Nylon composition

By introducing alkyl substituents into poly-2-pyrrolidone and using basic polymerization catalysts, the thermal instability of nylon is solved, its processing performance and biodegradability are improved, and more efficient fiber production is achieved.

CN118946636APending Publication Date: 2024-11-12SALEM LABORATORIES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027574.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-16
Filing Date
2023-02-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The thermal instability of nylon makes it difficult to process and is easy to degrade during melt spinning, resulting in a decrease in the molecular weight and structural defects of the product, affecting its tensile strength and fibrotic properties.

Method used

By introducing alkyl substituents of amide groups into poly-2-pyrrolidone, the polymer chain structure is adjusted, and polymerization is carried out in the presence of alkaline polymerization catalyst and carbon dioxide, reducing the melting temperature and improving thermal stability, forming a modified Polyamide composition.

Benefits of technology

The thermal stability and processing properties of the polymer are improved, the melting point is reduced, and the biodegradability is maintained, making the polymer easier to process into useful products without degradation, and the tensile strength and fibrosis characteristics of the fiber are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005042318210000011
    Figure BDA0005042318210000011
  • Figure BDA0005042318210000031
    Figure BDA0005042318210000031
  • Figure BDA0005042318210000032
    Figure BDA0005042318210000032
Patent Text Reader

Abstract

The polyamide includes a plurality of amide units forming a polymer chain, and an alkyl substituent on the amide group. The polyamide has substitutions of amide units in an amount of from about 0.1% to about 10% of the amide units in the polymer chain. A method of forming a polyamide composition includes providing a polyamide comprising a plurality of amide groups in a backbone structure of the polyamide, and modifying a portion of the plurality of amide groups in the backbone structure with one or more alkyl substituents to form the polyamide composition, wherein the amide units of the polyamide are substituted in an amount of about 0.1% to about 10% of the amide units in the main chain.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority to and the benefit of U.S. Provisional Patent Application No. 63 / 310,758, filed on February 16, 2022, entitled “NYLON COMPOSITIONS,” the entire contents of which are incorporated herein by reference. Background Art

[0002] Nylon can be produced by the polymerization of amide units, and the type of nylon produced can be determined by reference to the number of carbon atoms in the monomer units polymerized. Due to the presence of the amide units, nylon may not be as stable as other types of polymers (such as polyethylene). Instabilities may include thermal instability, which makes processing of nylon difficult. Summary of the invention

[0003] In some embodiments, the polyamide comprises a plurality of amide units forming a polymer chain, and alkyl substituents on the amide groups. The polyamide has an amide unit substitution amount of between about 0.1% and about 10% of the amide units in the polymer chain.

[0004] In some embodiments, the poly-2-pyrrolidone polymer comprises the formula: Wherein, m may be 3, R comprises an alkyl substituent on the amide group, and the amount of the amide group substituent of the poly-2-pyrrolidone is from about 0.1% to about 10% of the amide group in the poly-2-pyrrolidone.

[0005] In some embodiments, a method of forming a polyamide composition includes providing a polyamide, wherein the polyamide comprises a plurality of amide groups in a main chain structure of the polyamide, and modifying a portion of the plurality of amide groups in the main chain structure with one or more alkyl substituents to form the polyamide composition. The amide unit substitution amount of the polyamide is between about 0.1% and about 10% of the amide units in the main chain.

[0006]

[0011] These and other features will become more clearly understood from the following detailed description taken in conjunction with the accompanying drawings and claims. DETAILED DESCRIPTION

[0007] Various nylons or polyamides can be modified to provide useful polymers. For example, poly-2-pyrrolidone can be prepared by base-catalyzed polymerization of 2-pyrrolidone in the presence of various compounds such as carbon dioxide. According to the polymerization of monomers containing 4 carbon atoms, the resulting polymer may be referred to as nylon 4 in some cases. Additional modifications can be used to change the properties of polypyrrolidone (e.g., melting temperature, degradation temperature, molecular weight, functionalization, etc.), and the resulting material can show improved biodegradability compared to other polymers (e.g., olefin polymers including polyethylene, polypropylene, etc.). In terms of the fact that the article can be made of degradable materials, the environmental persistence of such polymers can be reduced relative to other polymers.

[0008] The resulting polypyrrolidone can be formed into various forms and various products to obtain a variety of end uses, including sheets, films, filaments, tapes, molded articles and fibers. Polypyrrolidone fibers have long been considered to have great commercial potential due to their hydrophilic properties, which are very similar to those of cotton and silk. For example, compared with other currently available synthetic fibers, fabrics made from polypyrrolidone are as easy to dye as cotton, they can be ironed at cotton temperatures, static electricity can be quickly dissipated, and in particular, the fabrics have the comfort of cotton, silk and wool.

[0009] There is a balance between biodegradability and the ability to form useful articles from polymers. In order to form filaments and fibers, polymers can be melt-spun into filaments by extrusion from a spinneret. In melt spinning, the polymer composition is extruded under molten conditions at a melt temperature that is generally greater than about 270°C. This extrusion must be done carefully because thermal degradation of the polymer may cause the polymer to be converted back into monomers. In addition to causing a large amount of product loss and increasing processing costs, this can also cause bubbles to form in the extrudate or filaments and form voids or pits. In addition, in addition to returning to monomers, the molecular weight will also degrade during the melt spinning process, resulting in a molecular weight of poly-2-pyrrolidone filaments that is significantly lower than the molecular weight of the original polymer. If the molecular weight of the original polymer is too low or if the molecular weight degradation is too severe, the molecular weight of the filament will not be enough to provide sufficient tensile strength and fiberization characteristics for the filament.

