Resin composition, resin molded article, and method for producing resin composition

By using a resin composition of thermoplastic resin, isotropic carbon fiber and silane coupling agent in a lithium-ion secondary battery, the melt deformation and flow of high-energy density lithium-ion secondary battery under high-temperature flame is solved, and the problem of melt deformation and flow of high-energy density lithium-ion secondary battery is achieved. Good moldability and safety are achieved while avoiding the production of harmful gases.

CN118946638APending Publication Date: 2024-11-12MITSUBISHI MATERIALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030287.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing resin materials are difficult to take into account both moldability and fire resistance under the exposure of high-temperature flame and high-pressure gases of high-energy density lithium-ion secondary batteries, especially under flame conditions above 1000°C, and traditional Halogen flame retardants will produce harmful gases when burned.

Method used

The resin composition consisting of thermoplastic resin, isotropic asphalt carbon fiber and silane coupling agent is used to suppress melt deformation caused by high temperature flame through specific mass ratios and process treatment, and the silane coupling is uniformly dispersed through dry mixing process. to improve the refractory resistance of the resin.

Benefits of technology

The melt deformation suppression during flame contact at about 1000°C is achieved, and good moldability is maintained, while the generation of harmful gases is avoided, and the safety and protection effect of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946638A_ABST
    Figure CN118946638A_ABST
Patent Text Reader

Abstract

The resin composition is characterized in that the thermoplastic resin is contained in the range of 59 parts by mass to 88 parts by mass (inclusive), the carbon fibers are contained in the range of 1 part by mass to 18 parts by mass (inclusive), and the silane coupling agent is contained in the range of 0.3 part by mass to 7 parts by mass (inclusive) relative to 100 parts by mass of the whole resin composition. The carbon fiber is an isotropic pitch-based carbon fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a fire-resistant resin composition, a resin molded body using the resin composition, and a method for producing the resin composition.

[0002] This application claims priority based on patent application No. 2022-060227 filed in Japan on March 31, 2022, and the contents of which are incorporated herein by reference. Background Art

[0003] In recent years, in order to reduce the weight of various devices, resin materials are often used to form the outer casing of components that were previously formed of metal. For example, the outer casing of lithium-ion secondary batteries (hereinafter, sometimes referred to as "batteries") is also mostly formed of resin materials for the purpose of reducing weight. Therefore, the resin material is required to have excellent moldability, such as molding along the outer shape of the object to be formed.

[0004] On the other hand, batteries using resin materials are developing towards high energy density (energy density of 300Wh / kg or more) as they become smaller, and this may cause high temperatures due to heat generation depending on the way they are used. Therefore, the safety of batteries and battery packs has become more important. On the other hand, if safety (fire resistance) is improved, there are cases where moldability deteriorates, so it is required to strike a balance between safety and moldability.

[0005] For example, if a lithium-ion secondary battery is overcharged or over-discharged, or is subjected to an unexpected impact that causes an internal short circuit or an external short circuit, thermal runaway may occur. A lithium-ion secondary battery that has thermal runaway generates gas, which increases the internal pressure of the battery. If this happens, the increase in internal pressure may cause the outer can to rupture, etc., so these batteries are provided with exhaust holes or safety valves for exhaust.

[0006] However, there are cases where high-temperature flames or high-temperature / high-pressure gases are ejected from exhaust holes or safety valves provided in lithium-ion secondary batteries that have thermal runaway and are used for exhaust, and the highest temperature thereof exceeds 999°C, so that deformation or melting of the resin material may occur. Furthermore, in automobile fires, etc., lithium-ion secondary batteries are exposed to external flames, so high-temperature and high-pressure flames are ejected from the lithium-ion secondary batteries due to heat from the outside, which may cause secondary damage to occupants or peripheral components.

[0007] As a resin material capable of improving moldability while suppressing deformation or melting due to such flame or high-temperature gas jet, for example, Patent Document 1 discloses a resin molding material in which warpage of a molded product is improved by adding specific fibers.

[0008] Furthermore, Patent Document 2 discloses a polyphenylene sulfide resin composition containing carbon fibers pretreated with a silane coupling agent.

