Dispersant composition for manufacturing battery pack

By using a polymer and amine composition in a specific ratio as a dispersant, the problems of increased viscosity and insufficient stability of battery electrode materials during storage were solved, resulting in a low-viscosity and low-volume resistivity electrode material dispersion, which improved the electrochemical performance of the battery pack.

CN118946979APending Publication Date: 2024-11-12BYK CHEMIE GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028621.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-20
Filing Date
2023-03-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The dispersions of existing battery pack electrode materials exhibit increased viscosity and poor dispersion stability and electrochemical properties during storage, especially high volume resistivity.

Method used

A dispersant composition comprising 30-80% of a first polymer, 10-60% of a low molecular weight amine and 5-20% of a second polymer, preferably using an N-vinyl lactam polymer and a fatty acid-modified polyether, in combination with an organic solvent, is used to form a low-viscosity and stable dispersion.

Benefits of technology

This achieved low viscosity, good dispersion stability, and low volume resistivity in the electrode material, thereby improving the electrochemical performance of the battery pack.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005049482800000191
    Figure BDA0005049482800000191
  • Figure BDA0005049482800000201
    Figure BDA0005049482800000201
Patent Text Reader

Abstract

The invention relates to a dispersant composition comprising a) 30 to 80% by weight of at least one first polymer, b) 10 to 60% by weight of at least one amine having a molecular weight of at most 250 g / mol, and c) 5 to 20% by weight of at least one second polymer different from the first polymer, where the% by weight is based on the total weight of a), b) and c).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a dispersant composition comprising a polymer and an amine, the use of the composition as a dispersant for conductive carbon-based materials and for reducing the viscosity of a composition for preparing an electrode for a rechargeable battery, to a composition for preparing an electrode for a rechargeable battery, to a method for preparing a dispersion of a conductive carbon-based material, and to a method for preparing an electrode for a rechargeable battery.

[0002] International patent application WO 2019 / 236313 A1 describes compositions that can be used to produce battery electrodes. In some examples, dispersions of conductive carbon are disclosed in which a cellulose derivative, a dispersant additive and a small amount of a low molecular weight amine are present. It has been found that the viscosity of these compositions is high and the viscosity of the composition tends to increase during storage. It is desirable to provide a composition with a lower viscosity, in particular to provide a composition with a limited viscosity increase during storage.

[0003] European patent application EP 3786110 A1 relates to a dispersion comprising carbon nanotubes, polyvinylpyrrolidone, N-methyl-2-pyrrolidone and an amino compound. The dispersion described in this document is not entirely satisfactory with regard to the sedimentation stability and volume resistivity of the resulting electrode material.

[0004] International patent application WO2020 / 173821A1 relates to a composition comprising a polymer having polymerized units of N-vinyllactam and a comb polymer, and to the use of the composition as a dispersant for carbon-based materials.

[0005] The present invention aims to provide a composition suitable for preparing electrodes for rechargeable batteries, which has a desirable low viscosity, good dispersion stability, and further provides desirable electrochemical properties for rechargeable batteries, especially low volume resistivity of the resulting electrode material.

[0006] The present invention provides a dispersant composition comprising

[0007] a) 30 to 80% by weight of at least one first polymer,

[0008] b) 10 to 60% by weight of at least one amine having a molecular weight of up to 250 g / mol, and

[0009] c) 5 to 20% by weight of at least one second polymer which is different from the first polymer,

[0010] The % by weight stated herein is based on the total weight of a), b) and c).

[0011] The dispersant composition according to the present invention is very suitable for use in a composition for preparing an electrode of a rechargeable battery. The composition for preparing an electrode has an ideal low viscosity, good dispersion stability, and further provides ideal electrochemical properties of a rechargeable battery, such as low volume resistivity of the resulting electrode material.

[0012] In a preferred embodiment, the dispersant composition comprises

[0013] a) 40 to 75% by weight of the at least one first polymer,

[0014] b) 15 to 55% by weight of the at least one amine having a molecular weight of up to 250 g / mol, and

[0015] c) 7 to 15 wt. % of at least one second polymer which is different from the first polymer.

[0016] When the amounts of the components in the dispersant composition are within these preferred ranges, the above advantages are achieved to a greater extent.