[0010] In addition to melt spinning, solution spinning is also a method for forming useful articles from polymers. If solution spinning is used, the polymer is dissolved in a solvent until a high concentration is reached, which is usually called a spinning solution (dope), and then the spinning solution is extruded into a non-solvent, where precipitation occurs to form the article. The typical concentration of the spinning solution can be between 2.5wt% and 50wt%, and a high viscosity solution is formed, the viscosity of which ranges from 1000 centipoise to 1,000,000 centipoise or higher, most preferably 5000 centipoise to 50,000 centipoise. Examples of solvents that can be used are acids, polar protic solvents, polar aprotic solvents, ionic liquids, fluorinated alcohols, etc.

[0011] Another problem is that, although higher molecular weight polymers (e.g., about 120,000 and above) have better thermal stability, they also have higher viscosity and are more difficult to extrude. If extrusion is attempted at significantly lower temperatures to avoid thermal degradation, the material cannot be fully melted, resulting in fibers with significantly lower tensile strength. Therefore, in order to effectively melt extrude polypyrrolidone, the thermal stability of the polymer and / or the extrudability of the polymer composition can be improved.

[0012] In some aspects, a polypyrrolidone is disclosed herein that allows for lowering the melting temperature and / or increasing thermal stability, thereby improving the processability of the polymer. In some aspects, the disclosed method and the resulting polymer allow for lowering the melting point of the resulting polymer without affecting the degradation temperature. Alternatively, it is also possible to increase the degradation temperature of the resulting polymer without affecting the melting point. This can then make the polymer more easily processed and formed into useful articles without degrading the polymer in the process.

[0013] The present disclosure relates to various polyamide compositions that can be modified to improve processing properties and simultaneously maintain biodegradability. Although various nylons can be produced as the method provided herein, in some aspects, as an example, a poly-2-pyrrolidone composition modified to have improved thermal stability is described herein, and a method for processing poly-2-pyrrolidone to prepare a modified poly-2-pyrrolidone composition. Other polyamides, such as nylon 3, nylon 4, nylon 6, proteins and other types of nylon (such as nylon 2,2, nylon 3,3, etc.) can be similarly modified to improve performance according to the method provided, including reducing melting point and / or increasing degradation temperature. In general, the modification techniques described herein can be used for any suitable polyamide.

[0014] Any suitable technique may be used to polymerize 2-pyrrolidone to form poly-2-pyrrolidone. A method for polymerizing 2-pyrrolidone to form poly-2-pyrrolidone (which may also be referred to as polypyrrolidone) may include polymerizing 2-pyrrolidone in the presence of a basic polymerization catalyst (and, if desired, an activator). Cationic ring-opening polymerization methods may also be used.

[0015] The polymer formed from 2-pyrrolidone is considered a linear polyamide, which is called nylon-4 and has the following structure: Where n can range from about 200 to over 1,000,000, or in some aspects up to 100,000. In some aspects, n can range up to about 10,000, or about 5000, depending on the type of nylon being considered. A more general formula for nylon formed from common starting materials may include: Wherein, when m is 1, the polyamide is nylon 2; when m is 2, the polyamide is nylon 3; when m is 3, the polyamide is nylon 4; n can be any value described above for Formula 1, and, as provided herein, R can be modified by hydrogen or other alkyl groups.

[0016] In some aspects, polypyrrolidone can be prepared by polymerizing 2-pyrrolidone using a basic polymerization catalyst in the presence of carbon dioxide (CO2). For example, polymerization can be achieved by passing CO2 in the form of bubbles through a mixture of 2-pyrrolidone and an alkali metal salt of 2-pyrrolidone (e.g., sodium pyrrolidate or potassium pyrrolidate), the alkali metal pyrrolidone salt being used as a basic polymerization catalyst. Polypyrrolidone can also be prepared by reacting CO2 with an alkali metal salt of 2-pyrrolidone to form an adduct of CO2 and an alkali metal pyrrolidone salt, and then polymerizing 2-pyrrolidone monomer in the presence of the adduct.

[0017] In certain aspects, the polymerization of 2-pyrrolidone can be carried out in the presence of CO2 using a basic polymerization catalyst. The 2-pyrrolidone monomer can be polymerized at a temperature of 18°C ​​to about 100°C, preferably at a temperature of 25°C to 70°C, and most preferably at a temperature of 25°C to 60°C, in the presence of a basic polymerization catalyst, at a pressure range from subatmospheric to superatmospheric. Bulk polymerization or suspension polymerization can be used.

[0018] The basic polymerization catalyst can be any catalyst for polymerizing 2-pyrrolidone. Suitable basic polymerization catalysts are derivatives of alkali metals, such as hydroxides and oxides of alkali metals, including potassium tert-butoxide. Alkoxides of alkali metals can also be used, such as sodium methoxide. In addition, oxides and hydroxides of alkaline earth metals (such as calcium and barium) can also be used as catalysts. In addition, organometallic compounds can also be used, preferably those with strong alkalinity, such as alkyl compounds of lithium, potassium and sodium (such as butyl lithium), and aryl compounds of alkali metals (such as sodium phenyl and sodium amide). The basic polymerization catalyst can be a quaternary ammonium base. In addition, as mentioned above, the catalyst can be an alkali metal hydride, such as sodium hydride. Although certain alkali metal derivatives can be used, many of them are not ideal. For example, alkali metal carbonates and alkaline earth metal hydroxides tend to be insoluble and are therefore not ideal. Lithium hydroxide (monohydrate) is also insoluble in 2-pyrrolidone.

[0019] In some aspects, nonionic bases can also be used as catalysts. For example, polymerization can be catalyzed by strong, nitrogen- and phosphorus-containing nonionic bases. Effective catalysts or initiators can include nonionic bases with a pKa equal to or greater than 30. Examples of useful nonionic bases can include polyaminophosphazenes, which include phosphazene bases with the following structure: Among them, R 1 is (C1-C8)alkyl, wherein when the alkyl group is greater than C3, it is branched or straight chain, and R is methyl (Me) or two R together form --(CH2)4--, and m, n and y are independently 0-3, or preferably as defined below for a specific phosphazene base Px (x=1 to 7) base. Preferred R 1 Groups include tert-butyl, tert-heptyl (--C(CH3)2C(CH2)3) and tert-octyl (--C(CH3)2CH2 C(CH2)3). Preferred R is methyl and --(CH2)4--. When a nonionic base is used as a catalyst, the polymerization can be carried out at a temperature of about 25°C to about 200°C, depending on the type of polyamide being polymerized. Generally speaking, the lower the molecular weight of the monomer, the lower the polymerization temperature.

