examples of dicarboxylic acid esters include but are not limited to dimethyl ester, diethyl ester, dipropyl ester, diisopropyl ester, dibutyl ester and diphenyl ester. In one embodiment, ester is selected from at least one of the following: methyl ester, ethyl ester, propyl ester, isopropyl ester and phenyl ester.

[0056] Based on the total mole percentage of diol or diacid residues, the copolyesters useful in the copolyester compositions of the present invention may contain 0 to 10 mol%, such as 0.01 mol% to 5 mol%, 0.01 mol% to 1 mol%, 0.05 mol% to 5 mol%, 0.05 mol% to 1 mol%, or 0.1 mol% to 0.7 mol%; one or more residues of a branching monomer (also referred to herein as a branching agent) having 3 or more carboxyl substituents, hydroxyl substituents, or a combination thereof. In certain embodiments, the branching monomer or agent may be added before and / or during and / or after the polymerization of the polyester. Thus, the copolyesters useful in the present invention may be linear or branched.

[0057] Examples of branching monomers include, but are not limited to, polyfunctional acids or polyfunctional alcohols, such as trimellitic acid, trimellitic anhydride, pyromellitic dianhydride, trimethylolpropane, glycerol, pentaerythritol, citric acid, tartaric acid, 3-hydroxyglutaric acid, etc. In one embodiment, the branching monomer residues may contain 0.1 mol% to 0.7 mol% of one or more residues selected from the following: trimellitic anhydride, pyromellitic dianhydride, glycerol, sorbitol, 1,2,6-hexanetriol, pentaerythritol, trimethylolethane and / or trimesic acid. The branching monomers may be added to the polyester reaction mixture or blended with the polyester in the form of a concentrate, such as described in U.S. Pat. Nos. 5,654,347 and 5,696,176, the disclosure of which about branching monomers is incorporated herein by reference.

[0058] In an embodiment, CHDM may be 1,4-cyclohexanedimethanol. 1,4-cyclohexanedimethanol may be cis, trans or a mixture thereof, for example, the cis / trans ratio is 60:40 to 40:60. In another embodiment, trans-1,4-cyclohexanedimethanol may be present in an amount of 60 mol% to 80 mol%. Alternatively, 1,2-cyclohexanedimethanol and / or 1,3-cyclohexanedimethanol may be used alone or in combination with each other and / or in combination with 1,4-cyclohexanedimethanol.

[0059] The diol component of the copolyester portion of the copolyester compositions used in various embodiments may contain modifying diols other than CHDM or TMCD; in one embodiment, the copolyesters useful in the present invention may contain less than 15 mol%, or 10 mol% or less of one or more modifying diols.

[0060] The modified diols that can be used in the copolyesters of the embodiments refer to diols that are different from CHDM or TMCD, and can contain 2 to 20, or 2 to 16 carbon atoms. Examples of suitable modified diols include, but are not limited to, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, p-xylene glycol, isosorbide, or mixtures thereof. In another embodiment, the modified diol is 1,3-propylene glycol and / or 1,4-butanediol.

[0061] In an embodiment, the copolyester composition comprises at least one polyester comprising:

[0062] (a) a dicarboxylic acid component comprising:

[0063] i) 70 mol % to 100 mol % of terephthalic acid residues;

[0064] ii) 0-30 mol % of aromatic dicarboxylic acid residues having up to 20 carbon atoms; and iii) 0 to 10 mol % of aliphatic dicarboxylic acid residues having up to 16 carbon atoms; and

[0065] (b) a diol component comprising:

[0066] i) 5 mol% to 55 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues; and

[0067] ii) 45 mol% to 95 mol% of 1,4-cyclohexanedimethanol (CHDM) residues, wherein the total mol% of the dicarboxylic acid component is 100 mol% and the total mol% of the diol component is 100 mol%; and

[0068] wherein the inherent viscosity of the polyester is 0.5 to 1.2 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C; and wherein the Tg of the polyester is 100 to 200°C.

[0069] In an embodiment, the polyester composition comprises at least one polyester comprising:

[0070] (a) a dicarboxylic acid component comprising:

[0071] i) 70 mol % to 100 mol % of terephthalic acid residues;

[0072] ii) 0-30 mol % of aromatic dicarboxylic acid residues having up to 20 carbon atoms; and iii) 0 to 10 mol % of aliphatic dicarboxylic acid residues having up to 16 carbon atoms; and

[0073] (b) a diol component comprising:

[0074] i) 20 mol% to 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues; and ii) 60 mol% to 80 mol% of 1,4-cyclohexanedimethanol residues, wherein the total mol% of the dicarboxylic acid component is 100 mol% and the total mol% of the diol component is 100 mol%;

[0075] as well as

[0076] wherein the inherent viscosity of the polyester is 0.35 to 0.85 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C; and wherein the Tg of the polyester is 100 to 120°C.

[0077] In an embodiment, the polyester composition comprises at least one polyester comprising:

[0078] (a) a dicarboxylic acid component comprising:

[0079] i) 70 mol % to 100 mol % of terephthalic acid residues;

[0080] ii) 0-30 mol % of aromatic dicarboxylic acid residues having up to 20 carbon atoms; and iii) 0 to 10 mol % of aliphatic dicarboxylic acid residues having up to 16 carbon atoms; and

[0081] (b) a diol component comprising:

[0082] i) 40 mol% to 55 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues; and ii) 45 mol% to 60 mol% of 1,4-cyclohexanedimethanol residues, wherein the total mol% of the dicarboxylic acid component is 100 mol% and the total mol% of the diol component is 100 mol%;

[0083] as well as

[0084] wherein the inherent viscosity of the polyester is 0.35 to 0.85 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C; and wherein the Tg of the polyester is 120 to 140°C.

[0085] In an embodiment, the polyester composition comprises at least one polyester comprising:

[0086] (a) a dicarboxylic acid component comprising:

[0087] i) 70 mol % to 100 mol % of terephthalic acid residues;

[0088] ii) 0-30 mol % of aromatic dicarboxylic acid residues having up to 20 carbon atoms; and iii) 0 to 10 mol % of aliphatic dicarboxylic acid residues having up to 16 carbon atoms; and

[0089] (b) a diol component comprising:

[0090] i) 15 mol% to 70 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues; and ii) 30 mol% to 85 mol% of 1,4-cyclohexanedimethanol residues, wherein the total mol% of the dicarboxylic acid component is 100 mol% and the total mol% of the diol component is 100 mol%;

[0091] as well as

[0092] wherein the inherent viscosity of the polyester is 0.35 to 0.85 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C; and wherein the Tg of the polyester is 100 to 140°C.

[0093] In an embodiment, the polyester composition comprises at least one polyester comprising:

[0094] (a) a dicarboxylic acid component comprising:

[0095] i) 70 mol % to 100 mol % of terephthalic acid residues;

[0096] ii) 0 to 30 mol % of aromatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0097] iii) 0 to 10 mol % of aliphatic dicarboxylic acid residues having up to 16 carbon atoms; and

[0098] (b) a diol component comprising:

[0099] i) 15 mol% to 90 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues; and ii) 10 mol% to 85 mol% of 1,4-cyclohexanedimethanol residues, wherein the total mol% of the dicarboxylic acid component is 100 mol% and the total mol% of the diol component is 100 mol%;

[0100] as well as

[0101] wherein the inherent viscosity of the polyester is 0.1 to 1.2 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C; and wherein the Tg of the polyester is 100 to 200°C.

[0102] In embodiments, any of the polyesters or polyester compositions described herein may further comprise the residue of at least one branching agent. In embodiments, any of the polyesters or polyester compositions described herein may comprise at least one thermal stabilizer or a reaction product thereof.