[0017] The dispersant composition comprises at least one first polymer. There is no particular restriction on the at least one polymer in terms of repeating units. Homopolymers are suitable, and copolymers comprising two or more different types of repeating units are also suitable. In a preferred embodiment, the repeating units comprise carbon atoms, and heteroatoms containing oxygen or nitrogen or oxygen and nitrogen.

[0018] Typically, the first polymer is selected from linear polymers having a linear polymer chain without polymer side chains or polymer branches.

[0019] In a preferred embodiment, the at least one first polymer comprises polymerized units of N-vinyl lactam. A polymerized unit refers to an N-vinyl lactam to which an ethylenically unsaturated vinyl group has been polymerized. Examples of suitable N-vinyl lactams may have 4-, 5-, 6- or 7-membered rings, also known as beta, gamma, delta or epsilon lactams. Preferred examples include N-vinyl pyrrolidone and N-vinyl caprolactam.

[0020] In one embodiment, the first polymer is a copolymer of N-vinyl lactam and other monomers having ethylenically unsaturated polymerizable groups. Examples of other monomers include acrylates and methacrylates, vinyl aromatic compounds and vinyl esters. In a preferred embodiment, the first polymer consists of at least 50% by weight, more preferably at least 80% by weight, of polymerized units of N-vinyl lactam.

[0021] In one embodiment, the first polymer comprises polymerized units of one type of N-vinyl lactam. In other embodiments, the first polymer comprises polymerized units of two or more different types of N-vinyl lactams. Preferably, the first polymer comprises or consists of polymerized units of N-vinyl pyrrolidone.

[0022] In other embodiments, the at least one first polymer comprises a vinyl polymer, such as polyvinyl butyral resin, polyvinyl caprolactam, polyvinyl pyrrolidone copolymers, such as polyvinyl pyrrolidone-co-vinyl acetate, butylated polyvinyl pyrrolidone such as Ganex TM P-904LC polymer, polyvinyl pyrrolidone-co-dimethylaminopropyl methacrylamide, polyvinyl pyrrolidone-co-dimethylaminoethyl methacrylate, maleimide copolymers such as isobutylene-ethylmaleimide-hydroxyethylmaleimide copolymer (Aquflex TM FX-64 product), poly(acrylonitrile-co-butadiene) or dicarboxyl terminated poly(acrylonitrile-co-butadiene).

[0023] In further embodiments, the at least one polymer comprises a polysaccharide or a modified polysaccharide. In some embodiments, the modified polysaccharide comprises at least one of an alkylated polysaccharide, a hydroxyalkylated polysaccharide, and an acetylated polysaccharide.

[0024] The expression alkylated polysaccharide or hydroxyalkylated polysaccharide is understood herein as a compound in which a hydroxyalkyl group or an alkyl group, preferably a hydroxyalkyl group, is attached to the polysaccharide moiety. The hydroxyalkyl group or the alkyl group, preferably the hydroxyalkyl group, can be attached to the polysaccharide moiety naturally or artificially, such as by means of chemical synthesis or enzymatic synthesis.

[0025] The polysaccharide portion may comprise any polysaccharide containing at least 5, preferably 10 monosaccharide monomers linked to each other by glycosidic bonds, for example by α and / or β glycosidic bonds. The polysaccharide portion may comprise a cellulose, an alkylcellulose, such as a C1-4 alkylcellulose, preferably methylcellulose, ethylcellulose or ethylmethylcellulose, an arabinoxylan, a chitin or a pectin portion.

[0026] The hydroxyalkyl of hydroxyalkylated polysaccharide can be straight chain or branched C1-10 hydroxyalkyl, preferably straight chain or branched C2-5 hydroxyalkyl. The hydroxyl of the hydroxyalkyl of hydroxyalkylated polysaccharide can be primary hydroxyl or secondary hydroxyl. The hydroxyalkyl can be connected to the polysaccharide part by ester bond, ether bond, amide bond or amino bond, preferably ether bond. Based on the hydroxyalkylation percentage of the potential free linking group of each polysaccharide, the hydroxyalkylated polysaccharide suitably has at least 80 mol % degree of hydroxyalkylation. Hydroxyalkylation is usually carried out by the reaction of the free hydroxyl of polysaccharide with alkylene oxide, preferably ethylene oxide or propylene oxide. When the polysaccharide is hydroxyalkylated with propylene oxide, the hydroxyalkylated polysaccharide usually contains 20 to 80 wt %, preferably 22 to 65 wt % of the reacted propylene oxide based on the weight of the hydroxylated polysaccharide.