[0020] Based on the 2-pyrrolidone monomer, the catalyst may be used in an amount of about 0.5 wt.% to about 50 wt.% or more, preferably 5 wt.% to 30 wt.%, and most preferably 8 wt.% to 20 wt.%.

[0021] The preferred ratio of CO2 to the basic polymerization catalyst has been found to be from about 2 to about 20 moles of catalyst per mole of CO2, or alternatively, from about 4 to about 10 moles of catalyst per mole of CO2. The temperature at which the CO2 is added to the catalyst can vary widely, with results being obtained at temperatures ranging from 18°C ​​(approximately the freezing point of the catalyst solution in the monomer) to 130°C or more, or at temperatures between about 40°C and about 60°C.

[0022] In certain aspects, the basic polymerization catalyst is an alkali metal salt of 2-pyrrolidone, such as sodium pyrrolidone or potassium pyrrolidone. When CO2 is bubbled into a reaction mixture of 2-pyrrolidone monomer and an alkali metal pyrrolidone catalyst, an adduct of CO2 and an alkali metal pyrrolidone catalyst is formed. It has been found that this adduct can be used for polymerization when an alkali metal pyrrolidone catalyst is also present.

[0023] CO2 can be bubbled into a mixture of 2-pyrrolidone monomer and alkali metal pyrrolidone salt in a ratio of about one quarter to about one mole of CO2 per mole of alkali metal pyrrolidone salt, although more or less CO2 may be used. If a larger amount of CO2 is used, for example, more than 0.5 mole of CO2 is used per mole of alkali metal pyrrolidone salt, the additional CO2 may not be easily absorbed. If a smaller amount of CO2 is used, for example, 2 moles of alkali metal pyrrolidone salt are used per 0.5 mole of CO2, the reaction mixture will contain 2-pyrrolidone monomer, alkali metal pyrrolidone salt, and CO2-alkali metal pyrrolidone salt adduct. Generally speaking, good results can be obtained by stopping the addition of CO2 before approaching absolute saturation, although this is not necessary. The best results are obtained by using slightly less than 1 / 2 mole of CO2 per mole of alkali metal pyrrolidone salt, for example, a ratio of 1 / 4 to 3 / 8 mole of CO2 per mole of pyrrolidone salt. In any case, the reaction mixture is then placed in a polymerization vessel to polymerize the monomer with or without further addition of CO2. If desired, the reaction between the CO2 and the alkali metal pyrrolidone salt can be carried out prior to contacting the bulk of the 2-pyrrolidone monomer.

[0024] Although the process described herein occurs in the presence of CO2, the process can also occur without adding any CO2, wherein the remaining components and conditions can remain unchanged. Even if CO2 is not added to the process, polymerization will occur as described, but the reaction time will be longer and the conversion rate will be lower.

[0025] In some aspects, the polymerization of 2-pyrrolidone can be carried out in the following manner. First, the 2-pyrrolidone monomer is reacted with an alkali metal hydroxide (preferably NaOH or KOH), and the water formed in the reaction is removed by distillation, thereby forming an anhydrous solution of an alkali metal salt of 2-pyrrolidone in situ in the 2-pyrrolidone to be polymerized. The removal of water can be carried out under subatmospheric pressure conditions (e.g., under a pressure of 14.7 psia below atmospheric pressure) and at a temperature of 18°C ​​to 150°C, preferably between 25°C and 100°C, and most preferably between 25°C and 45°C. In the presence of water, harmful reactions may occur and lead to the ring opening of the 2-pyrrolidone monomer, thereby inhibiting the polymerization reaction. In addition to alkali metal hydroxides, alkali metal pyrrolidone salts can also be formed by using alkali metal alcoholates (preferably NaOCH3 or KOCH3), thereby forming an alkali metal pyrrolidone salt solution in 2-pyrrolidone. Any alkali metal source can be used to form pyrrolidone salts as long as undesirable byproducts are not formed and the sensitive pyrrolidone ring is not damaged. Undesirable byproducts are those that act as polymerization inhibitors. Sodium metal is an example of an alkali metal source that should not be used. After removing water from the reaction mixture, CO2 can be introduced in the form of bubbles to form an alkali metal pyrrolidone salt-CO2 adduct in situ to start polymerization. If necessary, additional 2-pyrrolidone monomer can be added to the alkali metal pyrrolidone salt solution before introducing CO2. In appropriate cases, the 2-pyrrolidone monomer can be contacted with 0.01wt.% to 10wt.% CO2 based on the weight of the 2-pyrrolidone monomer. For example, based on the weight of 2-pyrrolidone, an amount of 0.2wt.% to 6wt.%, or 0.5wt.% to 3wt.% can be used.

[0026] Alternatively, polymerization of 2-pyrrolidone can occur by reaction of the monomer with potassium tert-butoxide. This base or a similar base can be used in a method similar to the above method, wherein the conditions and components can be the same or similar. However, in the example using potassium tert-butoxide, it is the tert-butyl alcohol that is removed, rather than water. In addition, the reaction proceeds as described above.

[0027] The amount of carbon dioxide can also be expressed as a molar percentage of the number of moles of the basic polymerization catalyst. Thus, the amount of carbon dioxide will be about 0.06 to 60 mole percent based on the number of moles of the basic polymerization catalyst, but higher amounts, such as up to about 80 mole percent of CO2 based on the number of moles of the basic polymerization catalyst have been used. Typically, the amount of CO2 based on moles is 10 to 80 mole percent based on the number of moles of the basic polymerization catalyst.

