Energy-ray-crosslinkable adhesive composition, crosslinked adhesive, adhesive sheet, and methods for producing energy-ray-crosslinkable adhesive composition, crosslinked adhesive, and adhesive sheet

Through the combination of energy-ray crosslinkable acrylic polymer and acrylic polymer without radical reactiveness, the problems of the increase in viscosity and the reduction in coating properties of existing hot melt adhesives during heating are solved, and the application is achieved. Adhesive effect with long periods and excellent coating properties.

CN118946646APending Publication Date: 2024-11-12LINTEC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202280094161.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-31
Publication Date
2024-11-12

Smart Images

  • Figure BDA0005058887200000231
    Figure BDA0005058887200000231
  • Figure HDA0005058887210000011
    Figure HDA0005058887210000011
  • Figure HDA0005058887210000012
    Figure HDA0005058887210000012
Patent Text Reader

Abstract

The present invention relates to an energy-ray-crosslinkable adhesive composition, an adhesive sheet using the energy-ray-crosslinkable adhesive composition, a crosslinked adhesive obtained by energy-ray crosslinking of the energy-ray-crosslinkable adhesive composition, a method for producing the crosslinked adhesive, an adhesive sheet using the crosslinked adhesive, and a method for producing the adhesive sheet. The energy-ray-crosslinkable adhesive composition contains (A) an energy-ray-crosslinkable acrylic polymer and (B) an acrylic polymer other than the component (A), said acrylic polymer substantially not containing a radically reactive unsaturated double bond and having a weight-average molecular weight (Mw) of 280000 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an energy-ray crosslinkable adhesive composition, a crosslinked adhesive, and an adhesive sheet, and methods for producing the same. Background Art

[0002] PSA sheets are used in a wide range of industrial fields, such as labels for displaying various information, fixing or temporarily fixing parts in the fields of OA equipment, home appliances, automobiles, and construction, and masking.

[0003] Hot melt adhesives are widely used as adhesives for adhesive sheets. Hot melt adhesives can be applied to substrates or the like by heating and melting without using a solvent, and therefore have the advantage of being able to reduce environmental burden when producing adhesive sheets.

[0004] As a hot melt adhesive, for example, a synthetic rubber hot melt adhesive is widely known. In recent years, demands for reducing environmental burdens have increased, and acrylic hot melt adhesives and the like have also been developed.

[0005] For example, Patent Document 1 discloses a radiation-curable hot melt adhesive comprising 100 parts by weight of an acrylic polymer having a radiation-reactive group, 3 to 20 parts by weight of an acrylic monomer, and 0.002 to 0.2 parts by weight of a polymerization inhibitor having a specific structure.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2015-214601 Summary of the invention

[0009] Problems to be solved by the invention

[0010] In the radiation-curing hot melt adhesive of Patent Document 1, a cross-linked structure is formed between acrylic polymers having radiation-reactive groups, and an acrylic monomer is contained as an essential component in order to improve the cohesive force of the radiation-curing hot melt adhesive after radiation irradiation. In addition, it is disclosed that a multifunctional acrylic monomer can be suitably used as the acrylic monomer.

[0011] However, when the hot melt adhesive contains monomers, oligomers, polymers, and other polymers having unsaturated double bonds with free radical reactivity, a polymerization reaction occurs by heating, and the viscosity of the hot melt adhesive increases over time, causing a decrease in coating properties and the formation of gel. As a result, the time during which the hot melt adhesive can be used, the so-called "pot life", is shortened. In addition, the hot melt adhesive is used as an adhesive layer of an adhesive sheet by a method of applying it to a substrate by heating and melting, and therefore, good coating properties are also required when applying it.

[0012] The present invention has been completed in view of the above-mentioned problems, and its purpose is to provide an energy-ray cross-linkable adhesive composition that can form an adhesive with a long applicability and excellent coating properties, an adhesive sheet using the energy-ray cross-linkable adhesive composition and a method for manufacturing the same, a cross-linked adhesive formed by energy-ray cross-linking the energy-ray cross-linkable adhesive composition and a method for manufacturing the same, and an adhesive sheet using the cross-linked adhesive and a method for manufacturing the same.

[0013] Solutions to the problem

[0014] The present inventors have found that the above-mentioned problems can be solved by using an acrylic resin and a specific acrylic polymer having energy-ray crosslinkability, thereby completing the present invention.

[0015] That is, the present invention relates to the following [1] to

[13] .

[0016] [1] An energy-ray crosslinkable adhesive composition comprising:

[0017] (A) an acrylic polymer having energy-ray crosslinkability, and

[0018] (B) An acrylic polymer other than the component (A) which contains substantially no radically reactive unsaturated double bonds and has a weight average molecular weight (Mw) of 280,000 or less.

[0019] [2] The energy-ray crosslinkable adhesive composition according to [1] above, wherein

[0020] The component (A) is an acrylic polymer having a benzophenone structure in a side chain.

[0021] [3] The energy-ray-crosslinkable pressure-sensitive adhesive composition according to [1] or [2] above, wherein

[0022] The content of the component (B) is 50 parts by mass or less relative to 100 parts by mass of the component (A).

[0023] [4] The energy-ray crosslinkable pressure-sensitive adhesive composition according to any one of [1] to [3] above, comprising (C) a hydrogen abstraction-type photoinitiator.

[0024] [5] The energy-ray cross-linkable pressure-sensitive adhesive composition according to any one of [1] to [4] above, further comprising (D) a tackifier.

[0025] [6] The energy-ray crosslinkable adhesive composition according to any one of [1] to [5] above, wherein

[0026] The content of the component (A) is 50 to 98% by mass in 100% by mass of the total amount of the adhesive composition.

[0027] [7] A pressure-sensitive adhesive sheet comprising an energy-crosslinkable pressure-sensitive adhesive composition layer formed from the energy-crosslinkable pressure-sensitive adhesive composition according to any one of [1] to [6] above on a substrate or a release liner.

[0028] [8] A method for producing a pressure-sensitive adhesive sheet having an energy-ray crosslinkable pressure-sensitive adhesive composition layer, the method comprising the following steps 11 and 12:

[0029] Step 11, a step of obtaining an energy-ray-crosslinkable adhesive composition by melt-kneading (A) an acrylic polymer having energy-ray crosslinkability and a component (B), wherein the component (B) is an acrylic polymer other than the component (A) which substantially does not contain a free radical-reactive unsaturated double bond and has a weight average molecular weight (Mw) of 280,000 or less;

[0030] Step 12 is a step of forming the energy-ray cross-linkable adhesive composition layer by melt-coating the energy-ray cross-linkable adhesive composition on a substrate or a release liner.

[0031] [9] A cross-linked adhesive obtained by irradiating the energy-ray-crosslinkable adhesive composition according to any one of [1] to [6] above with energy rays.

[0032]

[10] A method for producing a cross-linked adhesive, which is a method for producing the cross-linked adhesive described in [9] above, the method comprising:

[0033] A step of irradiating the energy-ray crosslinkable pressure-sensitive adhesive composition with energy rays.

[0034]

[11] A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer formed from the cross-linked pressure-sensitive adhesive described in [9] or

[10] above on a substrate or a release liner.

[0035]

[12] A method for producing a pressure-sensitive adhesive sheet, the method comprising the following steps 22 and 23:

[0036] Step 22, a step of forming an energy-ray crosslinkable adhesive composition layer formed of an energy-ray crosslinkable adhesive composition on a substrate or a release liner, wherein the energy-ray crosslinkable adhesive composition contains (A) an acrylic polymer having energy-ray crosslinkability, and (B) an acrylic polymer other than the component (A) which substantially does not contain free radical-reactive unsaturated double bonds and has a weight average molecular weight (Mw) of 280,000 or less;

[0037] Step 23: a step of irradiating the energy-ray crosslinkable adhesive composition layer with energy rays to form an adhesive layer composed of a crosslinked adhesive.