[0103] In an embodiment, the polyester may contain less than 15 mol% of ethylene glycol residues, such as 0.01 mol% to less than 15 mol% of ethylene glycol residues. In an embodiment, the polyester useful in the present invention contains less than 10 mol%, or less than 5 mol%, or less than 4 mol%, or less than 2 mol%, or less than 1 mol% of ethylene glycol residues, such as 0.01 mol% to less than 10 mol%, or 0.01 mol% to less than 5 mol%, or 0.01 mol% to less than 4 mol%, or 0.01 mol% to less than 2 mol%, or 0.01 mol% to less than 1 mol% of ethylene glycol residues. In one embodiment, the polyester useful in the present invention contains no ethylene glycol residues.

[0104] In other embodiments, the diol component for the polyester may include, but is not limited to, at least one of the following range combinations: 5 mol% to less than 55 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and greater than 45 mol% to 95 mol% of 1,4-cyclohexanedimethanol; 5 mol% to less than 50 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and greater than 50 mol% to 95 mol% of 1,4-cyclohexanedimethanol; 5 mol% to less than 45 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and greater than 55 mol% to 95 mol% of 1,4-cyclohexanedimethanol. alkane dimethanol; 5 mol% to less than 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and greater than 60 mol% to 95 mol% of 1,4-cyclohexanedimethanol; 10 mol% to 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 60 mol% to 90 mol% of 1,4-cyclohexanedimethanol; 10 mol% to 35 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 65 mol% to 90 mol% of 1,4-cyclohexanedimethanol; 10 mol% to 30 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 70 mol% to 90 mol% of 1,4-cyclohexanedimethanol; 10 mol% to 25 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 mol% to 90 mol% of 1,4-cyclohexanedimethanol; 15 mol% to 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 60 mol% to 85 mol% of 1,4-cyclohexanedimethanol; 15 mol% to 35 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 65 mol% to 85 mol% of 1,4-cyclohexanedimethanol; 15 mol% to 30 mol% of 2,2, 4,4-tetramethyl-1,3-cyclobutanediol and 70 mol % to 85 mol % of 1,4-cyclohexanedimethanol; 15 mol % to 25 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 mol % to 85 mol % of 1,4-cyclohexanedimethanol; 15 mol % to 20 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 mol % to 80 mol % of 1,4-cyclohexanedimethanol; and 17 mol % to 23 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 77 mol % to 83 mol % of 1,4-cyclohexanedimethanol.

[0105] In certain embodiments, the diol component of the polyester portion of the polyester composition may contain 25 mol% or less of one or more modified diols that are not 2,2,4,4-tetramethyl-1,3-cyclobutanediol or 1,4-cyclohexanedimethanol; in one embodiment, the polyester useful in the present invention may contain less than 15 mol% of one or more modified diols. In another embodiment, the polyester may contain 10 mol% or less of one or more modified diols. In another embodiment, the polyester may contain 5 mol% or less of one or more modified diols. In another embodiment, the polyester may contain 3 mol% or less of one or more modified diols. In another embodiment, the polyester may contain 0 mol% of modified diols. Certain embodiments may also contain 0.01 mol% or more mol%, such as 0.1 mol% or more mol%, 1 mol% or more mol%, 5 mol% or more mol%, or 10 mol% or more mol% of one or more modified diols. Thus, it is contemplated that the amount of modifying glycol(s), if present, can range between any of these aforementioned endpoints, including, for example, 0.01 mol% to 15 mol% and 0.1 mol% to 10 mol%.

[0106] In an embodiment, the modified glycol in the polyester may refer to a glycol other than 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 1,4-cyclohexanedimethanol, and may contain 2 to 16 carbon atoms. In certain embodiments, examples of suitable modified glycols include, but are not limited to, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, p-xylene glycol, or a mixture thereof. In one embodiment, the modified glycol is ethylene glycol. In another embodiment, the modified glycol is 1,3-propylene glycol and / or 1,4-butanediol. In another embodiment, ethylene glycol is not used as a modified glycol. In another embodiment, 1,3-propylene glycol and 1,4-butanediol are not used as modified glycols. In another embodiment, 2,2-dimethyl-1,3-propylene glycol is not used as a modified glycol.

[0107] In embodiments, certain polyesters have a mol % of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol greater than 50 mol % or greater than 55 mol % of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol or greater than 70 mol % of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol; wherein the total mol % of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol and trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol is equal to 100 mol %.

[0108] In embodiments, the mol % of isomers of 2,2,4,4-tetramethyl-1,3-cyclobutanediol of certain polyesters is 30 mol % to 70 mol % of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol or 30 mol % to 70 mol % of trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol or 40 mol % to 60 mol % of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol or 40 mol % to 60 mol % of trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol, wherein the total mol % of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol and trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol equals 100 mol %.

[0109] In certain embodiments, the polyester can be amorphous or semi-crystalline. In one aspect, certain polyesters can have a relatively low degree of crystallinity. Thus, certain polyesters can have a substantially amorphous morphology, meaning that the polyester comprises substantially disordered polymer regions.

[0110] In an embodiment, the Tg of the polyester may be at least one of the following ranges: 100 to 200°C; 100 to 190°C; 100 to 180°C; 100 to 170°C; 100 to 160°C; 100 to 155°C; 100 to 150°C; 100 to 145°C; 100 to 140°C; 100 to 138°C; 100 to 135°C; 100 to 130°C; 100 to 125°C; 100 to 120°C; 100 to 115°C; 100 to 110°C; 105 to 200°C; 105 to 190°C; 105 to 180°C; 105 to 170°C; 105 to 160°C; 105 to 155°C; 105 to 150°C; 105 to 145°C; 105 to 140°C ℃; 105 to 138 ℃; 105 to 135 ℃; 105 to 130 ℃; 105 to 125 ℃; 105 to 120 ℃; 105 to 115 ℃; 105 to 110 ℃; more than 105 to 125 ℃; more than 105 to 120 ℃; more than 105 to 115 ℃; more than 105 to 110 ℃; 110 to 200 ℃; 110 to 190 ℃; 110 to 180 ℃; 110 to 170 ℃; 110 to 160 ℃; 110 to 155 ℃; 110 to 150 ℃; 110 to 145 ℃; 110 to 140 ℃; 110 to 138 ℃; 110 to 135 ℃; 110 to 130 ℃; 110 to 125 ℃; 110 to 120 ℃; 110 to 115 ℃; 115 to 200℃; 115 to 190℃; 115 to 180℃; 115 to 170℃; 115 to 160℃; 115 to 155℃; 115 to 150℃; 115 to 145℃; 115 to 140℃; 115 to 138℃; 115 to 135℃; 110 to 130℃; 115 to 125℃; 115 to 120℃; 120 to 200℃; 120 to 190℃; 120 to 180℃; 120 to 170℃; 120 to 160℃; 120 to 155℃; 120 to 150℃; 120 to 145℃; 120 to 140℃; 120 to 138℃; 120 to 135℃; 120 to 130℃; 125 to 200℃; 125 to 190℃; 12 5 to 180°C; 125 to 170°C; 125 to 160°C; 125 to 155°C; 125 to 150°C; 125 to 145°C; 125 to 140°C; 125 to 138°C; 125 to 135°C; 127 to 200°C; 127 to 190°C; 127 to 180°C; 127 to 170°C; 127 to 160°C; 1 27 to 150°C; 127 to 145°C; 127 to 140°C; 127 to 138°C; 127 to 135°C; 130 to 200°C; 130 to 190°C; 130 to 180°C; 130 to 170°C; 130 to 160°C; 130 to 155°C; 130 to 150°C; 130 to 145°C; 130 to 140°C;130 to 138°C; 130 to 135°C; 135 to 200°C; 135 to 190°C; 135 to 180°C; 135 to 170°C; 135 to 160°C; 135 to 155°C; 135 to 150°C; 135 to 145°C; 135 to 140°C; 140 to 200°C; 140 to 190°C; 140 to 180°C; 140 to 170°C; 140 to 160°C; 140 to 155°C; 140 to 1 50°C; 140 to 145°C; 148 to 200°C; 148 to 190°C; 148 to 180°C; 148 to 170°C; 148 to 160°C; 148 to 155°C; 148 to 150°C; 150 to 200°C; 150 to 190°C; 150 to 180°C; 150 to 170°C; 150 to 160°C; 155 to 190°C; 155 to 180°C; 155 to 170°C; and 155 to 165°C;

[0111] The glass transition temperature (Tg) of the polyester can be determined using a TADSC 2920 from Thermal Analyst Instrument at a scanning rate of 20°C / min.