[0009] Patent Document 1: Japanese Patent Application Publication No. 2000-119405 (A)

[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 06-49362 (A)

[0011] However, with the high energy density of batteries in recent years, the output power of the flame generated during thermal runaway has increased significantly. When the lithium-ion secondary battery that has been rapidly popularized in recent years catches fire, its flame is around 1000°C. Regarding the evaluation of the melting deformation caused by the flame, the product safety standard (UL standard) formulated by Underwriters Laboratories Inc. is also only implemented under a flame with an output power of 500W. Under the condition that the flame temperature exceeds 1000°C, the resin composition disclosed in Patent Document 1 or Patent Document 2 may not be able to take into account both moldability and melting and fluidization.

[0012] On the other hand, since a resin composition that has been blended with a halogen-based flame retardant to improve flame retardancy may generate harmful substances such as halogen-containing gas during combustion, a flame-retardant resin composition that does not contain a halogen-based material is desired. Summary of the invention

[0013] The present invention has been completed in view of such background, and its object is to provide a resin composition which can suppress melting, deformation and fluidization caused by the injection of high-temperature gas or flame and has good moldability, a resin molded body using the resin composition, and a method for producing the resin composition.

[0014] The inventors of the present invention have discovered that by using a resin composition composed of a material including a thermoplastic resin, carbon fiber and a silane coupling agent, setting the content ratio of these components within a specific range, and selectively using isotropic pitch-based carbon fiber as carbon fiber, the amount of melt deformation when in contact with a flame above 1000°C can be suppressed, and the moldability is also good.

[0015] In order to solve the above problems, the invention proposes the following method.

[0016] That is, the resin composition of the present invention is characterized in that, relative to 100 parts by mass of the entire resin composition, it contains a thermoplastic resin in a range of 59 parts by mass to 88 parts by mass, contains carbon fibers in a range of 1 part by mass to 18 parts by mass, and contains a silane coupling agent in a range of 0.3 parts by mass to 7 parts by mass, and the carbon fibers are isotropic pitch-based carbon fibers.

[0017] According to the present invention, a resin composition can be obtained, which contains a thermoplastic resin in a range of 59 parts by mass to 88 parts by mass, contains carbon fibers in a range of 1 part by mass to 18 parts by mass, and contains a silane coupling agent in a range of 0.3 parts by mass to 7 parts by mass when the entire resin composition is set to 100 parts by mass. By using isotropic pitch-based carbon fibers as carbon fibers, resistance to melt deformation is improved, for example, even if it comes into contact with a flame of about 1000°C, melt deformation or fluidization can be suppressed.

[0018] Furthermore, in the present invention, the thermoplastic resin may include at least one of polyphenylene sulfide, polyamide, polybutylene terephthalate, modified polyphenylene ether, and polycarbonate.

[0019] Furthermore, in the present invention, the silane coupling agent may be at least one of an organic silicon compound and a siloxane compound.

[0020] Furthermore, in the present invention, the organic silicon compound may be at least one of an amine-based silane coupling agent and an epoxy-based silane coupling agent.

[0021] Furthermore, in the present invention, glass fiber may be further contained in an amount within a range of 3 parts by mass or more and 35 parts by mass or less relative to 100 parts by mass of the thermoplastic resin.

[0022] The resin molded article of the present invention is a resin molded article obtained by molding the resin composition described in the above items.

[0023] Furthermore, in the present invention, the resin molded body may be attached to the outer periphery of one or more lithium ion secondary battery cells having a safety valve or a vent hole so as to cover at least the safety valve or the vent hole.

[0024] The method for producing a resin composition of the present invention is characterized in that the method for producing a resin composition described in the above items is the method for producing a resin composition described in any one of claims 1 to 4, comprising: a silane coupling agent adding step, wherein the whole amount of the silane coupling agent is added dropwise to a part of the thermoplastic resin separated in a range of 4 parts by mass or more and 77 parts by mass or less from 100 parts by mass of the thermoplastic resin to obtain a part of the thermoplastic resin to which the silane coupling agent is added; a first mixing step, wherein the remaining 23 parts by mass or more and 96 parts by mass of the thermoplastic resin are added to the part of the thermoplastic resin to which the silane coupling agent is added and mixed to obtain an intermediate mixture in which the silane coupling agent and the whole amount of the thermoplastic resin are mixed; and a second mixing step, wherein the whole amount of the carbon fiber is added to the intermediate mixture and further mixed to obtain the resin composition.