[0038]

[13] The method for producing a pressure-sensitive adhesive sheet according to

[12] , which comprises the following step 21 before the above step 22, and further, in the above step 22, the energy-ray cross-linkable pressure-sensitive adhesive composition layer is formed by melt-coating the energy-ray cross-linkable pressure-sensitive adhesive composition obtained in the following step 21 onto the above substrate or the above release liner,

[0039] Step 21 is a step of obtaining an energy-ray-crosslinkable adhesive composition by melt-kneading (A) an acrylic polymer having energy-ray crosslinkability and a component (B), wherein the component (B) is an acrylic polymer other than the component (A) which substantially does not contain free radical-reactive unsaturated double bonds and has a weight-average molecular weight (Mw) of not more than 280,000.

[0040] Effects of the Invention

[0041] According to the present invention, there can be provided an energy-ray cross-linkable adhesive composition capable of forming an adhesive having a long applicability and excellent coating properties, an adhesive sheet using the energy-ray cross-linkable adhesive composition and a method for manufacturing the same, a cross-linked adhesive formed by energy-ray cross-linking the energy-ray cross-linkable adhesive composition and a method for manufacturing the same, and an adhesive sheet using the cross-linked adhesive and a method for manufacturing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a schematic cross-sectional view showing an example of the structure of the pressure-sensitive adhesive sheet of the present invention.

[0043] Figure 2 This is a schematic cross-sectional view showing another example of the structure of the pressure-sensitive adhesive sheet of the present invention.

[0044] Figure 3 This is a schematic cross-sectional view showing another example of the structure of the pressure-sensitive adhesive sheet of the present invention.

[0045] Explanation of symbols

[0046] 1 Energy-ray-crosslinkable adhesive composition layer

[0047] 2, 2a, 2b Release liner

[0048] 3 Adhesive layer

[0049] 4 Substrate

[0050] 10a, 20a, 30a First adhesive sheet

[0051] 10b, 20b, 30b Second adhesive sheet DETAILED DESCRIPTION

[0052] In this specification, regarding the preferred numerical range (for example, the range of content, etc.), the lower limit and upper limit recorded in the segment can be independently combined. For example, according to the record of "preferably 10 to 90, more preferably 30 to 60", the "preferable lower limit (10)" and the "preferable upper limit (60)" can be combined to be set to "10 to 60". In addition, for example, the recording method of "preferably 10 or more, more preferably 30 or more, and preferably 90 or less, more preferably 60 or less" is also the same.

[0053] In this specification, "energy ray" refers to a ray having an energy quantum in an electromagnetic wave or a charged particle beam, and examples thereof include ultraviolet rays, radiation, electron beams, etc. Ultraviolet rays can be irradiated using, for example, an electrodeless lamp, a high-pressure mercury lamp, a metal halide lamp, a UV-LED, etc. as an ultraviolet source. Electron beams can be irradiated with electron beams generated by electron beam accelerators, etc. It should be noted that, as energy rays in one embodiment of the present invention, ultraviolet rays are preferably used among the above energy rays.

[0054] In the present specification, "energy ray crosslinkability" refers to a property of forming a crosslinked structure by irradiation with energy rays.

[0055] In addition, in this specification, "(meth)acrylic acid" is used as a term representing one or both of "acrylic acid" and "methacrylic acid". Similarly, "(meth)acrylate" is used as a term representing one or both of "acrylate" and "methacrylate". Similarly, "(meth)acryloyl" is used as a term representing one or both of "acryloyl" and "methacryloyl".

[0056] In addition, in this specification, "weight average molecular weight (Mw)" is a value measured by gel permeation chromatography (GPC) method and is converted into standard polystyrene, and specifically, it is a value measured according to the method described in the Examples.

[0057] In addition, the action mechanism described in this specification is a presumed mechanism and does not limit the mechanism by which the effects of the present invention are exerted.

[0058] [Energy beam crosslinkable adhesive composition]

[0059] The energy-beam-crosslinkable adhesive composition as one embodiment of the present invention contains (A) an acrylic polymer having energy-beam-crosslinkability (hereinafter also referred to as "component (A)"), and (B) an acrylic polymer other than the above-mentioned component (A) which substantially does not contain a free radical-reactive unsaturated double bond and has a weight average molecular weight (Mw) of not more than 280,000 (hereinafter also referred to as "component (B)").

[0060] The energy-ray crosslinkable adhesive composition (hereinafter also referred to as "adhesive composition") forms a crosslinked structure by irradiation with energy rays to form a crosslinked adhesive. That is, the adhesive composition is a composition that is intended to be irradiated with energy rays before or after being attached to an adherend.

[0061] The adhesive composition can be irradiated with energy rays at any time, so the adhesive composition has a high degree of freedom in its production method and use method.

[0062] Specifically, since the adhesive composition does not form a desired cross-linked structure, it can be melted by heating and is suitable as a hot melt adhesive.

[0063] In addition, since the adhesive composition does not form a desired cross-linked structure, it also has excellent shape-conforming properties. Therefore, the adhesive composition can also be suitably used for bonding to an adherend having a height difference, etc., and then forming a cross-linked adhesive by energy ray irradiation.

[0064] Next, each component contained in the said adhesive composition is demonstrated in detail.

[0065] <(A) Energy-beam-crosslinkable acrylic polymer>

[0066] The component (A) is not particularly limited as long as it is an acrylic polymer having energy-beam crosslinking properties. The component (A) may be used alone or in combination of two or more.

[0067] As the component (A), for example, there can be mentioned an acrylic polymer having an energy ray reactive group which reacts by irradiation with energy rays and contributes to the formation of a crosslinked structure.

[0068] Examples of the energy ray reactive group include energy ray reactive groups that are excited by irradiation with energy rays and generate radicals that induce a crosslinking reaction.

[0069] Specific examples of the energy-ray-reactive group include functional groups having a benzophenone structure, a benzyl structure, an o-benzoylbenzoate structure, a thioxanthone structure, a 3-coumarin ketone structure, a 2-ethylanthraquinone structure, a camphorquinone structure, etc. Among them, the (A) energy-ray-crosslinkable acrylic polymer preferably has a benzophenone structure in the side chain.

[0070] When the component (A) has a benzophenone structure, for example, the benzophenone structure abstracts a hydrogen atom from a hydrocarbon group included in a side chain of the acrylic polymer by irradiation with energy rays, and the radical is re-bonded to form a crosslinked structure.

[0071] In addition, from the viewpoint of easily forming a crosslinked structure, it is preferable to introduce an energy ray reactive group into the side chain of the acrylic polymer. That is, component (A) is preferably an acrylic polymer having a benzophenone structure in the side chain.

[0072] The content of the energy ray reactive group in the component (A) is preferably 0.02 to 5.0 mass %, more preferably 0.05 to 3.0 mass %, based on the total amount (100 mass %) of the component (A).

[0073] As a method for introducing the energy-ray reactive group in component (A), for example, it can be introduced by copolymerizing a monomer having a functional group such as a vinyl group that can react with an acrylic monomer and having the energy-ray reactive group, with an acrylic monomer. Alternatively, for example, it can be introduced by reacting a compound having the energy-ray reactive group with a side chain of an acrylic polymer using a known method.

[0074] The acrylic polymer is a polymer containing an acrylic monomer as a monomer component and is not particularly limited as long as it has energy ray crosslinking properties, but preferably contains a structural unit derived from an alkyl (meth)acrylate.