[0112] For certain embodiments, the polyester may exhibit at least one of the following inherent viscosities, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C.: 0.10 to 1.2 dL / g; 0.10 to 1.1 dL / g; 0.10 to 1 dL / g; 0.10 to less than 1 dL / g; 0.10 to 0.98 dL / g; 0.10 to 0.95 dL / g; 0.10 to 0.90 dL / g; 0.10 to 0.85 dL / g; 0.10 to 0.80 dL / g; 0.10 to 0.75 dL / g; 0.10 to less than 0.75 dL / g; 0.10 to 0.72 dL / g; 0.10 to 0.70 dL / g g; 0.10 to less than 0.70 dL / g; 0.10 to 0.68 dL / g; 0.10 to less than 0.68 dL / g; 0.10 to 0.65 dL / g; 0.20 to 1.2 dL / g; 0.20 to 1.1 dL / g; 0.20 to 1 dL / g; 0.20 to less than 1 dL / g; 0.20 to 0.98 dL / g; 0.20 to 0.95 dL / g; 0.20 to 0.90 dL / g; 0.20 to 0.85 dL / g; 0.20 to 0.80 dL / g; 0.20 to 0.75 dL / g; 0.20 to less than 0.75 dL / g; 0.20 to 0.72 dL / g; 0.20 to 0.70 dL / g; 0.20 to less than 0. 70 dL / g; 0.20 to 0.68 dL / g; 0.20 to less than 0.68 dL / g; 0.20 to 0.65 dL / g; 0.35 to 1.2 dL / g; 0.35 to 1.1 dL / g; 0.35 to 1 dL / g; 0.35 to less than 1 dL / g; 0.35 to 0.98 dL / g; 0.35 to 0.95 dL / g; 0.35 to 0.90 dL / g; 0.35 to 0.85 dL / g; 0.35 to 0.80 dL / g; 0.35 to 0.75 dL / g; 0.35 to less than 0.75 dL / g; 0.35 to 0.72 dL / g; 0.35 to 0.70 dL / g; 0.35 to less than 0.70 dL / g; 0.35 to 0.68 dL / g; 0.35 to less than 0.68 dL / g; 0.35 to 0.65 dL / g; 0.40 to 1.2 dL / g; 0.40 to 1.1 dL / g; 0.40 to 1 dL / g; 0.40 to less than 1 dL / g; 0.40 to 0.98 dL / g; 0.40 to 0.95 dL / g; 0.40 to 0. 90dL / g; 0.40 to 0.85dL / g; 0.40 to 0.80dL / g; 0.40 to 0.75dL / g; 0.40 to less than 0.75dL / g; 0.40 to 0.72dL / g; 0.40 to 0.70dL / g; 0.40 to less than 0.70dL / g; 0.40 to 0.68dL / g; 0.40 to less than 0.68 dL / g; 0.40 to 0.65 dL / g; greater than 0.42 to 1.2 dL / g; greater than 0.42 to 1.1 dL / g; greater than 0.42 to 1 dL / g; greater than 0.42 to less than 1 dL / g; greater than 0.42 to 0.98 dL / g; greater than 0.42 to 0.95 dL / g; greater than 0.42 to 0.90 dL / g; greater than 0.42 to 0. 85 dL / g; greater than 0.42 to 0.80 dL / g; greater than 0.42 to 0.75 dL / g; greater than 0.42 to less than 0.75 dL / g; greater than 0.42 to 0.72 dL / g; greater than 0.42 to less than 0.70 dL / g; greater than 0.42 to 0.68 dL / g; greater than 0.42 to less than 0.68 dL / g; and greater than 0.42 to 0.65 dL / g.

[0113] For certain embodiments, the polyester may exhibit at least one of the following inherent viscosities, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C.: 0.45 to 1.2 dL / g; 0.45 to 1.1 dL / g; 0.45 to 1 dL / g; 0.45 to 0.98 dL / g; 0.45 to 0.95 dL / g; 0.45 to 0.90 dL / g; 0.45 to 0.85 dL / g; 0.45 to 0.80 dL / g; 0.45 to 0.75 dL / g; 0.45 to less than 0.75 dL / g; 0.45 to 0.72 dL / g; 0.45 to 0.70 dL / g; 0.45 to less than 0.70 dL / g; 0.45 to 0.68 dL / g; 0.45 to less than 0.68 dL / g; 0.45 to 0.65 dL / g; 0.50 to 1.2 dL / g; 0.50 to 1.1 dL / g; 0.50 to 1 dL / g; 0.50 to less than 1 dL / g; 0.50 to 0.98 dL / g; 0.50 to 0. 95dL / g; 0.50 to 0.90dL / g; 0.50 to 0.85dL / g; 0.50 to 0.80dL / g; 0.50 to 0.75dL / g; 0.50 to less than 0.75dL / g; 0.50 to 0.72dL / g; 0.50 to 0.70dL / g; 0.50 to less than 0.70dL / g; 0. 50 to 0.68 dL / g; 0.50 to less than 0.68 dL / g; 0.50 to 0.65 dL / g; 0.55 to 1.2 dL / g; 0.55 to 1.1 dL / g; 0.55 to 1 dL / g; 0.55 to less than 1 dL / g; 0.55 to 0.98 dL / g; 0.55 to 0.95 dL / g; 0.55 to 0.90 dL / g; 0.55 to 0.85 dL / g; 0.55 to 0.80 dL / g; 0.55 to 0.75 dL / g; 0.55 to less than 0.75 dL / g; 0.55 to 0.72 dL / g; 0.55 to 0.70 dL / g; 0.55 to less than 0.70 dL / g; 0.55 to 0.68 dL / g g; 0.55 to less than 0.68 dL / g; 0.55 to 0.65 dL / g; 0.58 to 1.2 dL / g; 0.58 to 1.1 dL / g; 0.58 to 1 dL / g; 0.58 to less than 1 dL / g; 0.58 to 0.98 dL / g; 0.58 to 0.95 dL / g; 0.58 to 0.90 dL / g; 0.58 to 0.85 dL / g; 0.58 to 0.80 dL / g; 0.58 to 0.75 dL / g; 0.58 to less than 0.75 dL / g; 0.58 to 0.72 dL / g; 0.58 to 0.70 dL / g; 0.58 to less than 0.70 dL / g; 0.58 to 0.68 dL / g; 0.58 to less than 0.68dL / g; 0.58 to 0.65dL / g; 0.60 to 1.2dL / g; 0.60 to 1.1dL / g; 0.60 to 1dL / g; 0.60 to less than 1dL / g; 0.60 to 0.98dL / g; 0.60 to 0.95dL / g; 0.60 to 0.90dL / g; 0.60 to 0.85dL / g; 0.60 to 0.80dL / g; 0.60 to 0.75dL / g; 0.60 to less than 0.75dL / g; 0.60 to 0.72dL / g; 0.60 to 0.70dL / g; 0.60 to less than 0.70dL / g; 0.60 to 0.68dL / g; 0.60 to less than 0.68dL / g; 0.60 to 0.65dL / g; 0.65 to 1.2dL / g; 0.65 to 1.1dL / g; 0.65 to 1dL / g; 0.65 to less than 1dL / g; 0.65 to 0.98dL / g; 0.65 to 0.95dL / g; 0.65 to 0.90dL / g; 0.65 to 0.85dL / g; 0.65 to 0.80dL / g; 0.65 to 0.75dL / g; 0.65 to less than 0.75dL / g; 0.65 to 0.72dL / g; 0.65 to 0.70dL / g; 0.65 to less than 0.70dL / g ; 0.68 to 1.2 dL / g; 0.68 to 1.1 dL / g; 0.68 to 1 dL / g; 0.68 to less than 1 dL / g; 0.68 to 0.98 dL / g; 0.68 to 0.95 dL / g; 0.68 to 0.90 dL / g; 0.68 to 0.85 dL / g; 0.68 to 0.80 dL / g; 0.68 to 0.75 dL / g; 0.68 to less than 0.75 dL / g; 0.68 to 0.72 dL / g; greater than 0.76 dL / g to 1.2 dL / g; greater than 0.76 dL / g to 1.1 dL / g; greater than 0.76 dL / g to 1 dL / g; greater than 0.76 dL / g to less than 1dL / g; greater than 0.76dL / g to 0.98dL / g; greater than 0.76dL / g to 0.95dL / g; greater than 0.76dL / g to 0.90dL / g; greater than 0.80dL / g to 1.2dL / g; greater than 0.80dL / g to 1.1dL / g; greater than 0.80dL / g to 1dL / g; greater than 0.80dL / g to less than 1dL / g; greater than 0.80dL / g to 1.2dL / g; greater than 0.80dL / g to 0.98dL / g; greater than 0.80dL / g to 0.95dL / g; greater than 0.80dL / g to 0.90dL / g. .