[0025] As described above, according to the present invention, it is possible to provide a resin composition capable of suppressing melting, deformation, and fluidization caused by injection of high-temperature gas or flame, a resin molded article using the resin composition, and a method for producing the resin composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a perspective view of a lithium ion secondary battery cell to which a resin molded body according to one embodiment of the present invention is to be attached.

[0027] Figure 2 It is a perspective view showing a resin molded body and a lithium ion secondary battery cell to which the resin molded body is to be attached according to one embodiment of the present invention.

[0028] Figure 3 It is equipped with Figure 2 A perspective view of a lithium-ion secondary battery cell of a resin molded body.

[0029] Figure 4 yes Figure 3 AA line section view. DETAILED DESCRIPTION

[0030] Hereinafter, with appropriate reference to the accompanying drawings, a resin composition of an embodiment of the present invention and a resin molded product using the resin composition are described in detail. With regard to the accompanying drawings used in the following description, in order to easily understand the features of the present invention, sometimes the part that becomes a feature is enlarged for convenience, and the dimensional ratio of each component element may not be consistent with the actual. The material, size, etc. illustrated in the following description are an example, and the present invention is not limited thereto, and can be implemented by appropriately changing within the scope of exerting its effect.

[0031] (Resin composition)

[0032] The resin composition according to one embodiment of the present invention is composed of a mixture of a thermoplastic resin, carbon fibers, and a silane coupling agent, and may further contain glass fibers as necessary.

[0033] The resin composition of the present embodiment contains a thermoplastic resin in an amount of 59 parts by mass to 88 parts by mass, a carbon fiber in an amount of 1 part by mass to 18 parts by mass, and a silane coupling agent in an amount of 0.3 parts by mass to 7 parts by mass, relative to 100 parts by mass of the entire resin composition.

[0034] The resin composition may contain 60 to 82 parts by mass of the thermoplastic resin, or 61 to 75 parts by mass of the thermoplastic resin.

[0035] The resin composition may contain 2 to 16 parts by mass of carbon fibers, or 4 to 13 parts by mass of carbon fibers.

[0036] The resin composition may contain 0.4 to 6 parts by mass of a silane coupling agent, or may contain 0.5 to 5 parts by mass of a silane coupling agent.

[0037] Furthermore, glass fiber may be further contained in an amount within a range of 3 parts by mass or more and 35 parts by mass or less relative to 100 parts by mass of the thermoplastic resin.

[0038] Examples of the thermoplastic resin used in the resin composition include polyphenylene sulfide (PPS), polyamide 6 (PA6), polybutylene terephthalate (PBT), modified polyphenylene ether (mPPE), polycarbonate (PC) and polypropylene (PP), or a mixture of two or more thereof.

[0039] Among them, PPS has a high melting point (278°C) and glass transition temperature (92-126°C), so it is particularly preferred as a thermoplastic resin. As a thermoplastic resin suitable for the resin composition, PPS can be either an oxidative cross-linked PPS that is heat-treated in the presence of oxygen to increase the melt viscosity, or a linear PPS that is added with lithium chloride, an organic acid salt, water, etc. in the polymerization series to maintain a linear state and increase the molecular weight. In addition, the oxidative cross-linked PPS and the linear PPS can also be mixed and used.

[0040] As the carbon fiber, isotropic pitch-based carbon fiber is used, which is a carbon fiber that is optically isotropic among pitch-based carbon fibers using asphalt. By using isotropic pitch-based carbon fiber, the deformation resistance of the resin composition can be improved.

[0041] As specific examples of the shape of the isotropic pitch-based carbon fibers used in the resin composition, the fiber diameter of a single fiber is 1 to 20 μm, the average fiber length is 0.01 to 10 mm, and the aspect ratio is about 1.5 to 1,300.

[0042] The silane coupling agent contained in the resin composition can suppress the melting and falling of the resin composition during combustion.

[0043] The silane coupling agent included in the resin composition may be, for example, at least one of an organic silicon compound and a siloxane compound. Furthermore, the silane coupling agent may be at least one of an amine silane coupling agent and an epoxy silane coupling agent. When comparing an amine silane coupling agent and an epoxy silane coupling agent, an amine silane coupling agent having an amino terminal is more preferred.