[0075] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, and lauryl (meth)acrylate. Among them, alkyl (meth)acrylates having an alkyl group with 1 to 8 carbon atoms are preferred, and 2-ethylhexyl (meth)acrylate, methyl (meth)acrylate, and butyl (meth)acrylate are more preferred.

[0076] In addition, these alkyl (meth)acrylates may be used alone or in combination of two or more.

[0077] In component (A), the content of the structural unit derived from the alkyl (meth)acrylate is preferably 80 to 100 mass %, more preferably 90 to 100 mass %, further preferably 95 to 100 mass %, and further preferably 98 to 100 mass % in all the structural units (100 mass %) of component (A).

[0078] In the present specification, the content of the structural unit of the monomer of component (A) relative to all structural units (100 mass %) may be regarded as the content of the monomer in 100 mass % of the total amount of monomers blended when synthesizing component (A).

[0079] Unless otherwise specified, all structural units (100% by mass) of the component (A) do not include structural units derived from, for example, a polymerization initiator, a chain transfer agent, and a compound having an energy ray reactive group used for polymerization of the polymer.

[0080] In addition, as a structural unit derived from a monomer constituting the acrylic polymer, a structural unit derived from a monomer other than the above-mentioned alkyl (meth)acrylate may be included as needed. Examples of other monomers other than the alkyl (meth)acrylate that can be used in component (A) include monomers other than the monomer (b1) described later in the column of component (B).

[0081] The weight average molecular weight (Mw) of component (A) is not particularly limited as long as the effects of the present invention can be exerted, but is preferably 10,000 or more, more preferably 50,000 or more, and even more preferably 100,000 or more, and is preferably 500,000 or less, more preferably 400,000 or less, and even more preferably 300,000 or less.

[0082] The content of the component (A) in the adhesive composition may be 50 to 98% by mass, 60 to 97% by mass, or 70 to 96% by mass, based on 100% by mass of the total amount of the adhesive composition.

[0083] <(B) An acrylic polymer other than the above-mentioned component (A) which contains substantially no radically reactive unsaturated double bonds and has a weight average molecular weight (Mw) of 280,000 or less>

[0084] Component (B) is not particularly limited as long as it is an acrylic polymer other than the above-mentioned component (A), is an acrylic resin that substantially does not contain a radically reactive unsaturated double bond, and has a weight average molecular weight (Mw) of 280000 or less. Component (B) may be used alone or in combination of two or more.

[0085] By including the component (B) in the pressure-sensitive adhesive composition, the pressure-sensitive adhesive performance can be improved.

[0086] Since component (B) does not substantially contain a radically reactive unsaturated double bond, when the adhesive composition is heated, the polymerization reaction of component (B) can be prevented or suppressed, and the viscosity increase of the adhesive composition over time can be suppressed. As a result, the pot life of the adhesive composition can be extended.

[0087] The above-mentioned "free radical reactive unsaturated double bonds" refer to unsaturated double bonds that can participate in free radical reactions by heating or energy irradiation, including both unsaturated double bonds that react with free radicals generated from components other than component (B) such as an initiator to generate active points for free radical reactions, and unsaturated double bonds that themselves are activated by heating or energy irradiation to generate free radicals and initiate reactions.

[0088] Examples of the radically reactive unsaturated double bond include radically reactive carbon-carbon double bonds, and examples of the functional group containing a radically reactive carbon-carbon double bond include (meth)acryloyl, vinyl, and allyl groups.

[0089] In addition, component (B) "does not substantially contain free radical reactive unsaturated double bonds" means, for example, that, among all the structural units (100 mass %) of component (B), the content of structural units derived from monomers having free radical reactive unsaturated double bonds even after polymerization is preferably 1.0 mass % or less, more preferably 0.1 mass % or less, and even more preferably 0.05 mass % or less.

[0090] In the present specification, the content of the structural unit of the monomer of the component (B) relative to all structural units (100 mass %) may be regarded as the content of the monomer in 100 mass % of the total amount of monomers blended when synthesizing the component (B).

[0091] Unless otherwise specified, all the structural units (100% by mass) of the component (B) do not include structural units derived from, for example, a polymerization initiator and a chain transfer agent used for polymerization of the polymer.

[0092] In addition, if the weight average molecular weight (Mw) of component (B) exceeds 280000, the viscosity of the above-mentioned adhesive composition becomes high and the coating property is poor. Therefore, from the viewpoint of suppressing the coating property of the above-mentioned adhesive composition from being reduced, the weight average molecular weight (Mw) of component (B) is preferably 260000 or less, more preferably 240000 or less, and further preferably 220000 or less. In addition, the weight average molecular weight (Mw) of component (B) is preferably 1000 or more, more preferably 5000 or more, and further preferably 10000 or more.

[0093] The component (B) is not particularly limited as long as it is a polymer that satisfies the above-mentioned requirements and contains an acrylic monomer as a monomer component, but preferably contains a structural unit derived from an alkyl (meth)acrylate (b1).

[0094] As the (meth)acrylic acid alkyl ester (b1) (hereinafter also referred to as "monomer (b1)") that can be used in the component (B), for example, an alkyl (meth)acrylic acid alkyl ester having an alkyl group with 1 to 18 carbon atoms can be preferably used. Specifically, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, stearyl (meth)acrylate, and the like can be mentioned.

[0095] The monomer (b1) may be used alone or in combination of two or more.

[0096] As the monomer (b1), among the above-mentioned monomers, a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms is more preferable.

[0097] In component (B), from the viewpoint of achieving better compatibility with component (A), the content of the structural unit derived from monomer (b1) in all the structural units (100% by mass) of component (B) is preferably 60 to 100% by mass, more preferably 80 to 100% by mass, further preferably 90 to 100% by mass, and further preferably 95 to 100% by mass.

[0098] Moreover, the component (B) may be an acrylic copolymer containing a structural unit derived from a monomer other than the monomer (b1) in addition to the structural unit derived from the monomer (b1).

[0099] Examples of monomers other than monomer (b1) include functional group-containing monomers having no two or more radically reactive unsaturated double bonds in the molecule, (meth)acrylates having a cyclic structure having no two or more radically reactive unsaturated double bonds in the molecule, vinyl acetate, styrene, and the like.

[0100] Monomers other than the monomer (b1) may be used alone or in combination of two or more.

[0101] Examples of the functional group-containing monomer having no two or more radically reactive unsaturated double bonds in the molecule include monomers having functional groups such as carboxyl, hydroxyl, epoxy, amino, cyano, nitrogen-containing cyclic groups, and alkoxysilyl groups.

[0102] Examples of the carboxyl group-containing monomer include ethylenically unsaturated carboxylic acids having only a radical-reactive unsaturated double bond, such as (meth)acrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, and citraconic acid.

[0103] Examples of hydroxyl-containing monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and unsaturated alcohols having only one free radical-reactive unsaturated double bond such as vinyl alcohol and allyl alcohol.

[0104] Examples of the (meth)acrylate having a cyclic structure and not having two or more radically reactive unsaturated double bonds in the molecule include cyclohexyl (meth)acrylate, benzophenone (meth)acrylate, and isobornyl (meth)acrylate.

[0105] When component (B) contains structural units derived from monomers other than monomer (b1), in component (B), the content of structural units derived from monomers other than monomer (b1) is preferably 0.5 to 40 mass%, more preferably 1 to 20 mass%, further preferably 2 to 10 mass%, and further preferably 3 to 5 mass%, relative to all structural units (100 mass%) of component (B).

[0106] When component (B) contains structural units derived from monomers other than monomer (b1) in addition to the structural units derived from monomer (b1), in the above-mentioned component (B), the total content of the structural units derived from monomer (b1) and the structural units derived from monomers other than monomer (b1) can be 100 mass% relative to all the structural units of component (B) (100 mass%).