[0114] In certain embodiments, unless otherwise stated, it is contemplated that the polyester composition can have at least one inherent viscosity range described herein and at least one monomer range for the composition described herein. It is also contemplated that the polyester composition can have at least one Tg range described herein and at least one monomer range for the composition described herein, unless otherwise stated. It is also contemplated that the polyester composition can have at least one Tg range described herein, at least one inherent viscosity range described herein, and at least one monomer range for the composition described herein, unless otherwise stated.

[0115] In embodiments, the molar ratio of cis / trans 2,2,4,4-tetramethyl-1,3-cyclobutanediol may be different from the respective pure forms or mixtures thereof. In certain embodiments, the mole percentage of cis- and / or trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol is greater than 50 mol% cis and less than 50 mol% trans; or greater than 55 mol% cis and less than 45 mol% trans; or 30 mol% to 70 mol% cis and 70 mol% to 30% trans; or 40 mol% to 60 mol% cis and 60 mol% to 40 mol% trans; or 50 mol% to 70 mol% trans and 50 mol% to 30% cis or 50 mol% to 70 mol% cis and 50 mol% to 30% trans; or 60 mol% to 70 mol% cis and 30 mol% to 40 mol% trans; or greater than 70 mol% cis and less than 30 mol% trans; wherein the sum of the mole percentages of cis- and trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol is equal to 100 mol%. The molar ratio of cis / trans 1,4-cyclohexanedimethanol may vary within the range of 50 / 50 to 0 / 100, for example between 40 / 60 and 20 / 80.

[0116] The polyester part of the polyester composition can be prepared by methods known in the literature, such as by a process in a homogeneous solution, by a transesterification process in a melt, and by a two-phase interface process. Suitable methods include those disclosed in U.S. Published Application 2006 / 0287484, the contents of which are incorporated herein by reference.

[0117] In an embodiment, the polyester may be prepared by a process comprising reacting one or more dicarboxylic acids (or derivatives thereof) with one or more diols under conditions that provide polyester, the process including but not limited to the step of reacting one or more dicarboxylic acids (or derivatives thereof) with one or more diols at a temperature of 100° C. to 315° C. at a pressure of 0.1 to 760 mmHg for a time sufficient to form the polyester. See U.S. Pat. No. 3,772,405 for methods of producing polyesters, the disclosure of which is incorporated herein by reference.

[0118] In an embodiment, the polyester composition can be a polymer blend, wherein the blend comprises: (a) 5 wt% to 95 wt% of at least one polyester described herein; and (b) 5 wt% to 95 wt% of at least one polymer component. Suitable examples of polymer components include, but are not limited to, nylon, polyesters other than those described herein, such as polyethylene or polybutylene terephthalate (PET or PBT), polyamides, such as those from DuPont Polystyrene, polystyrene copolymers, styrene acrylonitrile copolymers, acrylonitrile butadiene styrene copolymers, poly(methyl methacrylate), acrylic acid copolymers, poly(ether-imide) such as (poly(ether-imide) available from General Electric); polyphenylene ethers, such as poly(2,6-dimethylphenylene ether) or poly(phenylene ether) / polystyrene blends, such as NORYL (a blend of poly(2,6-dimethylphenylene oxide) and polystyrene resin from General Electric); polyphenylene sulfide; polyphenylene sulfide / sulfone; poly(ester-carbonate); polycarbonates, such as (General Electric Company polycarbonate); polysulfone; polysulfone ether; and poly(ether-ketone) of an aromatic dihydroxy compound; or a mixture of any other of the foregoing polymers. The blends can be prepared by conventional processing techniques known in the art such as melt blending or solution blending. In one embodiment, polycarbonate is not present in the polyester composition. However, polyester compositions useful in the present invention are also contemplated to not include polycarbonate as well as include polycarbonate.

[0119] Furthermore, the copolyester composition may further comprise one or more additional additives selected from colorants, dyes, mold release agents, additional flame retardants, plasticizers, processing aids, rheology modifiers, nucleating agents, antioxidants, light stabilizers, fillers and reinforcing materials.

[0120] In embodiments, the polyester compositions and polymer blend compositions may also contain (in addition to the components described herein) 0.01% to 25% of commonly used additives, such as colorants, dyes, mold release agents, additional flame retardants, plasticizers, nucleating agents, stabilizers, including but not limited to UV stabilizers, heat stabilizers and / or their reaction products, fillers and impact modifiers, based on the weight of the total composition. For example, UV additives can be introduced into articles (e.g., ophthalmic products) by addition to the bulk or in the hard coat. Examples of typical commercially available impact modifiers known in the art and useful in the present invention include, but are not limited to, ethylene / propylene terpolymers; functionalized polyolefins, such as those containing methyl acrylate and / or glycidyl methacrylate; styrene-based block copolymer impact modifiers, epoxide-functionalized impact modifiers, and various acrylic core / shell impact modifiers. Residues of these additives are also considered to be part of the polyester composition. In one embodiment, the composition comprises an epoxide-functionalized impact modifier.