[0028] In addition to bubbling CO2 into the mixture of 2-pyrrolidone and alkaline polymerization catalyst, CO2 can also be introduced into the system by other methods. For example, the CO2 source can be a compound that transfers CO2 to the mixture of 2-pyrrolidone monomer and alkaline polymerization catalyst, provided that the remaining anions of the compound after the loss of CO2 do not adversely affect the polymerization. Adducts of carbon dioxide and alkali metal or quaternary ammonium pyrrolidone monomer and alkaline polymerization catalyst can be added to the mixture of 2-pyrrolidone monomer and alkaline polymerization catalyst. Similarly, adducts of CO2 and alkali metal or quaternary ammonium caprolactam can also be added to the system regardless of whether any CO2 gas is added to the system. These adducts are added to the system on the same weight basis as CO2. A convenient method for preparing the adduct is to bubble CO2 into an anhydrous mixture of pyrrolidone and 2-pyrrolidone under vacuum until the pressure rises sharply, indicating that CO2 is no longer readily absorbed. The adduct is precipitated by adding benzene or other organic precipitant to the solution. A free-flowing, non-hygroscopic white powder is recovered from the precipitate. Alternatively, an organic precipitant may be added to an anhydrous solution of a pyrrolidone salt of 2-pyrrolidone prior to bubbling CO2 through the solution, in which case a precipitate forms as the CO2 is absorbed. Because it is necessary to react the CO2 with an anhydrous pyrrolidone salt, it is preferred to form the CO2-pyrrolidone salt adduct by adding the CO2 to an anhydrous solution of a pyrrolidone salt in 2-pyrrolidone, wherein the pyrrolidone salt is formed in situ as described herein.

[0029] Similarly, an adduct of CO2 and a caprolactam salt is formed by bubbling CO2 through an anhydrous solution of a caprolactam salt in caprolactam and adding an organic precipitant before or after the addition of CO2. Generally, temperatures exceeding 90°C should be avoided when forming the caprolactam salt in situ.

[0030] In certain aspects, carbon dioxide can be used as the sole polymerization activator, although other polymerization activators can be used with carbon dioxide. Other activators that can be used with carbon dioxide are acyl compounds, such as organic acyl peroxides, carboxylic acid anhydrides, lactones, lactides, N-acyl derivatives of lactams, acyl halides, and alcohol esters of carboxylic acids.

[0031] In addition, any of the following activators can be used: carbon disulfide, N-substituted secondary amides, cyanuric chloride, organic isocyanates, adipic acid imide, N-iminopyrrolidone, N-monocarbonylpyrrolidone and organic acid amides, aromatic carbonyl and organic acid amides, chlorine, bromine, N-bromopyrrolidone or N-chloropyrrolidone, NO2 or organic nitrites, P2O5 and other oxides or oxides of group V elements, N,N-disubstituted ureas, halides and halogenides of sulfur and phosphorus, oxides of group VI elements, halogenated silanes, phenylphosphine dichloride, phenylphosphine oxychloride, phosphorus trichloride, thionyl chloride and / or tetramethylammonium chloride. These activators can be used as substitutes for CO2, or as a supplement to CO2 for polymerization reactions. They can be added before adding CO2, or, preferably, after adding CO2. For example, in the case of using tetramethylammonium chloride, after forming the CO2 adduct, tetramethylammonium chloride is added to the solution, mixed thoroughly, and then polymerized.

[0032] Typically, the polymerization can be carried out under substantially anhydrous conditions, although anhydrous conditions are not required. For example, the water content can be less than about 1% based on the weight of the 2-pyrrolidone monomer, or less than about 0.1% based on the weight of the 2-pyrrolidone monomer. The 2-pyrrolidone used in the polymerization can be substantially pure. For example, the 2-pyrrolidone monomer can be purified by vacuum fractionation or recrystallization or a combination of both.

[0033] The resulting polymerized polypyrrolidone may have a formula of Formula 1 as shown above. Other polyamides may also be used herein for modification, with a more general polyamide formula being shown in Formula 2. For example, nylon 3 may be prepared by ring-opening polymerization of β-propiolactam using a base as described herein, or acrylamide may be polymerized to produce a polyamide. Similarly, nylon-2 may be synthesized using polymerization of glycine N-carboxyanhydride (NCA) and any other suitable method. Other polyamides may be produced using any suitable method.

[0034] In order to improve the stability of the resulting polypyrrolidone, the structure of the polypyrrolidone can be modified to a certain extent to change the properties of the polymer. In some aspects, the amide groups on the main chain structure of the polypyrrolidone can be modified between about 0.1% to about 10%, or between about 0.2% to about 8%, or between about 0.5% to about 5%. The percentage modification used herein refers to the average modification amount (number average modifications) of the amide units or amide groups on the polypyrrolidone main chain.

[0035] The resulting substituted polypyrrolidone may have the formula: Wherein, n is as shown in Formula 1, m is the same as in Formula 1, and any one of R1, R2 and R3 may contain a hydrogen atom or an alkyl substituent. Other substituents suitable for substitution as R may include methoxy, hydroxymethyl, methylmethoxy, etc. In some aspects, this may result in R=MeOH, MeOMe, MeOEt or MeOR. In different aspects, R may be any alkyl using a suitable substituent. In some aspects, the oxygen atom and sulfur atom contained in the repeating unit may be introduced or used to change the properties of the polymer. Although various methyl groups have been provided, these groups may also include EtOH and EtOMe, which all belong to the groups defined in the present invention for alkyl. The term "alkyl" used herein may refer to straight-chain alkyl and branched alkyl, and includes alkylene. Typical alkyl groups include, for example, methyl, methylene (--CH2--), ethyl, isopropyl, n-butyl, tert-butyl, hexyl, decyl, tetradecyl, 4-methylhexadecyl, eicosyl, etc. The term "alkyl" includes lower alkyl groups, wherein "lower alkyl" refers to an alkyl group having 1 to 6 carbon atoms.