[0044] Examples of the amine-based silane coupling agent include 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, and 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine.

[0045] Examples of the epoxy silane coupling agent include 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.

[0046] Furthermore, as the silane coupling agent contained in the resin composition, various silane coupling agents such as acrylic (e.g., 3-acryloxypropyltrimethoxysilane), vinyl, methacrylic, styrene, ureide, isocyanate, isocyanurate, and mercapto silane coupling agents can be used.

[0047] Furthermore, as the silane coupling agent, in addition to the above-mentioned amine silane coupling agents, epoxy silane coupling agents, acrylic, vinyl, methacrylic, styrene, ureide, isocyanate, isocyanurate, mercapto and other liquid silane coupling agents, solid silane coupling agents can also be used.

[0048] Examples of the solid silane coupling agent include X-12-1273ES (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0049] When comparing a liquid silane coupling agent with a solid silane coupling agent, the liquid silane coupling agent is superior in that it has a functional group and can be expected to have high reactivity (in principle, a high effect can be expected), whereas the solid silane coupling agent is superior in that it can be easily handled.

[0050] When the resin composition contains glass fibers, as the glass fibers to be used, any of long filaments (long fibers: glass fibers) and short filaments (short fibers: glass wool) can be used.

[0051] The resin composition of the present embodiment may further include a fluororesin. As the fluororesin, for example, polytetrafluoroethylene (PTFE) may be cited. PTFE is preferably used in a powdered state. For example, a PTFE having an average particle size of 10 to 30 μm and a specific surface area of ​​0.5 to 5 m based on the BET method may be used. 2 / g of PTFE powder. Regarding the fluororesin, the fluororesin may be contained in a range of 1 part by mass or more and 50 parts by mass or less relative to 100 parts by mass of the thermoplastic resin. Examples of the fluororesin include PTFE, PFA (perfluoroalkoxyalkane), and FEP (perfluoroethylene propylene copolymer).

[0052] The resin composition may contain carbon black as a colorant, polyolefin wax or stearyl alcohol as a mold release agent, and hydrotalcite or zinc carbonate as a mold antiseptic.

[0053] The resin composition of the present embodiment contains a thermoplastic resin in an amount of 59 parts by mass to 88 parts by mass, carbon fibers in an amount of 1 part by mass to 18 parts by mass, and a silane coupling agent in an amount of 0.3 parts by mass to 7 parts by mass, relative to 100 parts by mass of the entire resin composition. By using isotropic pitch-based carbon fibers as the carbon fibers, for example, even when in contact with a flame of about 1000° C., melt deformation or fluidization can be suppressed.

[0054] (Method for producing resin composition)

[0055] Next, an example of a method for producing the resin composition according to the present embodiment will be described.

[0056] When producing the resin composition of the present embodiment, first, the above-mentioned thermoplastic resin is prepared, and then, when the entire thermoplastic resin is 100 parts by mass, the thermoplastic resin is fractionated in an amount corresponding to 4 parts by mass or more and 77 parts by mass or less.

[0057] Next, the entire amount of the silane coupling agent constituting the resin composition is gradually added dropwise to the separated part of the thermoplastic resin (silane coupling agent adding step). Thus, a part of the thermoplastic resin to which the silane coupling agent is added (premix) can be obtained.

[0058] Next, 23 parts by mass or more and 96 parts by mass or less of the remaining thermoplastic resin after the fractionation are added to a portion of the thermoplastic resin to which the silane coupling agent is added, and dry-mixed to obtain an intermediate mixture of the silane coupling agent and the entire amount of the thermoplastic resin (first mixing step).

[0059] Furthermore, for the intermediate mixture obtained in the first mixing step, other materials other than the isotropic pitch-based carbon fiber constituting the resin composition are added and further dry-mixed (second mixing step). Then, a twin-shaft extruder is used, and the isotropic pitch-based carbon fiber constituting the entire amount of the resin composition is added again through a feeder, while, for example, the kneading processing temperature is managed to be above 270°C and below 300°C, the rotation speed of the spiral stirrer is managed to be above 100rpm and below 300rpm, and the kneading processing time is set to be above 30 minutes and below 60 minutes for granulation, thereby being able to form a granular resin composition.