[0107] In addition, when component (B) is an acrylic copolymer containing structural units derived from multiple monomers (b1); or an acrylic copolymer containing structural units derived from a single or multiple monomers (b1) and structural units derived from a single or multiple monomers other than monomer (b1), the copolymerization method is not particularly limited and it can be a block copolymer or a random copolymer.

[0108] Relative to 100 parts by mass of the above-mentioned component (A), the content of the component (B) in the above-mentioned adhesive composition is preferably 50 parts by mass or less, and from the viewpoint of being able to suppress the reduction of the cohesive force of the adhesive obtained from the adhesive composition and suppressing the contamination of the adherend to which the adhesive is attached, it is more preferably 45 parts by mass or less, and further preferably 40 parts by mass or less. In addition, from the viewpoint of adhesive performance, the lower limit of the content of the component (B) in the above-mentioned adhesive composition is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and further preferably 10 parts by mass or more.

[0109] In addition, from the viewpoint of making it easier to exert the effects of the present invention, the total content of the above-mentioned components (A) and (B) in 100 mass % of the total amount of the above-mentioned adhesive composition is preferably 60 mass % or more, more preferably 70 mass % or more, further preferably 80 mass % or more, and is less than 100 mass %.

[0110] <(C) Hydrogen abstraction type photoinitiator>

[0111] The adhesive composition may further contain (C) a hydrogen abstraction type photoinitiator (hereinafter also simply referred to as “component (C)”).

[0112] Component (C) has the function of generating free radicals. Moreover, the generated free radicals can generate free radicals in the acrylic polymer by taking away hydrogen bonded to carbon in the main chain skeleton, etc. in the above-mentioned component (A) and / or component (B), thereby directly crosslinking the above-mentioned components (A) with each other, components (B) with each other, or components (A) and (B).

[0113] As component (C), for example, aromatic ketones such as acetophenone, benzophenone, P,P'-dimethoxybenzophenone, 4-methylbenzophenone, P,P'-dichlorobenzophenone, P,P'-dimethylbenzophenone, and naphthyl acetonide can be mentioned. In addition, aromatic aldehydes such as terephthalaldehyde and quinone aromatic compounds such as methyl anthraquinone can also be mentioned. Among them, from the viewpoint of the ease of generating free radicals, it is preferred to use a compound containing benzophenone.

[0114] The component (C) may be used alone or in combination of two or more.

[0115] When the above-mentioned adhesive composition contains component (C), the content of component (C) in the above-mentioned adhesive composition is preferably 0.1 mass part or more, more preferably 0.2 mass part or more, further preferably 0.3 mass part or more, and is preferably 3.0 mass parts or less, more preferably 2.0 mass parts or less, further preferably 1.0 mass part or less, relative to 100 mass parts of the total of component (A) and component (B).

[0116] <(D) Thickener>

[0117] The pressure-sensitive adhesive composition may further contain (D) a tackifier (hereinafter also simply referred to as “component (D)”).

[0118] The component (D) is a component that can improve the adhesive properties of the obtained cross-linked adhesive, and is not particularly limited as long as the effects of the present invention can be exhibited.

[0119] Examples of the component (D) include: rosin resins such as polymerized rosin, polymerized rosin esters, and rosin derivatives, and hydrogenated products thereof (hydrogenated rosin resins); terpene resins such as polyterpene resins, aromatic modified terpene resins, and terpene phenolic resins, and hydrogenated products thereof (hydrogenated terpene resins); coumarone-indene resins; petroleum resins such as aliphatic petroleum resins, aromatic petroleum resins, and aliphatic / aromatic copolymer petroleum resins, and hydrogenated products thereof (hydrogenated petroleum resins); styrene or substituted styrene polymers; styrene resins such as α-methylstyrene homopolymer resins, copolymers of α-methylstyrene and styrene, copolymers of styrene monomers and aliphatic hydrocarbon monomers, copolymers of styrene, α-methylstyrene and aliphatic hydrocarbon monomers, homopolymers formed from styrene monomers, and copolymers of styrene monomers and aromatic monomers, and hydrogenated products thereof (hydrogenated styrene resins), etc.

[0120] The component (D) may be used alone or in combination of two or more.

[0121] The softening point of the component (D) is preferably 70 to 140°C, more preferably 80 to 135°C, and even more preferably 85 to 130°C.

[0122] When the softening point of component (D) is 70°C or higher, excellent adhesive strength tends to be easily obtained at high temperatures. When the softening point of component (D) is 140°C or lower, it tends to be easily mixed with the energy-beam crosslinkable acrylic resin (A).

[0123] In addition, in this specification, the softening point of component (D) means the value measured according to JIS K5601-2-2:1999.

[0124] When the adhesive composition contains component (D), the content of component (D) in the adhesive composition is preferably 5 to 35 parts by mass, more preferably 10 to 30 parts by mass, and even more preferably 15 to 25 parts by mass, relative to 100 parts by mass of component (A).

[0125] When the adhesive composition contains component (D), when the content of component (D) is 5 parts by mass or more, there is a tendency to more easily improve the adhesive force. In addition, when the content of component (D) is 40 parts by mass or less, there is a tendency to more easily improve the holding force.

[0126] <Other ingredients>

[0127] The pressure-sensitive adhesive composition may or may not contain components other than the above-mentioned components as long as the effects of the present invention can be exhibited.

[0128] As other components, a softener, an antioxidant, and an adhesive additive used for a general adhesive are mentioned, for example.

[0129] These other components may be used alone or in combination of two or more.

[0130] The antioxidant is not particularly limited, and a conventionally known antioxidant can be used. Examples of the antioxidant include hindered phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants.

[0131] Examples of adhesive additives used in the above-mentioned general adhesives include waxes, fillers, extenders, heat stabilizers, light stabilizers, ultraviolet absorbers, colorants (pigments, dyes, etc.), flame retardants, antistatic agents, stringing inhibitors, anti-aging agents, inorganic particles, organic particles, lightweight agents, etc.

[0132] These adhesive additives may be used alone or in combination of two or more.

[0133] When these other components are contained, the content of each other component is independently preferably 0.0001 to 20 parts by mass, more preferably 0.001 to 10 parts by mass, based on 100 parts by mass of the total of component (A) and component (B).

[0134] In addition, from the viewpoint of making it easier to exert the effects of the present invention, the above-mentioned adhesive composition preferably does not substantially contain a compound having an unsaturated double bond with free radical reactivity, such as a multifunctional acrylate. Here, the above-mentioned adhesive composition "does not substantially contain a compound having an unsaturated double bond with free radical reactivity" means, for example, that the content of the compound having an unsaturated double bond with free radical reactivity is preferably 1.0% by mass or less, more preferably 0.1% by mass or less, and further preferably 0.05% by mass or less in the total amount of 100% by mass of the above-mentioned adhesive composition.

[0135] In addition, from the viewpoint of reducing environmental burden, it is preferred that the adhesive composition does not substantially contain a solvent, and more preferably does not contain a solvent. Here, the adhesive composition "does not substantially contain a solvent" means, for example, that the content of the solvent is preferably 0.5% by mass or less, and more preferably 0.1% by mass or less in 100% by mass of the total amount of the adhesive composition.

[0136] In addition, when the above-mentioned adhesive composition further contains one or more selected from component (C), component (D) and the above-mentioned other components in addition to the above-mentioned components (A) and (B), the total content of one or more selected from the above-mentioned components (A) and (B), and component (C), component (D) and the above-mentioned other components in 100 mass% of the total amount of the above-mentioned adhesive composition is preferably 60 mass% or more, more preferably 70 mass% or more, further preferably 80 mass% or more, and is less than 100 mass%.