[0027] The alkyl group of the alkylated polysaccharide can be a linear or branched C1-10 alkyl group, preferably a linear or branched C2-5 alkyl group. The alkyl group can be connected to the polysaccharide part through an ester bond, an ether bond, an amide bond or an amino bond, preferably an ether bond. The alkylated polysaccharide generally has a degree of alkylation of 30 to 100%, based on the alkylation percentage of the potential free linking groups of the respective polysaccharide.

[0028] The alkylated polysaccharide preferably comprises a cellulose or methylcellulose moiety. The terms cellulose and methylcellulose are well known to the person skilled in the art. The alkylated polysaccharide may be an alkylated cellulose or a methylcellulose.

[0029] The alkylated or hydroxyalkylated polysaccharide preferably contains at least 1, preferably 2, free alcohol groups per 5 monosaccharide monomer units. The alkylated or hydroxyalkylated polysaccharide preferably contains at least 2, preferably at least 3, more preferably at least 4 free alcohol groups per 10 monosaccharide monomer units.

[0030] The alkylated or hydroxyalkylated polysaccharide is preferably selected from hydroxypropyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, ethyl hydroxyethyl cellulose, methyl cellulose, ethyl cellulose, ethyl methyl cellulose and any mixture thereof. The acetylated polysaccharide may be cellulose acetate.

[0031] In a preferred embodiment, the at least one first polymer is selected from polyvinylpyrrolidone, modified cellulose or mixtures thereof. It is particularly preferred that the modified cellulose comprises hydroxymethylpropyl cellulose.

[0032] The molecular weight of the at least one first polymer is not particularly limited. In some embodiments, the weight average molecular weight of the first polymer is in the range of 2000 to 500000 g / mol, preferably in the range of 5000 to 100000 g / mol. It is particularly preferred that the first polymer has a weight average molecular weight in the range of 15000 to 80000 g / mol.

[0033] The weight average molecular weight may suitably be determined by gel permeation chromatography (GPC) using polymethyl methacrylate as a calibration standard and N,N-dimethylacetamide as an eluent.

[0034] As mentioned above, the dispersant composition of the present invention comprises at least one amine having a molecular weight of up to 250 g / mol. The amine can be a primary amine, a secondary amine or a tertiary amine, and does not include ammonia or a quaternary ammonium compound. In addition to monoamines, available amines include amido compounds with multiple amino groups in the molecule, such as diamines, triamines and tetramines. In addition to the above compounds, nitrogen-containing alicyclic heterocyclic compounds can also be used. Therefore, the amino group herein is a primary, secondary or tertiary functional group.

[0035] The amine used in the composition of the present invention is preferably at least one amine compound selected from aliphatic primary amines, aliphatic secondary amines, aliphatic tertiary amines and alkanolamines. The amine is more preferably at least one amine compound having only one amino group, selected from aliphatic primary amines, aliphatic secondary amines, aliphatic tertiary amines and alkanolamines.

[0036] The amine may be used alone or in combination of two or more amines, regardless of whether it is a commercially available product or a synthesized product.

[0037] Specific examples of suitable amines include, but are not limited to, aliphatic primary amines such as ethylamine, octylamine, stearylamine, aliphatic secondary amines such as diethylamine, dibutylamine, aliphatic tertiary amines such as triethylamine, dimethyloctylamine, dimethyldecylamine, dimethyllaurylamine, dimethylstearylamine, and alkanolamines such as dimethylaminoethanol, monoethanolamine, diethanolamine, methyldiethanolamine and triethanolamine, and nitrogen-containing alicyclic heterocyclic compounds such as hexamethylenetetramine, morpholine and piperidine.

[0038] The amine preferably has a carbon atom number of 2 or more and 20 or less, more preferably 2 or more and 15 or less, still more preferably 2 or more and 10 or less.