[0060] The resin composition obtained in this way can be molded by a known molding method such as extrusion molding using an extruder, press molding using a press machine, or injection molding using an injection molding machine to produce a resin molded body.

[0061] As described above, in the method for producing the resin composition, the key is dry mixing. That is, the following steps are performed in sequence: first, only a portion of the thermoplastic resin is separated, a silane coupling agent is added dropwise thereto, and the remaining thermoplastic resin is added and mixed, thereby not only the silane coupling agent can be uniformly dispersed in the thermoplastic resin, but also the loss can be reduced and the function of suppressing flow and deformation caused by flame can be improved.

[0062] (Resin molded body)

[0063] Figure 1 It is a perspective view of a lithium ion secondary battery cell to which a resin molded body according to one embodiment of the present invention is to be attached.

[0064] The lithium-ion secondary battery cell 1 is a rectangular battery cell, and a positive electrode terminal 3 and a negative electrode terminal 4 are provided on the upper surface of an outer can 2 as a battery container, and a safety valve 5 is provided between them.

[0065] The safety valve 5 is activated when the internal pressure of the lithium ion secondary battery cell 1 increases due to thermal runaway, and prevents the outer can 2 from rupturing due to the ejection of high-temperature and high-pressure gas.

[0066] When thermal runaway occurs in the lithium ion secondary battery cell 1 , there is a possibility of ignition due to overheating. Once the high-temperature and high-pressure gas ejected from the safety valve 5 spreads rapidly over a wide area, it is difficult to prevent the spread of fire and burnout.

[0067] Therefore, in this embodiment, if Figure 2 , Figure 3 and as Figure 3 AA line section view Figure 4As shown, a flexible sheet-shaped resin molded body 6 is attached to the outer periphery of the lithium ion secondary battery cell 1 via an insulating sheet 7 so as to cover at least the safety valve 5. If the resin molded body 6 is made of an insulating material or does not require insulation, the insulating sheet 7 may not be inserted.

[0068] In this embodiment, the insulating sheet 7 and the sheet-shaped resin molded body 6 are both rectangular and have substantially the same size, so as to cover the upper surface including the safety valve 5 of the rectangular lithium-ion secondary battery cell 1 and cover the front and back surfaces ( Figure 4 It is attached in the manner of the upper part of the left and right surfaces).

[0069] Leads (not shown) connected to the positive electrode terminal 3 and the negative electrode terminal 4 of the lithium ion secondary battery cell 1 are led out using the side surface not covered by the insulating sheet 7 and the resin molded body 6 .

[0070] The lithium ion secondary battery cell 1 with the insulating sheet 7 and the sheet-shaped resin molded body 6 is housed in an outer casing (not shown). In the outer casing, the resin molded body 6 covering the upper part of the front and back of the lithium ion secondary battery cell 1 is pressed by the inner wall surface of the outer casing, so that the resin molded body 6 is retained.

[0071] Furthermore, regarding the thickness of the portion of the resin molded body 6 covering the safety valve 5, in this embodiment, the resin molded body 6 is in the form of a sheet having a uniform thickness, and the thickness of the sheet-shaped resin molded body 6 only needs to be greater than 0.5 mm and less than 10.0 mm, preferably greater than 0.7 mm and less than 5 mm, and more preferably greater than 1.0 mm and less than 2 mm.

[0072] If the thickness is less than 0.5 mm, a through hole is formed in the resin molded body 6 due to the high temperature / high pressure gas ejected from the safety valve 5, and the high temperature / high pressure gas is ejected from the through hole, which may cause the components outside the lithium ion secondary battery unit 1 covered by the insulating sheet 7 and the sheet-like resin molded body 6 to spread and burn. In addition, the through hole becomes an air (oxygen) supply port, which may cause the lithium ion secondary battery unit 1 itself covered by the insulating sheet 7 and the sheet-like resin molded body 6 to spread and burn.