[0036] In some aspects, the R group can be a reactive group. For example, the R group can be an epoxy group, an isocyanate group or a similar reactive component. The modification ability of the main chain can be achieved in the same manner as described herein with such groups, and the reactive group can change the chemical properties of the resulting polymer.

[0037] As shown in Formula 2, the modification may be associated with the amide groups in the polypyrrolidone, and the remaining groups, including the carboxyl groups, may not be significantly modified, and in some aspects, the modification of the carboxyl groups in the final polypyrrolidone composition may be less than 0.1%.

[0038] The modification process of polypyrrolidone can be achieved by contacting poly-2-pyrrolidone (Formula 1) with a base to remove the proton of the amide backbone, and then contacting with an alkylating agent under reaction conditions. Alternatively or additionally, the polymer can react with formaldehyde in the presence or absence of exposure to alcohol or thiol to modify the amide backbone. The process is usually carried out at a temperature of about 18°C ​​to about 265°C, and the duration is about from 0.1 hour to about 120 hours. Typically, about 0.1 to 10 moles of modifier are used per mole of polypyrrolidone. In order to maximize the contact of the polymer with the modified solution, the base polymer can be contacted as a finely divided powder. In addition, the base polymer can be dissolved in a suitable solvent for reaction. Such suitable solvents are organic acids (e.g., formic acid), fluorinated alcohols (hexafluoroisopropanol), polar protic solvents (DMF), polar aprotic solvents (DMSO, DMAc, NMP), or any solvent in which both the polymer and the reactant are soluble. The reaction rate is usually temperature dependent, therefore, the higher the reaction temperature, the shorter the reaction time, and vice versa. By adjusting the reaction time and reaction temperature as well as the above reaction conditions, the degree of substitution can be controlled accordingly.

[0039] Suitable modifying agents that can be used to modify the polypyrrolidones described herein can include, but are not limited to, formaldehyde, paraformaldehyde, methyl iodide, methanol, ethanol, sodium hydride, and the like.

[0040] In certain aspects, for example, in addition to backbone modification, polypyrrolidone can also be modified at one or more ends. In these aspects, polypyrrolidone can be modified with certain alkanolamines or alkylene polyamines [e.g., NH2(CH2) n NH2] is reacted for a sufficient time to achieve the desired capping. The end groups of polypyrrolidone may be unstable and open under very mild conditions (e.g., when in contact with water at room temperature).

[0041] The end-capping can result in the capping of one or more ends (e.g., any carboxyl end groups). In the case of using direct end-capping, the molecular weight of the product is close to (but usually slightly less than) the weight average molecular weight of the starting material polymer. The end-capping method of the present invention can be carried out by contacting the polypyrrolidone with an alcohol amine before or after any main chain modification, and the temperature range is about 20°C to 100°C, preferably about 25°C to 80°C, and the reaction time is about 0.5 to 50 hours, preferably about 1 to 30 hours.

[0042] The amount of end-capping agent can be selected to provide the required end-capping amount. In some respects, one to two moles of end-capping agent can be used per mole of polymer. The molar ratio between end-capping agent and polypyrrolidone is 2:1, which theoretically causes both ends of polypyrrolidone to be end-capped. However, in some respects, excessive end-capping agent (for example, the ratio of end-capping agent to polypyrrolidone is greater than 2:1) can be used to ensure full contact with polymer. Therefore, usually per gram of polymer can use about 2 to 10 grams, preferably about 2 to 4 grams of end-capping agent. Alternatively, it is also possible to advantageously use an inert organic diluent or an inert organic solvent suitable for end-capping agent to reduce the amount of required alkanolamine and / or alkylenediamine, to maximize the contact of polymer and facilitate operation.

[0043] Suitable alkanolamine capping agents that can be used may include, but are not limited to, alkanolamines having 2 to 12 carbon atoms, preferably 2 to 6 carbon atoms, and at least one hydroxyl substituent and at least one amino substituent, each substituent being substituted on a different carbon atom. The alkanolamine may also be selectively substituted with up to five and including a total of five hydroxyl and / or amino substituents, which are substituted on different carbon atoms. Importantly, the carbon atom contains only a single substituent, because compounds with carbon atoms having two amino groups or two hydroxyl groups or one amino group and one hydroxyl substituent are unstable, and such compounds are expected to degrade in the polymer during the initial process and / or during melt spinning. Suitable alkanolamine species that can be used include, for example, ethanolamine, 3-aminopropanol, 10-aminodecanol; 4-amino-2-ethylbutanol; 2-hydroxy-4-aminobutanol, 2,4-diaminobutanol, 2-hydroxymethyl-5-aminopentanol, etc.

[0044] Suitable alkylene polyamines that can be used in the end-capping process may include, for example, alkylene polyamines having 2 to 12 carbon atoms, preferably alkylene polyamines having 2 to 6 carbon atoms, which are substituted with 2 to 5 amino substituents (each amino substituent is located on a different carbon atom), and optionally, the alkylene polyamines are substituted with 1 to 3 hydroxyl substituents (each hydroxyl substituent is located on a different carbon atom), up to 5 and including a total of 5 such substituents. Suitable alkylene polyamine species include, for example, ethylenediamine, hexamethylenediamine, dodecenyldiamine; 1,5-diamino-2-methylpentane; 1,2,4-triaminobutane; 1,5-diamino-3-hydroxyhexane; 1,2,6-triamino-4-3-hydroxyethylhexane, etc. In terms of thermal stability of the end-capped polymer product of a given molecular weight, the best results are generally obtained using alkanolamines (especially ethanolamine). In the case of using alkylene polyamines, alkylene diamines such as ethylenediamine and hexamethylenediamine are preferably used.

[0045] In addition, various cyclic lactams can be used in the end-capping process, such as caprolactam, laurolactam, etc.