[0121] In certain embodiments, the polyester compositions and polymer blend compositions may include fillers or reinforcing additives, such as glass (or other) fibers, in an amount of 1 wt % to 45 wt %, or 1 wt % to 40 wt %, or 1 wt % to 35 wt %, or 1 wt % to 30 wt %, or 5 wt % to 45 wt %, or 5 wt % to 40 wt %, or 5 wt % to 35 wt %, or 5 wt % to 30 wt %, or 10 wt % to 45 wt %, or 10 wt % to 40 wt %, or 10 wt % to 35 wt %, or 10 wt % to 30 wt %, or 15 wt % to 45 wt %, or 15 wt % to 40 wt %, or 15 wt % to 35 wt %, or 15 wt % to 30 wt %, or 20 wt % to 45 wt %, or 20 wt % to 40 wt %, or 20 wt % to 35 wt %, or 20 wt % to 30 wt %, based on the total composition. In certain embodiments including such fillers or reinforcing additives, the polyester compositions and polymer blend compositions may also contain (in addition to the components and filler / reinforcing additives described herein) from 0.01% to 25%, or from 0.01% to 20%, or from 0.01% to 15%, or from 0.01% to 10%, by weight of the total composition, of other common additives, such as those discussed above.

[0122] In certain embodiments, the polyester compositions and polymer blend compositions may contain a colorant, such as TiO2, in an amount of 1 wt% to 40 wt%, or 1 wt% to 35 wt%, or 1 wt% to 30 wt%, or 1 wt% to 25 wt%, or 5 wt% to 40 wt%, or 5 wt% to 35 wt%, or 5 wt% to 30 wt%, or 5 wt% to 25 wt%, or 10 wt% to 40 wt%, or 10 wt% to 35 wt%, or 10 wt% to 30 wt%, or 10 wt% to 25 wt%, or 15 wt% to 40 wt%, or 15 wt% to 35 wt%, or 15 wt% to 30 wt%, or 15 wt% to 25 wt%, or 20 wt% to 40 wt%, or 20 wt% to 35 wt%, or 20 wt% to 30 wt%, or 20 wt% to 25 wt%, based on the total composition. In certain embodiments including such colorants, the polyester compositions and polymer blend compositions may also contain (in addition to the components and colorants described herein) from 0.01 wt % to 25 wt %, or from 0.01 wt % to 20 wt %, or from 0.01 wt % to 15 wt %, or from 0.01 wt % to 10 wt % of other common additives, such as those discussed above, of the total composition.

[0123] In an embodiment, the polyester composition and the polymer blend composition may include one or more antioxidants in an amount of 0.01 wt% to 2 wt%, or 0.01 wt% to 1.5 wt%, or 0.01 wt% to 1 wt%, or 0.01 wt% to 0.75 wt%, or 0.01 wt% to 0.5 wt%, or 0.01 wt% to 0.4 wt%, or 0.01 wt% to 0.3 wt%, based on the total composition. Examples of antioxidants may include Iranox 1010, Irgafos 168, or a combination thereof.

[0124] In one aspect, the copolyester composition of the present invention comprises a copolyester composition comprising any of the above copolyesters and a metal phosphinate compound flame retardant.

[0125] In an embodiment, the polyester may include at least one chain extender. Suitable chain extenders include, but are not limited to, multifunctional (including but not limited to difunctional) isocyanates, multifunctional epoxides, including, for example, epoxidized phenolic varnishes and phenoxy resins. In certain embodiments, the chain extender may be added at the end of the polymerization process or after the polymerization process. If added after the polymerization process, the chain extender may be introduced by compounding or by addition during a conversion process such as injection molding or extrusion. The amount of chain extender used may vary depending on the specific monomer composition used and the desired physical properties, but is typically 0.1 wt% to 10 wt%, such as 0.1 wt% to 5 wt%, based on the total weight of the polyester.

[0126] Heat stabilizers are compounds that stabilize polyesters during polyester manufacturing and / or post-polymerization, including but not limited to phosphorus compounds, including but not limited to phosphoric acid, phosphorous acid, phosphonic acid, phosphinic acid, phosphous acid and various esters and salts thereof. Esters can be alkyl, branched alkyl, substituted alkyl, difunctional alkyl, alkyl ether, aryl and substituted aryl. In one embodiment, the number of ester groups present in a particular phosphorus compound can vary from zero to a maximum value allowed by the number of hydroxyl groups present on the heat stabilizer used. The term "heat stabilizer" is intended to include its reaction products. The term "reaction product" used in conjunction with the heat stabilizer of the present invention refers to any product of a polycondensation or esterification reaction between a heat stabilizer and any monomer used to prepare polyester, as well as a product of a polycondensation or esterification reaction between a catalyst and any other type of additive. In an embodiment, these may be present in a polyester composition.

[0127] In an embodiment, reinforcing materials can be used in polyester compositions. Reinforcing materials may include, but are not limited to, carbon filaments, silicates, mica, clay, talc, titanium dioxide, wollastonite, glass flakes, glass beads and fibers, and polymer fibers and combinations thereof. In one embodiment, reinforcing materials are glass, such as fiberglass filaments, a mixture of glass and talc, glass and mica, and glass and polymer fibers.

[0128] In another aspect, the present invention relates to a copolyester composition comprising a copolyester produced by a process comprising the steps of:

[0129] (I) heating a mixture comprising monomers useful in any copolyester of the present invention at a temperature of from 150 to 240° C. in the presence of a catalyst for a time sufficient to produce an initial copolyester;

[0130] (II) heating the initial copolyester of step (I) at a temperature of 240 to 320° C. for 1 to 4 hours; and

[0131] (III) Removal of any unreacted diol.

[0132] Suitable catalysts for the method include, but are not limited to, organic zinc or tin compounds. The use of such catalysts is well known in the art. Examples of catalysts that can be used in the present invention include, but are not limited to, zinc acetate, butyltin tri-2-ethylhexanoate, dibutyltin diacetate, and dibutyltin oxide. Other catalysts may include, but are not limited to, those based on titanium, zinc, manganese, lithium, germanium, and cobalt. Based on the catalyst metal and based on the weight of the final polymer, the amount of the catalyst can be 10ppm to 20,000ppm or 10 to 10,000ppm, or 10 to 5000ppm or 10 to 1000ppm or 10 to 500ppm, or 10 to 300ppm or 10 to 250ppm. The method can be carried out in an intermittent or continuous process.

[0133] Typically, step (I) may be conducted until 50 wt% or more of the diol has reacted. Step (I) may be conducted at a pressure of from atmospheric pressure to 100 psig. The term "reaction product" used in conjunction with any catalyst used in the present invention refers to any product of a polycondensation or esterification reaction with the catalyst and any monomer used to prepare the polyester, as well as the product of a polycondensation or esterification reaction between the catalyst and any other type of additive.

[0134] Typically, step (II) and step (III) can be performed simultaneously. These steps can be performed by methods known in the art, such as by placing the reaction mixture under a pressure of 0.002 psig to below atmospheric pressure, or by blowing hot nitrogen through the mixture.

[0135] The flame retardant may be incorporated into the copolyester in the form of a concentrate by any conventional method for final formation into an article.

[0136] Flame retardants can be introduced into plastic compounding lines such as twin-screw compounding lines to form copolyester composition concentrates. The pellets are then fed into the feed port of the extruder and melted from 430°F to 520°F (221°C to 271°C) to produce a viscous thermoplastic material. Alternatively, the flame retardant is added as a single powder with a loss-in-weight feeder or added separately in a loss-in-weight feeder. The rotation of the two screws disperses the flame retardant into the copolyester. The mixture is then extruded through a die to produce a plurality of strands. In certain embodiments, the strands are fed through a water trough to cool the pellets. Upon leaving the water trough, the strands are dried and fed to a slicing machine to cut the strands into pellets. Alternatively, the mixture can be extruded through a circular flat die with a plurality of openings into the water. The flat die has a rotary cutter that slices the strands to produce pellets as they are extruded from the die. The continuous water flow cools the pellets and conveys them to a drying section, usually a centrifuge, to separate the pellets from the water.