[0137] <Method for producing adhesive composition>

[0138] The above-mentioned adhesive composition can be produced, for example, by a kneading method of melt-kneading (A) an acrylic resin having energy-ray crosslinking properties, component (B), and optional components used as needed, wherein the above-mentioned component (B) is an acrylic polymer that substantially does not contain free radical-reactive unsaturated double bonds and has a weight-average molecular weight (Mw) of 280,000 or less.

[0139] In addition, in the following description, the step of melt-kneading the component (A) and the component (B) and the like may be referred to as a "melt-kneading step".

[0140] The melt-kneading step is, for example, a step of placing the components into a mixing device equipped with a heating device such as a heating kneader, and mixing the components in a melted state.

[0141] Examples of the mixing device including a heating device include a single-screw extruder, a twin-screw extruder, a roll mill, a Banbury mixer, an intermixer, and a pressure kneader.

[0142] When a mixing device capable of reducing pressure is used, the interior of the mixing device may be reduced in pressure as necessary to perform melt-kneading under reduced pressure.

[0143] The kneading temperature in the melt kneading step is not particularly limited, and any temperature condition that allows the components to be sufficiently mixed in a molten state may be appropriately selected, but is preferably 80 to 180°C, more preferably 100 to 170°C, and even more preferably 120 to 150°C.

[0144] It should be noted that, when the adhesive composition is produced by melt kneading, the adhesive composition does not need to contain a solvent, and from the viewpoint of reducing environmental burden, it is preferably substantially free of solvent, and more preferably free of solvent. Here, the adhesive composition "substantially free of solvent" means, for example, that the content of the solvent is preferably 0.5% by mass or less, and more preferably 0.1% by mass or less in 100% by mass of the total amount of the adhesive composition.

[0145] The PSA composition obtained after melt kneading can be directly applied to a substrate or a release liner by an extruder or the like while being heated and molten, and used for the production of a PSA sheet as one embodiment of the present invention described below, or can be filled into various containers or the like as desired, for example, without undergoing a molding step.

[0146] [Cross-linking adhesive]

[0147] The cross-linked adhesive as one embodiment of the present invention is a cross-linked adhesive obtained by irradiating the above-mentioned energy-ray cross-linkable adhesive composition as one embodiment of the present invention with energy rays.

[0148] That is, the cross-linkable adhesive has a cross-linked structure formed by an energy-ray cross-linking reaction of the (A) energy-ray cross-linkable acrylic resin contained in the energy-ray cross-linkable adhesive composition.

[0149] The cross-linked adhesive itself also has good adhesive force and can also exert excellent adhesive force on the adherend. For example, from the viewpoint of not requiring an energy ray irradiation step after sticking to the adherend, the cross-linked adhesive may be formed by irradiating the adhesive composition with energy rays before sticking it to the adherend, and then sticking it to the adherend as a cross-linked adhesive.

[0150] The cross-linkable adhesive can be produced by irradiating the energy-ray cross-linkable adhesive composition with energy rays.

[0151] That is, the method for producing the cross-linkable adhesive comprises the step of irradiating the energy-ray cross-linkable adhesive composition with energy rays.

[0152] In addition, in the following description, the process of irradiating the said energy-ray crosslinkable adhesive composition with energy rays may be called "energy-ray irradiation process".

[0153] [Adhesive sheet]

[0154] As one embodiment of the present invention, the following first and second pressure-sensitive adhesive sheets can be provided.

[0155] The first pressure-sensitive adhesive sheet is a pressure-sensitive adhesive sheet having an energy-ray cross-linkable pressure-sensitive adhesive composition layer formed from the above-mentioned energy-ray cross-linkable pressure-sensitive adhesive composition on a substrate or a release liner.

[0156] The second PSA sheet is a PSA sheet having a PSA layer formed of the above-mentioned cross-linked PSA on a substrate or a release liner.

[0157] In the following description, the “energy-ray cross-linkable adhesive composition layer formed of the energy-ray cross-linkable adhesive composition” of the first adhesive sheet is also simply referred to as “adhesive composition layer”.

[0158] In addition, the "adhesive layer formed of the cross-linked adhesive" of the second adhesive sheet is also simply referred to as "adhesive layer".

[0159] In addition, when simply referred to as a "pressure-sensitive adhesive sheet", it refers to both the first pressure-sensitive adhesive sheet and the second pressure-sensitive adhesive sheet.

[0160] Next, an example of the structure of the pressure-sensitive adhesive sheet which is one embodiment of the present invention will be described using the drawings, but the present invention is not limited to the following examples.

[0161] exist Figure 1 In (a), as an example of the first PSA sheet, a PSA sheet 10a is shown which has a release liner 2 on one side of a PSA composition layer 1 and a substrate 4 on the other side of the PSA composition layer 1 .

[0162] In addition, Figure 1 In (b), as an example of the second PSA sheet, a PSA sheet 10b is shown which has a release liner 2 on one side of the PSA layer 3 and a substrate 4 on the other side of the PSA layer 3 .

[0163] The pressure-sensitive adhesive sheets 10a and 10b are suitable for applications such as pasting the exposed surface of the pressure-sensitive adhesive composition layer 1 or the pressure-sensitive adhesive layer 3 to an adherend after the release liner 2 is peeled off. Examples of such applications include label applications.

[0164] When the PSA sheet to be attached to the adherend is the first PSA sheet, after being attached to the adherend, the PSA composition layer is irradiated with energy rays to form a PSA layer composed of the crosslinked PSA.

[0165] exist Figure 2 In (a), as another example of the first adhesive sheet, a double-sided adhesive sheet 20a is shown, which has an adhesive composition layer 1 on both sides of a substrate 4, a release liner 2a on the side of one adhesive composition layer 1 opposite to the substrate 4, and a release liner 2b on the side of the other adhesive composition layer 1 opposite to the substrate 4.

[0166] In addition, Figure 2 In (b), as another example of the second adhesive sheet, a double-sided adhesive sheet 20b is shown, which has adhesive layers 3 on both sides of a substrate 4, a release liner 2a on one side of one adhesive layer 3 opposite to the substrate 4, and a release liner 2b on the other side of the other adhesive layer 3 opposite to the substrate 4.

[0167] exist Figure 3 In (a), as another example of the first PSA sheet, a substrate-free PSA sheet 30a having release liners 2a and 2b on both surfaces of the PSA composition layer 1 is shown.

[0168] In addition, Figure 3 In (b), as another example of the second PSA sheet, a substrate-free PSA sheet 30b having release liners 2a and 2b on both sides of the PSA layer 3 is shown.

[0169] The adhesive sheets 20a, 20b, 30a and 30b are suitable for laminating adherends, for example, in which the release liner 2a on one side is peeled off and removed, and the exposed surface of the adhesive composition layer 1 or the adhesive layer 3 is adhered to the adherend, and then the release liner 2b is further peeled off and removed, and the exposed surface of the adhesive composition layer 1 or the adhesive layer 3 is adhered to another adherend. Such applications include, for example, fixing or temporarily fixing various components.

[0170] It should be noted that, for the adhesive sheets 30a and 30b, when the release force when the release liner 2a is peeled off from the adhesive composition layer 1 or the adhesive layer 3 is about the same as the release force when the release liner 2b is peeled off from the adhesive composition layer 1 or the adhesive layer 3, if the two release liners are pulled outward to peel, the adhesive composition layer 1 or the adhesive layer 3 may be peeled off as the two release liners are broken. From the viewpoint of suppressing such a phenomenon, it is preferred that two types of release liners designed to have different release forces are used for the two release liners 2a and 2b.