[0046] Endcapping can improve thermal stability, which can facilitate melt extrusion, especially melt spinning, of the compositions of the present invention at temperatures ranging from 260°C to 285°C, or temperatures below about 280°C, or temperatures below 275°C.

[0047] Modification of polypyrrolidone can result in a modified polymer having a lower melting temperature. In certain aspects, the melting temperature can be reduced by about 0.1°C to about 20°C, or about 1°C to about 10°C, compared to the base polypyrrolidone.

[0048] The resulting modified polypyrrolidone may have a melting temperature of about 220° C. to about 400° C., or about 245° C. to about 260° C. In certain aspects, the degradation temperature of the modified polypyrrolidone (e.g., based on backbone or end-capping modification) is at least about 200° C. or at least about 300° C., or between about 290° C. and about 330° C.

[0049] The temperature difference between the melting temperature and the degradation temperature can be expanded to allow a larger temperature range to form useful articles. In certain aspects, the temperature difference can be between about 10°C and about 60°C, which can be greater than the difference between the melting temperature and the degradation temperature of unmodified polypyrrolidone.

[0050] Although described herein for nylon 4, any suitable polyamide composition can be modified as described herein. Specifically, the same main chain and end-capping process can be used for other nylons, such as nylon 2, nylon 3, nylon 6, etc. In some aspects, the modifications provided herein can be used for proteins. In some aspects, proteins can be regarded as functionalized nylon 2, and these compounds can be either natural sources or made using new biotechnology. The final chemical properties of proteins may be similar to the chemical properties of polypyrrolidone described herein. In general, the degradation temperatures of nylon 2, nylon 3 and proteins may be lower than the melting points of these polymers. Using the modification techniques provided herein can reduce the melting point and / or increase the degradation temperature enough to make polymers and proteins more easily processed using any process described herein. Example

[0051] After the disclosure has been generally described, the following examples are given as specific embodiments of the disclosure to demonstrate its practice and advantages. It should be understood that the examples are given only as illustrations and are not intended to limit the specification or claims in any way. Example 1

[0052] Example 1: In the example, 0.5 g of polypyrrolidone was dissolved in 17 mL of formic acid at 60°C. 57 mg of paraformaldehyde was suspended in 680 mg of methanol at 60°C. At the same time, an additional 680 mg of methanol was also incubated at 60°C. After the polypyrrolidone was completely dissolved in the formic acid, the paraformaldehyde solution was quickly added. The formic acid solution, which now contained polypyrrolidone, paraformaldehyde and methanol, was allowed to react at 60°C for 5 minutes. At the end of this time, an additional 680 mg of methanol was quickly added to the solution and reacted for 30 minutes. After the reaction time was over, the solution was added dropwise to 350 mL of cold acetone. The precipitate was then taken out, soaked in 150 mL of clean acetone for 10 minutes, taken out and dried at 50°C. The melting point of this sample was 259°C, the degradation temperature was 313°C, and the initial melting point temperature of polypyrrolidone was 267°C, and the degradation temperature was 288°C. Example 2

[0053] Example 2: The reaction conditions are similar to those of Example 1, except that 100 mg of paraformaldehyde is suspended in 680 mg of methanol. In addition, the reaction time after adding the paraformaldehyde suspension is 10 minutes. The melting point temperature of this sample is 226°C, and the degradation temperature is >304°C. Example 3

[0054] Example 3: The reaction conditions are similar to those described above, except that 159 mg of paraformaldehyde is suspended in 680 mg of methanol. The melting point of this sample is 218°C, and the degradation temperature is >303°C. Example 4

[0055] Example 4: 1.07 g of polypyrrolidone was added to a test tube containing 1.6 g of formic acid, 1.07 g of paraformaldehyde, and 5.4 ml of methanol. The test tube was shaken by hand, sealed, and placed in an oven at 50°C for 119 hours. The sample was then washed with excess 1:1 acetone:water, filtered, and then washed with excess acetone. The sample was dried. The melting point temperature of this sample was 263°C and the degradation temperature was 306°C. Example 5

[0056] Example 5: 11.2 g of pyrrolidone was mixed with 0.869 g of KOH at 110°C under N2 atmosphere until KOH was completely dissolved, causing pyrrolidone to polymerize into polypyrrolidone. After the sample was completely dissolved, it was stirred for at least 10 minutes. Dehydration was performed by short-path distillation, removing about 10% of the volume to ensure dryness. The reaction was then cooled to <60°C under N2 atmosphere, and CO2 was then bubbled into the solution to produce a turbid yellow suspension. The suspension was then placed in a scintillation bottle and placed in an oven at 50°C for at least 8 hours. After the reaction was completed, the solid polypyrrolidone was removed from the bottle, mechanically crushed into small pieces, washed with excess water and dried. The melting point temperature was 263°C. Example 6

[0057] Example 6: The polymerization conditions are similar to those of Example 5, except that after adding CO2 to the solution, 1.422 g of tetramethylammonium chloride (pre-dried) is added and stirred for 5 minutes. The solution is then transferred to a bottle, placed in an oven at 50°C and reacted for at least 8 hours. The purification process is the same as that of Example 5. The melting point of this sample is 264°C and the degradation temperature is 282°C. Example 7

[0058] Example 7: The purified sample in Example 6 was dissolved in formic acid and precipitated in water. The sample was then filtered and washed with excess water to neutralize the solution. The polypyrrolidone was then dried. The melting point temperature of this sample was 266°C and the degradation temperature was 299°C. Example 8

[0059] Example 8: Polymerization of pyrrolidone Same as Examples 5 and 6, but using 1.477 g potassium tert-butoxide instead of KOH. After purification, the melting point temperature of this sample is 267°C and the degradation temperature is 285°C. Example 9

[0060] Example 9: The polymer of Example 8 was dissolved in formic acid and purified as in Example 7. The melting point of this sample was 264°C and the degradation temperature was 294°C. Example 10

[0061] Example 10: 1 g of polypyrrolidone was mixed with 3 g of ethanolamine. The bottle was kept at 150°C for 40 minutes. The bottle was then cooled, the polymer was washed with excess water and dried. The melting point temperature of the sample was 268°C and the degradation temperature was 304°C. Example 11

[0062] Example 11: A sample of polypyrrolidone with a reduced melting point (Example 2) was reacted with ethanolamine to modify the endcapping (as described in Example 10). The melting point temperature of this sample was 231°C and the degradation point was >321°C.