[0137] Alternatively, the flame retardant is added to a plastic compounding line, such as a twin-rotor continuous compounding mixer (e.g., Farrell continuous mixer), to form a copolyester composition concentrate. In this case, the copolyester pellets are dried at 150°F to 190°F (65.6°C to 87.8°C) for 4-6 hours to reduce moisture. The copolyester pellets and flame retardant are fed into the feed port of the continuous mixer and melted into a uniform mixture at 430°F to 520°F (221°C to 271°C). The output rate of the mixer is controlled by changing the area of ​​the discharge hole. The melt can be cut into "loafs" and fed to the feed port of a twin-roll mill or a single screw extruder. In the case where the melt is fed into a twin-roll mill, the melt covers one of the rolls to form a sheet of concentrate, which is cut into strips that are fed into the feed port of a single screw extruder. The mixture is then extruded through a die to produce a plurality of strips. The strips are fed through a water trough to cool the pellets. When leaving the water trough, the strips are dried and fed to a dicing machine to cut the strips into pellets. Alternatively, the mixture can be extruded through a circular flat die with multiple openings entering the water. The flat die has a rotary cutter, and when the strips are extruded from the die, the rotary cutter slices the strips to produce pellets. The continuous water flow cools the pellets and transports them to a drying section, typically a centrifuge, to separate the pellets from water. In the case of "strips" (relatively most of the concentrate) being fed to a single screw extruder, the mixture is extruded through the die to produce multiple strips. The strips can be fed through a water trough to cool the pellets. When leaving the water trough, the strips are dried and fed to a dicing machine to cut the strips into pellets. Alternatively, the mixture can be extruded through a circular flat die with multiple openings entering the water. The flat die has a rotary cutter, and when the strips are extruded from the die, the rotary cutter slices the strips to produce pellets. The continuous water flow cools the pellets and conveys them to a drying section, usually a centrifuge, to separate the pellets from the water.

[0138] Optionally, the flame retardant is introduced into a high intensity mixer such as The copolyester composition concentrate is formed in an intermittent mixer. In this case, the copolyester pellets can be dried at 150°F to 190°F (65.6°C to 87.8°C) for 4-6 hours to reduce moisture. The copolyester pellets and flame retardant are loaded into a high-intensity mixer, and the punch is lowered to press the pellet / flame retardant mixture into the mixing chamber. Two rotating mixer blades melt the pellets and disperse the flame retardant into the melt. When the desired temperature is reached, the door at the bottom of the mixer is opened and the mixture is dripped onto a double-roll mill. The ribbon from the double-roll mill can then be fed to a single screw extruder. The mixture is then extruded through a die to produce a plurality of strands. The strands can be fed through a water trough to cool the pellets. When leaving the water trough, the strands are dried and fed to a slicing machine to cut the strands into pellets. Alternatively, the mixture can be extruded through a circular flat die with a plurality of openings into the water. The flat die has a rotating cutter that slices the strands as they exit the die to produce pellets. A continuous stream of water cools the pellets and conveys them to a drying section, usually a centrifuge, to separate the pellets from the water.

[0139] The present invention includes plastic articles containing the copolyester composition. The plastic articles can be prepared by a method including but not limited to the following steps: extruding the copolyester composition to prepare a continuous flat sheet or profile, or injection molding to produce a discrete article, or calendering to prepare a continuous film or sheet, or additive manufacturing a powder or filament to produce a three-dimensional shape.

[0140] Films and / or sheets useful for the present invention can have any thickness apparent to one of ordinary skill in the art. In one embodiment, the film (s) of the present invention have a thickness of less than 30 mils, or less than 20 mils, or less than 10 mils, or less than 5 mils. In one embodiment, the sheet of the present invention has a thickness greater than 30 mils. In one embodiment, the sheet of the present invention has a thickness of 30 mils to 100 mils, or 30 mils to 200 mils, or 30 mils to 500 mils.

[0141] The present invention further relates to films and / or sheets comprising the polyester composition of the present invention. Methods of forming polyester into films and / or sheets are well known in the art. Examples of films and / or sheets of the present invention include, but are not limited to, extruded films and / or sheets, calendered films and / or sheets, compression molded films and / or sheets, injection molded films or sheets, and solution cast films and / or sheets. Methods for preparing films and / or sheets include, but are not limited to, extrusion, calendering, extrusion molding, compression molding, and solution casting. These films or sheets can be manufactured or subjected to further processing, such as orientation (uniaxial or biaxial), heat setting, surface treatment, etc.

[0142] In one embodiment of the present invention, a flat sheet or profile is included. The sheet or profile is prepared by extruding the copolyester composition to produce a flat sheet or profile. In this case, the pellets of the copolyester composition are dried at 150°F to 190°F (65.6°C to 87.8°C) for 4-6 hours and then fed into a single screw extruder, a twin screw extruder or a tapered twin screw extruder. The copolyester composition pellets are conveyed and compressed by the screw down the extruder barrel to melt the pellets and discharge the melt from the end of the extruder. The melt is fed through a screening device to remove debris and / or a melt pump to reduce the pressure changes caused by the extruder. The melt is then fed through a die to produce a continuous flat sheet or into a forming die to produce a continuous shape. In one embodiment of the present invention including a flat sheet die, the melt is extruded onto a series of metal rollers, typically three, to cool the melt and impart a finish to the sheet. The flat sheet is then conveyed in the form of a continuous sheet for a distance or time period sufficient to cool the sheet. The sheet is then trimmed to the desired width, then rolled into a coil or sheared or sawed into a sheet form of the desired size. It is also possible to mechanically form a flat sheet into a shaped article to form the desired shaped article, then cooled by spraying water, conveying through a water tank or by blowing air on the shaped article. The article is then sawn or sheared into the desired length. In the case of a forming die, the mold is designed to produce the desired shape of the profile. After leaving the mold, the profile is then cooled by spraying with water, conveying through a water tank or by blowing air on the profile. The profile is then sawn or sheared into the desired length. In the case of a fiber, the fiber can be pulled out from the extrusion die spinneret to the desired fiber diameter and crystallized to improve physical properties.

[0143] Another embodiment of the present invention includes mixing pure copolyester pellets with a concentrate of flame retardant and then extruding the copolyester composition. The flame retardant concentrate can be compounded as pellets. Before extrusion, the pellets are dried at 150°F to 190°F (65.6°C to 87.8°C) for 4-6 hours. The pellets are dried after mixing in a low intensity mixer such as a ribbon mixer, a drum or a conical screw mixer. The pellets are then fed to an extruder, which includes but is not limited to a single screw extruder, a twin screw extruder or a conical twin screw extruder. The pellets are conveyed and compressed by the screw down the extruder barrel to melt the pellets and discharge the melt from the end of the extruder. The melt is usually fed through a screening device to remove debris and / or a melt pump to reduce the pressure changes caused by the extruder. The melt is then fed through a die to produce a continuous flat sheet or into a forming die to produce a continuous shape. In the case of a flat sheet die, the melt is extruded onto a series of metal rollers, typically three, to cool the melt and impart the oil to the sheet. Then, the flat sheet is transported in the form of a continuous sheet for a distance or time period sufficient to cool the sheet. It can then be trimmed to the desired width, then rolled into a roll or sheared or sawn into sheet form. The flat sheet can also be mechanically formed into the desired shape, then cooled by spraying water, by a water tank, or by blowing air on the molded product. It can then be sawed or sheared into the desired length. In the case of a film, a film can be prepared and wound into a roll. In the case of a molding die, the mold is designed to produce the desired shape of the profile. After leaving the mold, the profile can then be cooled by spraying water, by a water tank, or by blowing air on the profile. It can then be sawed or sheared into the desired length. In the case of a fiber, the fiber can be pulled out from the extrusion die spinneret to the desired fiber diameter and crystallized to improve physical properties.