[0039] The number of amino groups contained in the amine is preferably 1 or more and 4 or less, more preferably 1 or more and 2 or less, particularly preferably 1 or 2.

[0040] In a further preferred embodiment, the at least one amine having a molecular weight of up to 250 g / mol has one amine group and one hydroxyl group.

[0041] It has been found that the presence of the at least one amine having a molecular weight of up to 250 g / mol in a specified amount is essential to achieve the desired properties of the dispersant composition, such as providing a composition having a desirable low and stable viscosity, good dispersion stability for preparing electrodes for rechargeable batteries.

[0042] The dispersant composition of the present invention further comprises at least one second polymer, which is different from the first polymer.

[0043] In some embodiments, the at least one second polymer is a fatty acid-modified polyether. The polyether is preferably a polyalkylene oxide based on polyethylene oxide, polypropylene oxide and mixtures thereof. In a typical embodiment, the polyether has 4 to 100 ether groups, preferably 5 to 50 ether groups. The fatty acid is typically a fatty acid with 12 to 24 carbon atoms. The fatty acid can be saturated or unsaturated. Unsaturated fatty acids are preferred. Typically, fatty acids are connected to the polyether via a connecting portion comprising an ester group or consisting of an ester group. In a preferred embodiment, the fatty acid-modified polyether comprises a terminal carboxylic acid group, which is optionally neutralized by an amine. The neutralizer amine preferably has a molecular weight higher than 250g / mol. Suitable neutralizer amines are aminoamides based on fatty acids and polyamines.

[0044] In a preferred embodiment, the at least one second polymer is selected from the group consisting of comb polymers, branched polymers, hyperbranched polymers and mixtures thereof.

[0045] Comb polymers are copolymers having at least two polymer side chains attached to a polymer backbone.

[0046] In some embodiments, the comb polymer in the composition of the present invention is a comb polymer having a polymer backbone based on a vinyl aromatic compound and an ethylenically unsaturated polymerizable carboxylic acid anhydride and having at least two polyalkylene oxide side chains.

[0047] The polymer backbone of the comb polymer is generally substantially linear, i.e. it is prepared by polymerization of ethylenically unsaturated polymerizable monomers having one ethylenically unsaturated polymerizable bond. If desired, there may be a small amount of branching in the polymer backbone, for example by including monomers having more than one ethylenically unsaturated polymerizable bond.

[0048] The polymer backbone of the comb polymer suitably comprises polymerized units of vinyl aromatic compounds. Examples of suitable vinyl aromatic compounds include styrene, vinyl toluene, vinyl xylene, vinyl ethylbenzene and mixtures thereof. The polymer backbone of the comb polymer further suitably comprises polymerized units of ethylenically unsaturated polymerizable carboxylic acid anhydride or ethylenically unsaturated polymerizable dicarboxylic acid. Examples of suitable monomers include maleic anhydride, itaconic anhydride, citraconic anhydride, fumaric acid, esters of the above compounds and mixtures thereof. The polymer backbone of the comb polymer can be suitably prepared by copolymerization of the above two types of monomers. If desired, other monomers, such as acrylic acid or methacrylic acid and esters thereof, may be included in the polymer backbone. In a preferred embodiment, the polymer backbone of the comb polymer is a copolymer of styrene and maleic anhydride.

[0049] In a preferred embodiment, the comb polymer has at least two polyalkylene oxide side chains connected to the polymer backbone. Comb copolymers generally have 2 to 100, preferably 2 to 50, more preferably 3 to 25, and most preferably 4 to 12 polyalkylene oxide side chains. Typically, the polyalkylene oxide side chains are polyethers based on polymerized units of epoxides or oxetanes. Typically, the polyalkylene oxide side chains are based on polymerized units of ethylene oxide, propylene oxide, butylene oxide, and mixtures thereof. In the case of mixtures of alkylene oxides, these may be present in the polyalkylene oxide chain in the form of two or more blocks or in random order. Polyalkylene oxide side chains based on ethylene oxide, propylene oxide, and in particular mixtures thereof are preferred.