[0063] Having described certain compositions and methods, specific aspects may include, but are not limited to, the following:

[0064] In a first aspect, a polyamide includes a plurality of amide units forming a polymer chain; and includes alkyl substituents on the amide groups, wherein the polyamide has a substitution of the amide units in an amount ranging from about 0.1% to about 10% of the amide units in the polymer chain.

[0065] The second aspect may include the polyamide of the first aspect, wherein the polymer chain includes end caps, and wherein at least a portion of the end caps include alkyl substituents.

[0066] The third aspect may include the polyamide of the first or second aspect, wherein the alkyl substituent is methyl, ethyl or butyl.

[0067] The fourth aspect may include the polyamide of any one of the first to third aspects, wherein the polymer is biodegradable.

[0068] The fifth aspect may include the polyamide of any one of the first to fourth aspects, wherein the polymer is in the form of a sheet, a film, a filament, a tape, a molded article, a woven material, or a fiber.

[0069] The sixth aspect may include the polyamide of any one of the first to fifth aspects, wherein the melting point of the polymer is between 220°C and about 400°C.

[0070] A seventh aspect may include the polyamide of any one of aspects 1 to 6, wherein the degradation temperature of the polymer is at least about 200°C.

[0071] An eighth aspect may include the polyamide of any one of aspects 1 to 7, wherein the temperature difference between the melting temperature and the degradation temperature of the polymer is at least about 20°C.

[0072] The ninth aspect may include the polyamide of any one of the first to fifth aspects, wherein the polyamide is nylon 2, nylon 3, nylon 4, nylon 6, or protein.

[0073] In a tenth aspect, the poly-2-pyrrolidone polymer comprises the formula: wherein m is 3, R comprises an alkyl substituent on the amide group, and the amount of the amide group substituent of the poly-2-pyrrolidone is from about 0.1% to about 10% of the amide group in the poly-2-pyrrolidone.

[0074] The eleventh aspect may include the polymer of the tenth aspect, wherein R is methyl, ethyl, or butyl.

[0075] The twelfth aspect may include the polymer of the eleventh aspect, wherein the polymer has a melting point between 220°C and about 400°C.

[0076] A thirteenth aspect may include the polymer of any one of the tenth to twelfth aspects, wherein the polymer has a degradation temperature of at least about 200°C.

[0077] A fourteenth aspect may include the polymer of any one of aspects ten to thirteen, wherein the temperature difference between the melting temperature and the degradation temperature of the polymer is at least about 20°C.

[0078] A fifteenth aspect may include the polymer of any one of the tenth to fourteenth aspects, wherein the polymer is biodegradable.

[0079] A sixteenth aspect may include the polymer of any one of the tenth to fifteenth aspects, wherein the polymer is in the form of a sheet, a film, a filament, a tape, a molded article, a woven material, or a fiber.

[0080] In a seventeenth aspect, a method for forming a polyamide composition comprises providing a polyamide, wherein the polyamide comprises a plurality of amide groups in a main chain structure of the polyamide; and modifying a portion of the plurality of amide groups in the main chain structure with one or more alkyl substituents to form a polyamide composition, wherein the amide unit substitution amount of the polyamide is from about 0.1% to about 10% of the amide units in the main chain.

[0081] An eighteenth aspect may include the method of the seventeenth aspect, wherein the polyamide composition has the form of: Wherein, R includes an alkyl substituent on the amide group in the plurality of amide groups. A nineteenth aspect may include the method of aspect seventeen, wherein the polyamide composition has the formula: wherein n is between 200 and 100,000, m is 1-11, and any one of R1, R2 and R3 may include hydrogen or an alkyl substituent.

[0082] A twentieth aspect may include the method of any one of aspects seventeen to nineteen, wherein the carboxyl groups in the polyamide have less than 0.1% modification in the polyamide composition.

[0083] Aspect twenty-one may include the method of any one of aspects seventeen to twentieth, wherein modifying a portion of the multiple amide groups in the main chain structure with one or more alkyl substituents comprises: contacting the polyamide with a modifier; deprotonating a portion of the multiple amide groups; and alkylating a portion of the multiple amide groups to form a polyamide composition.

[0084] The twenty-second aspect may include the method of the twenty-first aspect, wherein modifying a portion of the plurality of amide groups in the backbone structure with one or more alkyl substituents further comprises: dissolving the polyamide in a solvent prior to contacting the polyamide with the modifying agent.

[0085] The twenty-third aspect may include the method of the twenty-first aspect or the twenty-second aspect, wherein the modifier comprises a base, formaldehyde, paraformaldehyde, iodomethane, methanol, ethanol, sodium hydride, or any combination thereof.

[0086] A twenty-fourth aspect may include the method of any of aspects seventeen to twenty-fifth, wherein modifying a portion of the plurality of amide groups occurs at a temperature of about 18°C ​​to about 265°C and for a duration of between about 0.1 to about 120 hours.

[0087] A twenty-fifth aspect may include the method of any one of aspects seventeen to twenty-fourth, further comprising: modifying a portion of the endcaps of the polyamide composition.

[0088] The twenty-sixth aspect may include the method of the twenty-fifth aspect, wherein modifying a portion of the endcap comprises modifying the endcap using an endcapping agent, wherein the endcapping agent comprises an alkanolamine, an alkylene polyamine, a cyclic lactam, or any combination thereof.