[0073] If the thickness of the sheet-shaped resin molded body 6 is greater than 10.0 mm, high temperature / high pressure gas can be blocked, i.e., through holes will not be formed, but the resin molded body 6 tends to be larger, and the molding process becomes complicated. In addition, it is difficult to accommodate the lithium ion secondary battery cell 1 in the existing outer casing for accommodation.

[0074] The surface hardness of the resin molded body 6 is preferably above 50, and the value of the surface hardness is a value obtained by measuring the resin molded body 6 using a sheet having a thickness of 2 mm and using a D-type hardness meter according to JIS K7215. If the surface hardness is less than 50, the resin molded body 6 may be damaged or a through hole may be formed due to the high-temperature / high-pressure gas ejected from the safety valve 5 (especially the influence of the pressure (ejection force)). Regarding the upper limit of the surface hardness, the upper limit is 90 as the appropriate value in the above standard, but it can be greater than 90 as long as it is within the range that can be molded. In addition, in a general measuring device, it can be measured to about 100, and the surface hardness of the resin molded body 6 displayed in the measuring device can be below 100.

[0075] As described above, the resin molded body 6 of the present embodiment uses the aforementioned resin composition and is formed in a manner that covers the safety valve 5 of the lithium-ion secondary battery cell 1. Therefore, even if thermal runaway occurs in the lithium-ion secondary battery, no through holes will be generated on the resin molded body 6 due to the high-temperature / high-pressure gas ejected from the safety valve 5, thereby being able to suppress the spread of fire and burning caused by the ejection of high-temperature / high-pressure gas.

[0076] Example

[0077] (Evaluation of deformation resistance)

[0078] Next, for deformation resistance (fire resistance) evaluation, samples (resin compositions) of Example 1 of the present invention and Comparative Examples 1 to 3 were prepared in which the types of carbon fibers contained in the resin compositions were changed.

[0079] The common composition ratios of the samples of Inventive Example 1 and Comparative Examples 1 to 3 are as follows.

[0080] Thermoplastic resin (polyphenylene sulfide (PPS) resin): 70.4% by mass

[0081] Silane coupling agent (3-aminopropyltriethoxysilane): 0.70 mass%

[0082] Carbon fiber: (see next item) 7.00 mass%

[0083] Glass fiber: 20.00 mass%

[0084] Release agent: (PE520: manufactured by Clariant Chemicals Co., Ltd., polyethylene wax) 0.40 mass%

[0085] · Antiseptic: (zinc carbonate (ZnCO3)) 0.70 mass%

[0086] Colorant: (BP880: manufactured by Cabot Japan KK., carbon black) 0.80 mass%

[0087] The above total is 100% by mass

[0088] [Example 1 of the present invention] As carbon fiber, the following carbon fiber was used: OGC360 (DONACARBO: manufactured by Osaka Gas Chemicals Co., Ltd.), isotropic pitch-based carbon fiber, average fiber length 360 μm, average fiber diameter 11 μm.

[0089] [Comparative Example 1] As carbon fibers, the following carbon fibers were used: MCC6000 (DIALEAD: manufactured by Mitsubishi Chemical Corporation), anisotropic pitch-based carbon fibers with an average fiber length of 6000 μm and an average fiber diameter of 11 μm.

[0090] [Comparative Example 2] As carbon fibers, the following carbon fibers were used: MCC200 (DIALEAD: manufactured by Mitsubishi Chemical Corporation), anisotropic pitch-based carbon fibers with an average fiber length of 179 μm and an average fiber diameter of 11 μm.

[0091] [Comparative Example 3] As carbon fibers, the following carbon fibers were used: MCC50 (DIALEAD: manufactured by Mitsubishi Chemical Corporation), anisotropic pitch-based carbon fibers with an average fiber length of 58 μm and an average fiber diameter of 11 μm.

[0092] Regarding the test method for deformation resistance, for each resin composition of Example 1 of the present invention and Comparative Examples 1 to 3, a burner with an output power of 5580W was fixed vertically downward, and a resin composition (each sample) of 100mm×120mm×2mmt was prepared, and each sample was arranged horizontally with the ground at a position 170mm away from the burner of the burner. Then, the burner was ignited and flame was applied to each sample for evaluation.

[0093] The distance between the sample and the burner: 170mm

[0094] Local exhaust through ventilation

[0095] Firepower: 5580W

[0096] Temperature: 20℃

[0097] Humidity: 75%RH

[0098] Weather: Sunny

[0099] The test is considered to be completed when part of the sample melts and falls to the ground.