[0050] The weight average molecular weight of the polyalkylene oxide side chains is typically in the range of 200 to 6000 g / mol, preferably 300 to 4000 g / mol. In some embodiments, the polyalkylene oxide side chains have ether end groups, for example alkyl ether end groups, such as ethyl or methyl ether end groups.

[0051] The polyoxyalkylene oxide side chains can be attached to the polymer backbone by reaction of monofunctional polyoxyalkylene oxides terminated with amines or alcohols with carboxylic anhydride groups of the polymer backbone. The reaction of primary amine groups with carboxylic anhydride groups can produce amide bonds or imide bonds. Preferably, the polyoxyalkylene oxide side chains of the comb copolymer b) are attached to the polymer backbone via amide groups or imide groups, for example by reaction of copolymers of styrene and maleic anhydride with polyether monoamines. Suitable polyether amines are available under the trade name M is available from Huntsman. In a further preferred embodiment, the polyalkylene oxide side chains are attached to the polymer backbone via ester bonds. This can be achieved by reacting the carboxylic anhydride groups of the polymer backbone with hydroxyl-terminated polyalkylene oxide monoethers.

[0052] In a preferred embodiment, the comb copolymer comprises additional functional groups comprising at least one of hydroxyl, carboxylic acid, carboxylate salt, tertiary amine, tertiary amine salt, and quaternary ammonium.

[0053] Hydroxyl groups can be introduced by reacting the carboxylic acid anhydride groups of the polymer backbone with an alkanolamine, such as ethanolamine.

[0054] The carboxylic acid group can be introduced by the ring-opening reaction of the carboxylic acid anhydride group of the polymer backbone with an alcohol or an amine. The carboxylic acid group can be neutralized with a base to form a salt of the carboxylic acid.

[0055] The comb copolymer b) suitably has an acid number in the range of 0 to 300 mg KOH / g. In a preferred embodiment, the acid number of the comb copolymer is in the range of 0 to 150 mg KOH / g, more preferably 0 to 100 mg KOH / g or 0 to 70 mg KOH / g.

[0056] Tertiary amine groups can be introduced by reacting the carboxylic anhydride groups of the polymer backbone with diamines having tertiary amine groups and primary or secondary amine groups, such as 3-dimethylaminopropylamine. The tertiary amine can be neutralized with an acid to form its salt. Alternatively, the tertiary amine can be quaternized with a quaternizing agent to form a quaternary ammonium group. Examples of suitable quaternizing agents include alkyl halides or benzyl halides, and epoxides combined with carboxylic acids. Comb copolymers comprising at least one of a tertiary amine, a tertiary amine salt and a quaternary ammonium are preferred.

[0057] The comb copolymer suitably has an amine value in the range of 0 to 300 mg KOH / g. In a preferred embodiment, the comb copolymer has an amine value in the range of 0 to 150 mg KOH / g, more preferably 0 to 100 mg KOH / g or 0 to 70 mg KOH / g.

[0058] The weight average molecular weight of the comb copolymer is suitably in the range of 4000 to 100000 g / mol, preferably in the range of 6000 to 60000 g / mol. The weight average molecular weight may be determined as described above for the at least one first polymer.

[0059] Examples of further suitable comb polymers and their preparation are described in detail in European patent application EP 2125910A.

[0060] In a preferred embodiment, the at least one second polymer comprises a comb polymer having a polymer backbone comprising polymerized units of styrene and maleic anhydride and side chains comprising ether groups.

[0061] It is further preferred that the at least one second polymer further comprises neutralized carboxylic acid groups.

[0062] In a further embodiment, the at least one second polymer is a polymer having a linear or substantially linear polymer backbone and having amide side groups. Typically, the polymer backbone is composed of polymerized units of monoethylenically unsaturated monomers. Examples of suitable monomers include alkyl acrylates, itaconates, maleates, (meth) acrylates, (meth) acrylic acid, styrene, alkyl vinyl ethers and vinyl esters, such as vinyl acetate. The amide side groups are typically present as alkylamides, arylamides, arylalkylamides or aminoalkylamides. In some embodiments, the amide side groups are generated by the amidation of the ester groups of the polymer with suitable amines, for example, with primary monoamines or with primary amines further having tertiary amine groups. Examples of suitable polymers having a linear or substantially linear polymer backbone and having amide side groups are described in US 6596816 B1.