[0089] It should also be understood that this specification is not limited to the specific methods, compounds, materials, manufacturing techniques, uses and applications described herein, as these may vary. It should also be understood that the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of the present system and method. It should be noted that as used herein and in the appended claims (in this application or any derivative application thereof), the singular forms "a", "an" and "the" include plural references unless the context clearly states otherwise. Thus, for example, a reference to "an element" is a reference to one or more elements and includes equivalents thereof known to those skilled in the art. All conjunctions used should be understood in the broadest sense possible. Therefore, unless the context clearly states otherwise, the word "or" should be understood to have a logical "or" definition, rather than a logical "exclusive or" definition. The structures described herein should also be understood to refer to functional equivalents of such structures. Any language that may be interpreted as indicating approximation should be understood as an approximate meaning unless the context clearly states otherwise.

[0090] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this specification belongs. Preferred methods, techniques, devices, and materials are described, although any methods, techniques, devices, or materials similar or equivalent to those described herein may also be used in the practice or testing of the present systems and methods. Structures described herein are also understood to refer to functional equivalents of such structures. The present systems and methods will now be described in detail with reference to the embodiments shown in the accompanying drawings.

[0091] By reading this disclosure, other changes and modifications will be apparent to those skilled in the art. Such changes and modifications may involve equivalent features and other features known in the art, and may be used to replace or supplement the features described herein.

[0092] Although the claims in this application or any further application derived therefrom may be limited to specific combinations of features, it should be understood that the scope of the present disclosure also includes any novel feature or combination of any novel features or any generalization thereof disclosed explicitly or implicitly herein, regardless of whether such features relate to the same system or method as currently claimed in any claim, and regardless of whether the derivative solves any or all of the same technical problems as the present system and method.

[0093] Features described in the context of separate embodiments may also be provided in combination in a single embodiment. Conversely, various features described in the context of a single embodiment, for the sake of brevity, may also be provided separately or in any suitable subcombination. Applicants hereby give notice that new claims may be formulated to such features and / or combinations of such features during the prosecution of this application or any further application derived therefrom.

Claims

1. A polyamide comprising: A plurality of amide units forming a polymer chain; as well as Alkyl substituents on the amide groups, wherein the polyamide has amide units substituted in an amount of from about 0.1% to about 10% of the amide units in the polymer chain.

2. The polyamide of claim 1, wherein the polymer chain comprises endcaps, and wherein at least a portion of the endcaps comprise alkyl substituents.

3. The polyamide of claim 1, wherein the alkyl substituent is methyl, ethyl or butyl.

4. The polyamide of claim 1, wherein the polymer is biodegradable.

5. The polyamide according to claim 1, wherein the polymer is in the form of a sheet, a film, a filament, a tape, a molding, a woven material or a fiber.

6. The polyamide according to any one of claims 1 to 5, wherein the melting point of the polymer is between 220°C and about 400°C.

7. The polyamide of claim 1, wherein the polymer has a degradation temperature of at least about 200°C.

8. The polyamide of claim 1, wherein the temperature difference between the melting temperature and the degradation temperature of the polymer is at least about 20°C.

9. The polyamide of claim 1, wherein the polyamide is nylon 2, nylon 3, nylon 4, nylon 6, or protein.

10. A poly-2-pyrrolidone polymer comprising the formula: in, R comprises an alkyl substituent on the amide group, and the amount of the amide group substituent of the poly-2-pyrrolidone is from about 0.1% to about 10% of the amide group in the poly-2-pyrrolidone.

11. The polymer of claim 10, wherein R is methyl, ethyl or butyl.

12. The polymer of claim 10, wherein the polymer has a melting point between 220°C and about 400°C.

13. The polymer of claim 10, wherein the polymer has a degradation temperature of at least about 200°C.

14. The polymer of claim 10, wherein the temperature difference between the melting temperature and the degradation temperature of the polymer is at least about 20°C.

15. The polymer of claim 10, wherein the polymer is biodegradable.

16. The polymer of claim 10, wherein the polymer is in the form of a sheet, a film, a filament, a tape, a molding, a woven material, or a fiber.

17. A method of forming a polyamide composition, the method comprising: Providing a polyamide, wherein the polyamide comprises a plurality of amide groups in the backbone structure of the polyamide; A portion of the plurality of amide groups in the backbone structure is modified with one or more alkyl substituents to form a polyamide composition wherein the polyamide has amide units substituted in an amount of about 0.1% to about 10% of the amide units in the backbone.

18. The method of claim 17, wherein the polyamide composition has the following form: in, R includes alkyl substituents on the amide groups in the plurality of amide groups.

19. The method of claim 17, wherein the polyamide composition has the formula: in, n is between 200 and 100,000, m is 1-11, and any one of R1, R2 and R3 may include hydrogen or an alkyl substituent.

20. The method of claim 17, wherein the carboxyl groups in the polyamide have less than 0.1% modification in the polyamide composition.

21. The method of claim 17, wherein modifying a portion of the plurality of amide groups in the backbone structure with one or more alkyl substituents comprises: contacting the polyamide with a modifier; deprotonating a portion of the multiple amide groups; as well as A portion of the plurality of amide groups is alkylated to form a polyamide composition.

22. The method of claim 21, wherein modifying a portion of the plurality of amide groups in the backbone structure with one or more alkyl substituents further comprises: Prior to contacting the polyamide with the modifying agent, the polyamide is dissolved in a solvent.

23. The method of claim 21, wherein the modifier comprises a base, formaldehyde, paraformaldehyde, methyl iodide, methanol, ethanol, sodium hydride, or any combination thereof.

24. The method of claim 17, wherein modifying a portion of the plurality of amide groups occurs at a temperature of 18°C ​​to about 265°C and for a duration of between about 0.1 to about 120 hours.

25. The method of claim 17, further comprising: A portion of the endcaps of the polyamide composition are modified.

26. The method of claim 25, wherein modifying a portion of the endcaps comprises modifying the endcaps using an endcapping agent, wherein the endcapping agent comprises an alkanolamine, an alkylene polyamine, a cyclic lactam, or any combination thereof.