[0144] Another embodiment can include mixing pure copolyester pellets with flame retardant concentrates and then extruding them with short or long glass fiber reinforcements, or extruding them into continuous glass fiber composite films, sheets or tapes. The flame retardant can be compounded as a single pellet. Before extrusion, the pellets are dried at 150°F to 190°F (65.6°C to 87.8°C) for 4-6 hours. After mixing in a low-intensity mixer such as a ribbon mixer, a drum or a conical screw mixer, the pellets can be dried separately or together. The pellets are then added to a single screw extruder, a twin screw extruder or a conical twin screw extruder. The pellets are conveyed and compressed by the screw down the extruder barrel to melt the pellets and discharge the melt from the end of the extruder. The melt can be fed through a screening device to remove debris and / or a melt pump to reduce the pressure changes caused by the extruder. The melt can then be fed through a die to produce a continuous flat sheet or into a forming die to produce a continuous shape. In the case of a flat sheet die, the melt is extruded onto a series of metal rollers, typically three, to cool the melt and impart the oil to the sheet. Then, the flat sheet is transported in the form of a continuous sheet to cool the sheet. It can then be trimmed to the desired width, then rolled into a roll or sheared or sawn into a sheet form. The flat sheet can also be formed into a desired shape by a mechanical device, then cooled by spraying water, by a water tank or by blowing air on the profile. It can then be sawed or sheared into a desired length, or a film can be prepared and wound into a roll. In the case of a forming die, the mold is designed to produce the desired shape of the profile. After leaving the mold, it can then be cooled by spraying water, by a water tank or by blowing air on the profile. It can then be sawed or sheared into a desired length. In the case of a fiber, the fiber can be pulled out from the extrusion die spinneret to the desired fiber diameter and crystallized to improve physical properties.

[0145] Another embodiment can include extruding fully compounded pellets of a copolyester composition to produce an injection molded article, the copolyester composition comprising a copolyester and a flame retardant. In this case, the pellets are dried at 150°F to 190°F (65.6°C to 87.8°C) for 4 to 6 hours, dried, and then fed into an injection molding machine. Once the pellets reach the desired temperature, a gate is opened at the end of the extruder and the molten plastic is pumped through a screw into a heated mold to form an article of the desired shape. Once the mold is filled, a coolant is pumped through the mold to cool the mold and the molten plastic. Once the plastic has solidified, the mold is opened and the article is removed from the mold.

[0146] Another embodiment may include mixing pure copolyester pellets with a concentrate of a flame retardant, with or without the addition of short or long glass fibers, to form a copolyester composition, and then molding the copolyester composition to produce an injection molded article. The pellets are dried at 150°F to 190°F (65.6°C to 87.8°C) for 4 to 6 hours and then added to an injection molding machine. Once the pellets reach the desired temperature, a gate is opened at the end of the extruder and the molten plastic is pumped through a screw into a heated mold to form an article of the desired shape. Once the mold is filled, a coolant is pumped through the mold to cool the mold and the molten plastic. Once the plastic has solidified, the mold is opened and the article is removed from the mold.

[0147] Another embodiment may include mixing pure copolyester pellets with a concentrate of a flame retardant to form a copolyester composition, which is then calendered to produce a film product. Calendering is a well-known method of forming a film or sheet by continuously co-rotating parallel rolls. In certain calendering processes, if the processing temperature is sufficiently low (e.g., 350°F to 400°F; 177°C to 204°C), the pellets do not need to be pre-dried. In this case, degradation and hydrolysis of the polyester may not occur in significant amounts. The copolyester and flame retardant composition may be melted using a high intensity mixer or extruder, including but not limited to a Buss Ko-kneader, a planetary gear extruder, a Farrell continuous mixer, a twin screw extruder, or type mixer. The melt is then conveyed to a calender. A calender generally consists essentially of a system of three or more large diameter heated rollers that convert the high viscosity plastic into a film or sheet. The flat sheet or film is conveyed in the form of a continuous web to cool the sheet. It can then be trimmed to the desired width and then rolled into rolls or sheared or sawn into sheet form.

[0148] Although the copolyester composition can be prepared by mixing or blending a concentrate of the flame retardant and the copolyester, the copolyester composition can alternatively be prepared by blending the flame retardant directly with the copolyester, using any of the mixing or blending methods previously described for preparing the copolyester composition by blending a flame retardant concentrate with the copolyester. The two flame retardants can be mixed or blended with the copolyester simultaneously or sequentially.

[0149] In embodiments, articles comprising any of the copolyester compositions (described herein) may be articles or components of articles configured for or otherwise useful in any application where flame retardant properties are beneficial (e.g., in one or more of the following applications: medical device housings or components, electronic device or peripheral device housings, personal electronic device components, television or monitor housings or components, power tool housings or components, power adapter housings or components, home automation device components, gaming device housings or components, building and construction materials and components, furnishings and home decor components, wiring and connector housings or components, and automotive structural or decorative components).

[0150] The present invention may be further illustrated by the following examples of specific embodiments thereof, but it should be understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the present invention unless otherwise expressly stated.

[0151] Examples

[0152] The following abbreviations are used: J is joule; J / m is joule per meter; MPa is megapascal; FR is flame retardant; FRS is flame retardant synergist, DS is drip inhibitor, IM is impact modifier; RM is reinforcement material; CP is compatibilizer; FOT is flame out time; wt% is weight percent; TPA is terephthalic acid; TMCD is 2,2,4,4-tetramethyl-1,3-cyclobutanediol, and 1,4-CHDM is 1,4-cyclohexanedimethanol. PCTM is glycol-modified polyethylene cyclohexanedimethanol terephthalate. The materials used in the tests are listed in Table 1.

[0153] Table 1: Materials used in the tests

[0154]

[0155]

[0156] The copolyester composition was prepared by compounding the combination of materials by extrusion process using a 26 mm twin screw extruder (Coperion ZSK 26Mc18). OP1240 and filler (534A GF and / or Jetfine3CA, if used) were fed through separate feeders, while all other components were blended with the base resin and fed into the extruder from the main stream. The processing conditions are shown in Table 2.

[0157] Table 2. Extrusion processing conditions

[0158]

[0159]

[0160] The extruded strands are pelletized by a water bath / cutter or underwater pelletizer system to obtain suitable pellet size / shape for further processing.

[0161] The copolyester composition was molded into parts for testing by injection molding using a FANUC 100 injection molding machine. The barrel temperature range was 260 to 280°C, and the water-cooled mold temperature range was 20 to 80°C. The thickness of the test bars was 1.5 mm (for UL 94 testing) and 3.2 mm (for heat distortion temperature testing). Shorter bars were molded for notched cantilever beam testing.

[0162] Examples 1-10 and Comparative Example 1

[0163] Examples 1 to 10 (and Comparative Example 1) were prepared as described above and molded into test parts (or panels). The UL 94 vertical burning and notched Izod impact strengths were measured for each example. The UL 94 vertical burning test results include FOT (seconds for 10 test bars), FD (drop count), and UL 94 classification. The compositions and test results are listed in Table 3 below.