[0171] The thickness of the adhesive composition layer in the first adhesive sheet and the thickness of the adhesive layer in the second adhesive sheet are each independently preferably 5 to 100 μm, more preferably 10 to 60 μm, and even more preferably 15 to 30 μm.

[0172] When the thickness of the adhesive composition layer and the adhesive layer is 5 μm or more, the adhesive strength tends to be further improved. When the thickness of the adhesive composition layer and the adhesive layer is 100 μm or less, the handling property tends to be better.

[0173] <Base material>

[0174] Examples of the material for forming the substrate include resins, metals, and paper materials.

[0175] Examples of the resin include: polyolefin resins such as polyethylene and polypropylene; vinyl resins such as polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polystyrene; acrylonitrile-butadiene-styrene copolymer; cellulose triacetate; polycarbonate; urethane resins such as polyurethane and acrylic modified polyurethane; polymethylpentene; polysulfone; polyetheretherketone; polyethersulfone; polyphenylene sulfide; polyimide resins such as polyetherimide and polyimide; polyamide resins; acrylic resins; fluorine resins, etc.

[0176] Examples of the metal include aluminum, tin, chromium, and titanium.

[0177] Examples of the paper material include thin paper, medium-weight paper, fully-pulped paper, impregnated paper, coated paper, art paper, sulphate paper, and glassine paper.

[0178] The material for forming the substrate may be composed of one kind or a combination of two or more kinds.

[0179] Examples of substrates formed by combining two or more forming materials include substrates formed by laminating a paper material with a thermoplastic resin such as polyethylene, and substrates formed by forming a metal film on the surface of a resin film or sheet containing a resin. It should be noted that examples of methods for forming the metal layer include: a method of vapor-depositing the above metal by a PVD method such as vacuum evaporation, sputtering, or ion plating; or a method of attaching a metal foil formed of the above metal using a general adhesive.

[0180] In order to improve the interlayer adhesion between the substrate and other laminated layers, when the substrate contains a resin, the surface of the substrate may be subjected to surface treatment such as oxidation and embossing, or primer treatment.

[0181] Depending on the purpose of the adhesive sheet, the substrate may have, for example, an easy-adhesion layer for facilitating printing; a recording layer for realizing thermal transfer recording, inkjet recording, etc.; an outer coating film or outer lamination film for protecting their surface; information areas such as magnetic recording, bar codes, micro-semiconductor elements, etc.

[0182] On the other hand, when the pressure-sensitive adhesive sheet is made into a transparent pressure-sensitive adhesive sheet, it is preferable that the base material has transparency.

[0183] The substrate may contain a substrate additive as required. Examples of the substrate additive include ultraviolet light absorbers, light stabilizers, antioxidants, antistatic agents, slip agents, antiblocking agents, colorants, etc. It should be noted that these substrate additives may be used alone or in combination of two or more.

[0184] The thickness of the substrate is preferably 5 to 1000 μm, more preferably 15 to 500 μm, and even more preferably 20 to 200 μm.

[0185] When the thickness of the substrate is 5 μm or more, the deformation resistance of the PSA sheet tends to be improved. On the other hand, when the thickness of the substrate is 1000 μm or less, the handling properties of the PSA sheet tends to be improved.

[0186] In addition, "the thickness of a base material" means the thickness of the whole base material, and when the base material is a base material formed of a plurality of layers, it means the total thickness of all the layers constituting the base material.

[0187] <Release liner>

[0188] As the release liner, a double-sided release liner, a single-sided release liner, or the like can be used. Examples of the release liner include a release liner obtained by coating a release agent on a substrate for the release liner.

[0189] Examples of the release liner substrate include paper such as full-grain paper, glassine paper, and kraft paper; plastic films such as polyester resin films such as polyethylene terephthalate resin, polybutylene terephthalate resin, and polyethylene naphthalate resin; and polyolefin resin films such as polypropylene resin and polyethylene resin.

[0190] Examples of the release agent include rubber elastomers such as silicone resins, olefin resins, isoprene resins, and butadiene resins; long-chain alkyl resins, alkyd resins, and fluorine resins.

[0191] The thickness of the release liner is not particularly limited, but is preferably 10 to 200 μm, more preferably 20 to 180 μm, and even more preferably 30 to 150 μm.

[0192] [Method for producing the first adhesive sheet]

[0193] As a method for producing the first pressure-sensitive adhesive sheet, for example, there can be mentioned a method for producing a pressure-sensitive adhesive sheet comprising the following steps 11 and 12.

[0194] Step 11: A step of obtaining an energy-ray-crosslinkable adhesive composition by melt-kneading (A) an energy-ray-crosslinkable acrylic resin and component (B), wherein the component (B) is an acrylic polymer substantially free of free radical-reactive unsaturated double bonds and having a weight average molecular weight (Mw) of 280,000 or less.

[0195] Step 12: A step of forming the energy-ray cross-linkable adhesive composition layer by melt-coating the energy-ray cross-linkable adhesive composition onto a substrate or a release liner.

[0196] In addition, in this specification, when a release liner is subjected to a release treatment on one side, "on the release liner" means the side subjected to the release treatment.

[0197] The description of the above step 11 is as described in the description of the melt-kneading step in the method for producing the energy-ray crosslinkable adhesive composition as one embodiment of the present invention. Similarly, in the above step 11, components (A) and (B), as well as any components used as needed, such as the above-mentioned component (C), component (D) and other components, can be melt-kneaded to obtain an adhesive composition. The component (A), component (B), substrate, release liner, and component (C), component (D) and other components used in the method for producing the first adhesive sheet are the same as those described in the column of the energy-ray crosslinkable adhesive composition, and the preferred embodiments are also the same.

[0198] The step 12 may be a method of directly coating the energy-beam crosslinkable adhesive composition obtained in the step 11 in a heated and molten state on a substrate or a release liner using an extruder and a T-die etc. to form an adhesive composition layer. Thereafter, a step of cooling the adhesive composition layer may be included as required.

[0199] Through the above step 12, a PSA composition layer can be formed on the substrate or the release liner.

[0200] The sheet having the substrate or release liner and the PSA composition layer may be used as the first PSA sheet as one embodiment of the present invention as it is, or may be subjected to other steps to obtain a desired PSA sheet configuration as required.

[0201] For example, by attaching the release-treated surface of a release liner to the exposed surface of a PSA composition layer formed on a substrate, a film such as Figure 1Like the PSA sheet 10a shown in (a), the PSA sheet has a release liner on one side of the PSA composition layer and a substrate on the other side of the PSA composition layer.

[0202] In addition, by attaching the substrate surface of the pressure-sensitive adhesive sheet 10a to the exposed surface of the pressure-sensitive adhesive composition layer formed on the release liner, a pressure-sensitive adhesive sheet 10a can be produced. Figure 2 Like the PSA sheet 20a shown in (a), this is a double-sided PSA sheet having PSA composition layers on both sides of a substrate, and having a release liner on the side of each PSA composition layer opposite to the substrate.

[0203] In addition, by attaching the release-treated surface of another release liner to the exposed surface of the adhesive composition layer formed on the release liner, a film such as Figure 3 This is a substrate-free PSA sheet having release liners on both sides of the PSA composition layer, such as the PSA sheet 30a shown in (a).

[0204] [Method for producing the second adhesive sheet]

[0205] As a method for producing the second pressure-sensitive adhesive sheet, for example, there can be mentioned a method for producing a pressure-sensitive adhesive sheet having the following steps 22 and 23.