[0063] The at least one second polymer may also be a branched or hyperbranched polymer. Mixtures of these polymers are also suitable.

[0064] In a preferred embodiment, branched or hyperbranched polymers are based on a polyamine core with multiple amine groups. Particularly preferably, the polyamine core is a polyalkylene imine, such as polyethyleneimine. The polyamine core is suitably connected to a plurality of polymer branches. The polymer branches suitably comprise polyether units or polyester units or a combination thereof. The polymer branches are connected to the polyamine core via a linking group. Examples of suitable linking groups include urea groups, urethane groups, ether groups and amide groups.

[0065] In one embodiment, such branched polymers can be obtained by reacting the following components:

[0066] a) one or more polyisocyanates containing uretdione groups and

[0067] b) one or more compounds of formula (I)

[0068] Y—(XH) n (I)

[0069] in

[0070] XH is an isocyanate-reactive group, and

[0071] Y is a monomeric or polymeric radical which is unreactive toward isocyanates and comprises one or more aliphatic, cycloaliphatic, araliphatic and / or aromatic groups, Y has a number-average molar mass of less than 20 000 g / mol, and n is 1, 2 or 3, and for at least 50 mol % of the compounds of the formula (I) in the case of n=1, with the proviso that substantially all free isocyanate groups of component a) are reacted with the compounds of the formula (I) to give an intermediate containing uretdione groups,

[0072] The uretdione group is then reacted with c)

[0073] c) one or more compounds of general formula (II)

[0074] Z—NHR (II)

[0075] wherein R is hydrogen or a straight-chain or branched alkyl group having 1 to 4 carbon atoms, and Z is an aliphatic, alicyclic and / or aromatic basic group,

[0076] And if desired, after this reaction, any reactive amino groups still present in the reaction product are reacted with an amino-reactive compound.

[0077] Examples of such branched polymers are described in more detail in US 8362300 B2.

[0078] In some embodiments, the branched polymer is based on a polyamine core having polymer branches with polyester segments, and wherein the branched polymer is further modified by reaction with an epoxy-functional compound. Preferably, the epoxy-functional compound comprises one epoxy group. The reaction with the epoxy-functional compound can be carried out before, during or after the polymer branches of the polyester segments are attached to the polyamine core.

[0079] Examples of such branched polymers are described in more detail in US 9574121.

[0080] The polymer branches of the polyester segments typically contain at least 3, preferably 4 to 50 ester groups. In some embodiments, the polyester segments additionally contain ether groups.

[0081] In a preferred embodiment, the polyester segments are linear caprolactone polyesters, each of which preferably has a weight average molecular weight of 500 to 10,000, preferably 800 to 8,000 g / mol.

[0082] Particularly suitable polyester segments are those obtainable by polycondensation of one or more optionally alkyl-substituted hydroxycarboxylic acids, such as ricinoleic acid or 12-hydroxystearic acid and / or ring-opening polymerization of the corresponding lactones, such as propiolactone, valerolactone and caprolactone. Particularly preferred are polyester segments based on ε-caprolactone, optionally in combination with δ-valerolactone.

[0083] Other suitable polyester segments are produced by reacting dicarboxylic acids and their esterifiable derivatives, such as anhydrides, acid chlorides or dialkyl esters, such as dimethyl esters or diethyl esters, with diols and monofunctional carboxylic acids. If necessary, the formation of dihydroxy polyesters can be suppressed by using corresponding stoichiometric amounts of monofunctional carboxylic acids. Examples of dicarboxylic acids that can be used in this way are succinic acid, maleic acid, fumaric acid, glutaric acid, adipic acid, sebacic acid, pimelic acid, phthalic acid or dimer fatty acids and their isomers, and their hydrogenation products. Examples of diols that can be used in this way are: ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, cis-1,2-cyclohexanedimethanol, trans-1,2-cyclohexanedimethanol and polyglycols based on ethylene glycol and / or propylene glycol. The corresponding monocarboxylic acids used as starting components preferably have 1 to 42 carbon atoms, in particular 4 to 18 carbon atoms, preferably 8 to 14 carbon atoms, and may be saturated or unsaturated, aliphatic or aromatic, linear, branched and / or cyclic. Examples of corresponding suitable monocarboxylic acids are stearic acid, isostearic acid, oleic acid, lauric acid and benzoic acid. Other suitable acids are tertiary monocarboxylic acids, also known as Koch acids, such as 2,2-dimethylpentanoic acid, tert-nonanoic acid and neodecanoic acid.