[0100] This test method was carried out twice for each sample.

[0101] Table 1 shows the time (seconds) required for each sample to deform by 10 mm.

[0102] [Table 1]

[0103]

[0104] According to the evaluation of deformation resistance shown in FIG. 5 and Table 1, it was confirmed that by using isotropic pitch-based carbon fibers as the carbon fibers contained in the resin composition, deformation caused by heat can be significantly delayed compared to the conventional example using anisotropic pitch-based carbon fibers. Therefore, according to the present embodiment, a resin composition that can suppress melting, deformation, and fluidization caused by the injection of high-temperature gas or flame can be realized.

[0105] In addition, in the above-mentioned deformation resistance evaluation, each sample contains a mold preservative, a release agent and a colorant, but the resin composition constituting the resin molded body of the present invention does not contain these preservatives, release agents, and colorants as essential components. Even if these preservatives, release agents, and colorants are not contained, a resin molded body with excellent deformation resistance can be obtained.

[0106] The contents of the antiseptic, release agent, and colorant in the above-mentioned deformation resistance evaluation are examples, and the contents of the antiseptic, release agent, and colorant can be increased or decreased to any amount as required, and the contents are not limited.

[0107] Industrial Applicability

[0108] A resin composition capable of suppressing melting, deformation, and fluidization caused by injection of high-temperature gas or flame, a resin molded article using the resin composition, and a method for producing the resin composition can be provided.

[0109] Explanation of symbols

[0110] 1 Lithium-ion secondary battery cell

[0111] 2 Outer cans

[0112] 3 Positive terminal

[0113] 4 Negative terminal

[0114] 5 Safety valve

[0115] 6 Resin molding

[0116] 7 Insulation sheet

Claims

1. A resin composition, characterized in that The present invention relates to a resin composition having an amount of at least 59 parts by mass but no greater than 88 parts by mass, a carbon fiber having an amount of at least 1 part by mass but no greater than 18 parts by mass, and a silane coupling agent having an amount of at least 0.3 parts by mass but no greater than 7 parts by mass, relative to 100 parts by mass of the entire resin composition. The carbon fiber is an isotropic pitch-based carbon fiber.

2. The resin composition according to claim 1, characterized in that The thermoplastic resin includes at least one of polyphenylene sulfide, polyamide, polybutylene terephthalate, modified polyphenylene ether and polycarbonate.

3. The resin composition according to claim 1 or 2, characterized in that The silane coupling agent is at least one of an organic silicon compound and a siloxane compound.

4. The resin composition according to claim 3, characterized in that The organic silicon compound is at least one of an amine-based silane coupling agent and an epoxy-based silane coupling agent.

5. The resin composition according to any one of claims 1 to 4, characterized in that The thermoplastic resin further contains glass fibers in an amount within a range of 3 parts by mass or more and 35 parts by mass or less based on 100 parts by mass of the thermoplastic resin.

6. A resin molded body, characterized in that: The resin molded body is obtained by molding the resin composition according to any one of claims 1 to 5.

7. The resin molded article according to claim 6, wherein: The resin molded body is attached to the outer periphery of one or more lithium ion secondary battery cells having a safety valve or a vent hole so as to cover at least the safety valve or the vent hole.

8. A method for producing a resin composition, characterized in that: The manufacturing method is a manufacturing method of the resin composition according to any one of claims 1 to 4, comprising: a silane coupling agent adding step of dripping the entire amount of the silane coupling agent to a portion of the thermoplastic resin separated in a range of 4 parts by mass or more and 77 parts by mass or less from 100 parts by mass of the thermoplastic resin to obtain a portion of the thermoplastic resin to which the silane coupling agent is added; A first mixing step of adding 23 parts by mass or more and 96 parts by mass or less of the remaining thermoplastic resin to a portion of the thermoplastic resin to which the silane coupling agent is added and mixing the mixture to obtain an intermediate mixture of the silane coupling agent and the entire amount of the thermoplastic resin; and In the second mixing step, the entire amount of the carbon fibers is added to the intermediate mixture and further mixed to obtain the resin composition.