[0206] Step 22: A step of forming an energy-ray cross-linkable adhesive composition layer formed by an energy-ray cross-linkable adhesive composition on a substrate or a release liner, wherein the energy-ray cross-linkable adhesive composition contains (A) an acrylic resin having energy-ray cross-linkability, and (B) an acrylic polymer that substantially does not contain free radical-reactive unsaturated double bonds and has a weight-average molecular weight (Mw) of not more than 280,000.

[0207] Step 23: a step of irradiating the energy-ray-crosslinkable pressure-sensitive adhesive composition layer with energy rays to form a pressure-sensitive adhesive layer composed of a crosslinked pressure-sensitive adhesive.

[0208] The step 22 can be performed, for example, in the same manner as the step 12 in the method for producing the first adhesive sheet, preferably in the same manner as the step 12 in the method for producing the first adhesive sheet. That is, the step 22 is preferably performed by melt-coating the energy-ray crosslinkable adhesive composition on a substrate or a release liner to form the energy-ray crosslinkable adhesive composition layer.

[0209] In the above step 23, the timing of energy ray irradiation is not particularly limited and can be appropriately determined in consideration of the production method of the pressure-sensitive adhesive sheet, desired physical properties, and the like.

[0210] For example, the adhesive composition layer may be irradiated with energy rays directly or through a substrate or a release liner in a state where one side of the adhesive composition layer is exposed, or the adhesive composition layer may be irradiated with energy rays through a substrate or a release liner in a state where a substrate or a release liner is provided on one side and a release liner is provided on the other side.

[0211] In addition, the energy ray irradiation can be performed once or divided into multiple times. In the case of dividing into multiple times to perform the energy ray irradiation, for example, the first energy ray irradiation can be performed in a state where one side of the adhesive composition layer is exposed, and then, after a substrate or a release liner is pasted on the side, the second energy ray irradiation is performed across the substrate or the release liner.

[0212] Furthermore, the first energy ray irradiation may be performed at any time before the adhesive is attached to the adherend, and the second energy ray irradiation may be performed after the adhesive is attached to the adherend.

[0213] In addition, as a method for manufacturing the above-mentioned second adhesive sheet, it is preferred that the following step 21 is included before the above-mentioned step 22, and further, in the above-mentioned step 22, the above-mentioned energy-ray cross-linkable adhesive composition layer is formed by melt-coating the energy-ray cross-linkable adhesive composition obtained through the following step 21 onto the above-mentioned substrate or the above-mentioned release liner.

[0214] Step 21: A step of obtaining an energy-ray crosslinkable adhesive composition by melt-kneading (A) an energy-ray crosslinkable acrylic resin and component (B), wherein the component (B) is an acrylic polymer substantially free of free radical-reactive unsaturated double bonds and having a weight average molecular weight (Mw) of not more than 280,000.

[0215] The above step 21 is the same as step 11 in the method for producing the first pressure-sensitive adhesive sheet, and is as described in the above step 11.

[0216] [Application of energy-ray crosslinkable adhesive composition, crosslinked adhesive, and adhesive sheet]

[0217] The energy-ray crosslinkable pressure-sensitive adhesive composition, the crosslinkable pressure-sensitive adhesive, and the pressure-sensitive adhesive sheet described above as one embodiment of the present invention can be used for various purposes.

[0218] Specifically, for example, the use can be for labels, for fixing or temporarily fixing various parts, for surface protection, for sealing materials, for decoration, for display, and the like.

[0219] Among them, the use for labels and the use for fixing or temporarily fixing various parts is preferred.

[0220] The adhesive sheet for label use can be directly attached to various products, or attached to packaging films, packaging containers, etc. of various products. Examples of the constituent materials of packaging films and packaging containers include: olefin resins such as polypropylene and polyethylene; polyester resins such as polyethylene terephthalate (PET) and polylactic acid; glass, paper, metal, etc.

[0221] The pressure-sensitive adhesive sheet for fixing or temporarily fixing is suitable for fixing or temporarily fixing electronic components, optical components, automobile parts, mechanical components, building components, decorative components, and the like.

[0222] Example

[0223] The present invention will be specifically described by the following examples, but the present invention is not limited to the following examples. It should be noted that the physical property values ​​in each example are values ​​measured by the following methods.

[0224] [Weight average molecular weight (Mw)]

[0225] The weight average molecular weight (Mw) was measured using a gel permeation chromatography apparatus under the following conditions and determined in terms of standard polystyrene.

[0226] (Measurement equipment)

[0227] · Measurement device: Product name "HLC-8320GPC", manufactured by Tosoh Corporation

[0228] Detector: Differential refractometer

[0229] Column: One "TSK guard column super HH", two "TSK gel super HM-H" were connected in series, and one "TSK gel super H2000" (all manufactured by Tosoh Corporation) were connected in order from the inlet side of the measurement sample.

[0230] (Measurement conditions)

[0231] Column temperature: 40℃

[0232] Elution solvent: tetrahydrofuran

[0233] Flow rate: 1.0mL / min

[0234] [Thickness of each layer]

[0235] The measurement was performed at 23° C. using a constant pressure thickness tester manufactured by TECLOCK (model: “PG-02J”, in accordance with standard standards: JIS K6783, Z 1702, Z 1709).

[0236] The details of the materials used in the following Examples and Comparative Examples are as follows.

[0237] <Component (A): Energy-beam crosslinkable acrylic polymer>

[0238] A260UV: acrylic polymer having a benzophenone structure in the side chain, trade name "acResin (registered trademark) A260UV" (manufactured by BASF): weight average molecular weight (Mw): 185,000

[0239] <Component (B): an acrylic polymer other than component (A) which contains substantially no radically reactive unsaturated double bonds and has a weight average molecular weight (Mw) of 280,000 or less>

[0240] ·P(BA)-1: "Poly(n-butyl acrylate)": weight average molecular weight (Mw) 200,000

[0241] ·P(BA)-2: "Poly(n-butyl acrylate)": weight average molecular weight (Mw) 100,000

[0242] <Component (C): Hydrogen abstraction type photoinitiator>

[0243] MBP: 4-methylbenzophenone, trade name "SpeedCure (registered trademark) MBP" (manufactured by Lambson Corporation)

[0244] <Ingredient (D): Thickener>

[0245] ·D-125: rosin-based resin (polymerized rosin ester), trade name "PENCEL (registered trademark) D-125" (manufactured by Arakawa Chemical Industries, Ltd.)

[0246] <Other ingredients>

[0247] ·P(BA)-3: “Polybutyl acrylate”: weight average molecular weight (Mw) 300,000

[0248] SR399E: dipentaerythritol pentaacrylate, trade name "Sartomer (registered trademark) SR399E" (manufactured by Sartomer Co., Ltd.)

[0249] CN104NS: Epoxy acrylate, trade name "Sartomer (registered trademark) CN104NS" (manufactured by Sartomer)

[0250] Examples 1 to 7, Comparative Examples 1 to 3

[0251] (Production of Energy-beam Crosslinkable Adhesive Composition)

[0252] The components were blended according to the composition shown in Table 1 (unit: parts by mass), and kneaded at 130° C. for 20 minutes under nitrogen purge using a heating kneader to obtain an energy-ray crosslinkable adhesive composition.

[0253] (Manufacturing of the first adhesive sheet)

[0254] The energy-ray crosslinkable adhesive composition obtained above was directly applied to a transparent polyethylene terephthalate film (thickness: 50 μm) as a substrate in a heated and molten state using a die coater, thereby obtaining a first adhesive sheet having an energy-ray crosslinkable adhesive composition layer (thickness: 20 μm) formed of the energy-ray crosslinkable adhesive composition on the substrate.