[0084] In a preferred embodiment, the dispersant composition of the present invention is liquid at a temperature of 20° C. In order to make the composition liquid, the dispersant composition preferably comprises an organic solvent. Typically, an organic solvent is selected that is capable of dissolving the essential components of the dispersant composition, i.e., the at least one first polymer, the at least one amine and the at least one second polymer. The organic solvent may also comprise more than one type of organic solvent, such as a mixture of two or more types of solvents. It is generally preferred that the solvent comprises an aprotic dipolar solvent, such as dimethyl sulfoxide, dimethylformamide or N-methylpyrrolidone, or other solvents comprising an amide group.

[0085] Typically, the organic solvent is present in the dispersant composition of the present invention in an amount of 10 to 90 weight percent, based on the total weight of the composition.

[0086] The dispersant composition of the present invention is very suitable as a dispersant for carbon-based materials. Therefore, in some embodiments, the composition of the present invention comprises a carbon-based material. A carbon-based material is a material composed of 90 to 100% by weight of carbon. In order to be used in the field of electrode manufacturing of a battery pack, a conductive carbon-based material is selected. Examples of suitable conductive carbon-based materials include carbon black, carbon nanotubes, graphite, carbon fiber, graphene, fullerene and mixtures thereof. Preferred carbon-based materials are carbon black, graphene and carbon nanotubes. The specific types of suitable carbon black are furnace black and acetylene black.

[0087] In a further embodiment, the dispersant composition of the present invention can be used as a dispersant for carbon-coated non-conductive electrode materials. An example of a non-conductive electrode material is LiFePO4 and other cathode materials used in lithium ion or lithium metal batteries for high power applications such as power tools, electric vehicles, and hybrid or plug-in hybrid vehicles. LiFePO4 suffers from low intrinsic rate performance, which is attributed to low electronic conductivity. One of the most promising approaches to overcome this problem is to add conductive carbon to the surface of the LiFePO4 particles.

[0088] The present invention also relates to the use of the dispersant composition of the present invention as a dispersant for conductive carbon-based materials.

[0089] In a further embodiment, the present invention relates to a method for preparing a dispersion of a conductive carbon-based material comprising

[0090] i) providing a conductive carbon-based material,

[0091] ii) providing a dispersant composition of the present invention,

[0092] iii) mixing the components provided in steps i) and ii) and applying shear force to prepare a dispersion.

[0093] The shearing forces can be provided by known apparatus for dispersing pigments, for example by a ball mill or by a high-speed stirrer.

[0094] Dispersions of carbon-based materials in which the composition of the present invention is used as a dispersant exhibit advantageous properties such as low viscosity and small particle size of the carbon-based material.

[0095] The dispersant composition of the present invention is very suitable for reducing the viscosity of the composition used to prepare the electrode of the rechargeable battery. In particular, the dispersant composition can be added to the composition used to prepare the electrode of the rechargeable battery, which leads to a significant decrease in the viscosity of the composition. This facilitates the handling of the composition without the need to add large amounts of viscosity reducing solvents.

[0096] The present invention therefore also relates to the use of the dispersant composition according to the invention for reducing the viscosity of a composition for producing an electrode for a rechargeable battery.

[0097] The dispersant composition of the present invention is very suitable for preparing materials for preparing electrodes for rechargeable batteries.

[0098] Therefore, the present invention also relates to a composition for preparing an electrode of a rechargeable battery, comprising

[0099] i) cathode active material,

[0100] ii) Conductive carbon-based materials,

[0101] iii) a polymer binder different from the polymer contained in the dispersant composition, and

[0102] iv) The dispersant composition of the present invention.

[0103] The expression "battery" encompasses a single electrochemical cell containing electrodes, separator and electrolyte, as well as a group of cells or an assembly of cells.