[0164] Table 3 - Examples 1-10 Compositions / Results

[0165]

[0166]

[0167] Review of Table 3 shows that EX.1 to EX.3 show that the combination of OP-1240FR and FA5601 is very effective in achieving a V0 rating at 10%-20% loading in TX1001. In addition, the use of different FR synergists (PA1, SPB-100, and RDP) in EX.4 to EX.10 still requires at least 10wt% of OP1240 to achieve a UL 94 V0 rating.

[0168] Examples 11-16

[0169] Examples 11 to 16 were prepared as described above and molded into test parts (or plaques). UL 94 vertical burning and notched cantilever beam were measured for each example. The compositions and test results are listed in Table 4 below.

[0170] Table 4 - Examples 11-16 Compositions / Results

[0171]

[0172]

[0173] A review of Table 4 shows that many formulations can achieve a V0 rating, but typically with a significant drop in notched Izod impact performance. Additionally, of the impact modifiers tested, AX9800 IM is the most effective, showing the largest improvement in notched Izod impact strength without significantly sacrificing other properties of the TX1001 and TX1501 formulations.

[0174] Examples 17-21

[0175] Examples 17 to 21 were prepared as described above and molded into test parts (or plaques). UL 94 vertical burning and notched cantilever beams were measured for each example similar to Tables 3 and 4. The compositions and test results are listed in Table 5 below.

[0176] Table 5 - Examples 17-21 Compositions / Results

[0177]

[0178]

[0179] Review of Table 5 shows that filled formulations with 15 wt% to 30 wt% glass fiber or talc filler can still achieve a V0 rating.

[0180] Examples 22-26

[0181] Examples 22 to 26 were prepared as described above and molded into test parts (or plaques). UL 94 vertical burning and notched cantilever beam were measured for each example. The compositions and test results are listed in Table 6 below.

[0182] Table 6 - Examples 22-26 Compositions / Results

[0183]

[0184]

[0185] Review of Table 6 shows that the presence of silicone compatibilizer improves the FR properties of the formulations and reduces the FOT compared to formulations without silicone additives. Likewise, Examples 23-25 ​​show significant increases in notched Izod impact strength while improving FR properties.

[0186] The invention has been described in detail with reference to the embodiments disclosed herein, but it will be understood that variations and modifications can be effected within the spirit and scope of the invention.

Claims

1. A copolyester composition comprising: (a) from about 50 wt % to about 95 wt % of a copolyester comprising: (i) a diacid component comprising 70 mol % to 100 mol % of terephthalic acid residues, 0 to 30 mol% of a modified aromatic diacid residue having 8 to 12 carbon atoms, and 0 to 10 mol % of aliphatic dicarboxylic acid residues; and (ii) a diol component comprising 45 mol% to 95 mol% of cyclohexanedimethanol (CHDM) residues, 5 mol% to 65 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues, and 0 to 10 mol% of a modifying diol having 2 to 20 carbon atoms; wherein the copolyester has an inherent viscosity of about 0.5 to 1.2 dL / g, measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C., and wherein the weight % is based on the weight of the copolyester, wherein the total mol % of the dicarboxylic acid components is 100 mol % and the total mol % of the diol components is 100 mol %; and (b) from about 10 wt % to about 20 wt % of a flame retardant additive comprising a metal phosphinate compound; and (c) from about 0.05 wt % to about 0.5 wt % of a drip suppressant additive; wherein the copolyester composition has a UL 94 V-0 rating or better; and The copolyester composition has a notched Izod impact strength of 60 joules / m or more measured according to ASTM D256.

2. The copolyester composition according to claim 1, wherein The copolyester composition further comprises: (d) from about 1 wt % to about 10 wt % of an impact modifier component.

3. The copolyester composition according to claim 1 or 2, wherein The copolyester composition further comprises: (e) from about 0.1 wt % to about 5 wt % of a compatibilizer.

4. The copolyester composition according to claim 3, wherein The compatibilizer comprises a silicone compatibilizer.

5. The copolyester composition according to claim 4, wherein The silicone compatibilizer is a liquid at 25°C.

6. The copolyester composition according to claim 5, wherein The liquid silicone compatibilizer is an alkyl, phenyl or alkyl-phenyl silicone resin that is liquid at 25°C.

7. The copolyester composition according to any one of claims 1 to 6, wherein The diol component comprises: 60 mol % to 95 mol % of cyclohexanedimethanol residues and 5 mol% to 40 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues.

8. The copolyester composition according to claim 7, wherein The diol component comprises: 70 mol% to 95 mol% of cyclohexanedimethanol residues and 5 mol% to 30 mol%, or 10 mol% to 30 mol%, or 15 mol% to 30 mol%, or 20 mol% to 30 mol%, or 15 mol% to 25 mol% of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues.

9. The copolyester composition according to claim 7, wherein The diol component comprises: 60 mol% to 75 mol% of cyclohexanedimethanol residues and 25 mol % to 40 mol %, or 30 mol % to 40 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues.

10. The copolyester composition according to any one of claims 1 to 9, wherein The copolyester has an inherent viscosity of 0.55 to 0.85, or 0.55 to 0.65, or 0.65 to 0.80, or 0.65 to 0.75 dL / g.

11. The copolyester composition according to any one of claims 1 to 10, wherein The flame retardant additive is present in an amount of 11 wt % to 20 wt %, or 12 wt % to 20 wt %, or 15 wt % to 20 wt % of the copolyester composition.

12. The copolyester composition according to any one of claims 1 to 11, wherein The copolyester composition further comprises a flame retardant synergist additive, wherein the flame retardant synergist additive comprises a phosphorus-containing, nitrogen-containing and / or sulfur-containing compound; a phosphorus compound; a phosphazene compound; an oligomeric phosphate ester; or a combination thereof.

13. The copolyester composition according to any one of claims 1 to 12, wherein The copolyester composition comprises an impact modifier selected from a reactive acrylic impact modifier, a non-reactive MBS impact modifier, an epoxy functional impact modifier or a mixture thereof.

14. The copolyester composition according to any one of claims 1 to 13, wherein The copolyester composition further comprises a chain extender comprising a multifunctional epoxide chain extender.

15. The copolyester composition according to any one of claims 1 to 14, wherein The copolyester composition has a notched Izod impact strength of 150, or 200, or 250, or 300, or 500 Joules / m or more measured according to ASTM D256.

16. The copolyester composition according to any one of claims 1 to 15, wherein When tested according to ASTM D256, the copolyester composition exhibits 100% ductile behavior.

17. The copolyester composition according to any one of claims 1 to 16, wherein The copolyester composition may further comprise one or more additional additives selected from colorants, dyes, mold release agents, additional flame retardants, plasticizers, processing aids, rheology modifiers, nucleating agents, antioxidants, light stabilizers, fillers, and reinforcing materials.

18. An article comprising the copolyester composition according to any one of claims 1 to 17.

19. The article of claim 18, wherein the article is in the form of a film, a sheet, a molded part or a profile.

20. The article of claim 18 or 19, wherein the article is selected from medical device housings or components, electronic device or peripheral device housings, personal electronic device components, television or monitor housings or components, power tool housings or components, power adapter housings or components, home automation device components, gaming device housings or components, building and construction materials and components, furniture and home decor components, wiring and connector housings or components, and automotive structural or decorative components.

Citation Information

Patent Citations

  • Processes for dispersing an impact modifier in a macrocyclic polyester oligomer

    EP1694771B1

  • Polyester compositions, method of manufacture, and uses thereof

    EP2139948B1

  • Opththalmic devices comprising polyester compositions formed from 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 1,4-cyclohexanedimethanol

    US20060287484A1

  • Impact-modified polycarbonate / polyester or polycarbonate / polyamide compositions

    US20140256848A1

  • Process for preparing aromatic diester containing copolyesters and products obtained thereby

    US3772405A