[0255] (Manufacturing of Second Adhesive Sheet)

[0256] The energy-beam crosslinkable pressure-sensitive adhesive composition layer of the first pressure-sensitive adhesive sheet obtained above was irradiated with a high-pressure mercury lamp (manufactured by EYE GRAPHICS) at a cumulative light intensity of 60 mJ / cm in the UV-C region. 2 The exposed surface was irradiated with ultraviolet rays under the conditions of . Thus, an adhesive layer (thickness: 20 μm) was formed by energy-ray crosslinking the energy-ray crosslinkable adhesive composition layer of the first adhesive sheet. Then, a release-treated surface of a release liner (thickness: 38 μm) was attached to the side of the adhesive layer opposite to the substrate, thereby obtaining a second adhesive sheet having a substrate, an adhesive layer, and a release liner in this order.

[0257] [Melt viscosity]

[0258] The energy-beam crosslinkable adhesive composition prepared in each example and each comparative example was measured for viscosity at 160° C. 1 hour and 10 hours after the start of heating using a viscometer (manufactured by Brookfield, trade name “DV-III ULTRA”) and a heater (manufactured by Brookfield, trade name “THERMOSEL”). The obtained results are shown in Table 1 below.

[0259] [Evaluation of contamination by adherends]

[0260] The second adhesive sheet prepared in each example and comparative example was cut into 25 mm x 50 mm in an environment of 23°C and 50% RH (relative humidity) to prepare two test pieces. The release liner of the test piece was removed and the exposed adhesive layer was attached to an adherend (stainless steel plate).

[0261] Then, the test piece attached to the adherend was allowed to stand for 7 days in an environment of 70°C and then for 1 day in an environment of 23°C and 50% RH. One of the test pieces was peeled off from the adherend by hand at a speed of about 300 mm / min in a 180° direction in an environment of 23°C and 50% RH (slow-speed peeling), and the other test piece was peeled off by hand at a speed of about 30 m / min in a 180° direction (high-speed peeling).

[0262] On this basis, the state of each layer of the pressure-sensitive adhesive layer after peeling was visually observed, and contamination of the adherend was confirmed according to the following criteria. The obtained results are shown in Table 1 below.

[0263] No contamination: Peeling occurs at the interface between the adhesive layer and the adherend, and no adhesive remains on the adherend, indicating excellent peeling properties.

[0264] Cohesive failure: The adhesive layer was broken, and the adhesive layer remained on the adherend.

[0265] surface

[0266]

[0267] Table 1 shows that the adhesive compositions obtained in Examples 1 to 7 have low melt viscosities at 160°C and excellent coating properties. In addition, it was confirmed that the viscosity did not increase significantly even after continuous heating at 160°C for 10 hours, and that the adhesive compositions had a long pot life and could be fully used even after heating for 10 hours.

[0268] It was also confirmed that the second adhesive sheets obtained in Examples 1 to 3 and Examples 5 to 7 did not contaminate the adherend even when peeled off from the adherend at a low speed after being attached to the adherend, and even when peeled off at a high speed. It was confirmed that although cohesive failure occurred in Example 4 when peeled off at a high speed, the adherend was not contaminated when peeled off at a low speed.

[0269] On the other hand, it was confirmed that the adhesive compositions obtained in Comparative Examples 1 and 2 both contained a compound having an unsaturated double bond with free radical reactivity instead of component (B). Therefore, the melt viscosity after continuous heating at 160°C for 10 hours exceeded 45,000 cP, and the coating properties were significantly reduced. Therefore, the adhesive compositions had a short applicability period.

[0270] In addition, it was confirmed that the weight average molecular weight (Mw) of component (B) of the adhesive composition obtained in Comparative Example 3 exceeded 280,000, and therefore the melt viscosity after 1 hour at 160° C. was as high as 42,000 cP, and the coating property was inferior to that of the Examples.

Claims

1. An energy-ray crosslinkable adhesive composition comprising: (A) an acrylic polymer having energy-ray crosslinkability, and (B) An acrylic polymer other than the component (A) which contains substantially no radically reactive unsaturated double bonds and has a weight average molecular weight (Mw) of 280,000 or less.

2. The energy-ray crosslinkable adhesive composition according to claim 1, wherein The component (A) is an acrylic polymer having a benzophenone structure in a side chain.

3. The energy-ray crosslinkable adhesive composition according to claim 1 or 2, wherein The content of the component (B) is 50 parts by mass or less relative to 100 parts by mass of the component (A). 4 . The energy-ray-crosslinkable pressure-sensitive adhesive composition according to claim 1 , further comprising (C) a hydrogen abstraction-type photoinitiator. 5 . The energy-ray-crosslinkable pressure-sensitive adhesive composition according to claim 1 , further comprising (D) a tackifier.

6. The energy-ray crosslinkable adhesive composition according to any one of claims 1 to 5, wherein The content of the component (A) is 50 to 98% by mass in 100% by mass of the total amount of the adhesive composition. 7 . A pressure-sensitive adhesive sheet comprising an energy-crosslinkable pressure-sensitive adhesive composition layer formed from the energy-crosslinkable pressure-sensitive adhesive composition according to claim 1 on a substrate or a release liner.

8. A method for producing a pressure-sensitive adhesive sheet having an energy-ray crosslinkable pressure-sensitive adhesive composition layer, the method comprising the following steps 11 and 12: Step 11, a step of obtaining an energy-ray-crosslinkable adhesive composition by melt-kneading (A) an acrylic polymer having energy-ray crosslinkability and a component (B), wherein the component (B) is an acrylic polymer other than the component (A) which substantially does not contain a free radical-reactive unsaturated double bond and has a weight average molecular weight (Mw) of 280,000 or less; Step 12 is a step of forming the energy-ray cross-linkable adhesive composition layer by melt-coating the energy-ray cross-linkable adhesive composition on a substrate or a release liner. 9 . A cross-linked adhesive obtained by irradiating the energy-ray cross-linkable adhesive composition according to claim 1 with energy rays.

10. A method for producing a cross-linked adhesive, which is a method for producing the cross-linked adhesive according to claim 9, the method comprising: A step of irradiating the energy-ray crosslinkable pressure-sensitive adhesive composition with energy rays. 11 . A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer formed of the cross-linking pressure-sensitive adhesive according to claim 9 or 10 on a substrate or a release liner.

12. A method for producing a pressure-sensitive adhesive sheet, the method comprising the following steps 22 and 23: Step 22, a step of forming an energy-ray crosslinkable adhesive composition layer formed of an energy-ray crosslinkable adhesive composition on a substrate or a release liner, wherein the energy-ray crosslinkable adhesive composition contains (A) an acrylic polymer having energy-ray crosslinkability, and (B) an acrylic polymer other than the component (A) which substantially does not contain a free radical-reactive unsaturated double bond and has a weight average molecular weight (Mw) of 280,000 or less; Step 23 is a step of irradiating the energy-ray crosslinkable pressure-sensitive adhesive composition layer with energy rays to form a pressure-sensitive adhesive layer composed of a crosslinked pressure-sensitive adhesive.

13. The method for producing a pressure-sensitive adhesive sheet according to claim 12, comprising the following step 21 before the step 22, wherein in the step 22, the energy-crosslinkable pressure-sensitive adhesive composition layer is formed by melt-coating the energy-crosslinkable pressure-sensitive adhesive composition obtained in the step 21 on the substrate or the release liner, Step 21 is a step of melt-kneading (A) an energy-ray-crosslinkable acrylic polymer and a component (B) to obtain an energy-ray-crosslinkable adhesive composition, wherein the component (B) is an acrylic polymer other than the component (A) which substantially does not contain free radical-reactive unsaturated double bonds and has a weight-average molecular weight (Mw) of not more than 280,000.

Citation Information

Patent Citations

  • Radiation curable hot-melt adhesive

    JP2015214601A