[0104] The term cathode refers to the electrode where reduction occurs during the discharge cycle.

[0105] Lithium-containing transition metal oxides or lithium metal phosphates, such as LiFePO4, are generally used as cathode active materials. It is preferred to use an oxide mainly containing lithium and at least one transition metal element selected from Ti, V, Cr, Mn, Fe, Co, Ni, Mo and W, which is a compound with a molar ratio of lithium to the transition metal element of 0.3 to 2.2. More preferably, an oxide mainly containing lithium and at least one transition metal element selected from V, Cr, Mn, Fe, Co and Ni is used, which is a compound with a molar ratio of lithium to the transition metal of 0.3 to 2.2. It should be noted that Al, Ga, In, Ge, Sn, Pb, Sb, Bi, Si, P, B, etc. can be contained in a range of less than 30 mol% relative to the main transition metal present. Among the active materials mentioned above, it is preferred to use at least one having the general formula Li x MO2 (M represents at least one of Co, Ni, Fe and Mn, and x is 0 to 1.2) or Li y A spinel structure material represented by N2O4 (N contains at least Mn, and y is 0 to 2).

[0106] Furthermore, as the cathode active material, at least one each including Li y M a D 1-a O2 materials (M represents at least one of Co, Ni, Fe and Mn, D represents at least one of Co, Ni, Fe, Mn, Al, Zn, Cu, Mo, Ag, W, Ga, In, Sn, Pb, Sb, Sr, B and P, provided that the element corresponding to M is excluded, y = 0 to 1.2, and a = 0.5 to 1) and each having a Li z (N b E 1-b )2O4 (N represents Mn, E represents at least one of Co, Ni, Fe, Mn, Al, Zn, Cu, Mo, Ag, W, Ga, In, Sn, Pb, Sb, Sr, B and P, b = 1 to 0.2, and z = 0 to 2) represents a spinel structure material.

[0107] Specifically, take Li x CoO2、Li x NiO2、Li x MnO2、Li x Co a Ni 1-a O2、Li x Co b V 1-b O z , Li x Co b Fe 1-b O2、Lix Mn2O4、Li x Mn c Co 2-c O4、Li x Mn c Ni 2-c O4、Li x Mn c V 2-c O4 and Li x Mn c Fe 2-c O4 (wherein x=0.02 to 1.2, a=0.1 to 0.9, b=0.8 to 0.98, c=1.6 to 1.96, and z=2.01 to 2.3). As the most preferred lithium-containing transition metal oxide, Li x CoO2、Li x NiO2、Li x MnO2、Li x Co a Ni 1-a O2、Li x Mn2O4 and Li x Co b V 1-b O z (x=0.02 to 1.2, a=0.1 to 0.9, b=0.9 to 0.98 and z=2.01 to 2.3) It should be noted that the value of x may increase and decrease with charging and discharging.

[0108] Although there is no particular limitation on the average particle size of the cathode active material, the particle size is preferably 0.1 to 50 μm. Preferably, the volume of particles of 0.5 to 30 μm is 95% or more. More preferably, the volume occupied by a particle group having a particle size of 3 μm or less is 18% or less of the total volume, and the volume occupied by a particle group having a particle size of 15 μm or more and 25 μm or less is 18% or less of the total volume.

[0109] Although the specific surface area is not particularly limited, the area measured by the BET method is preferably 0.01 to 50 m 2 / g, particularly preferably 0.2m 2 / g to 1m 2 / g.

[0110] The conductive carbon-based material in the composition for preparing the electrode suitably comprises at least one of carbon black, carbon nanotubes, graphite, carbon fiber, graphene and fullerene. Preferred carbon-based materials are carbon black, graphene and carbon nanotubes.

[0111] The composition for preparing the electrode further comprises a polymer binder different from the polymer contained in the dispersant composition. Examples of binders include known binders, such as: fluorine-based polymers, such as polyvinylidene fluoride and polytetrafluoroethylene; rubber-based binders, such as styrene-butadiene rubber (SBR) or acrylonitrile-butadiene rubber (NBR), and binders based on polyacrylates or their aqueous dispersions.

[0112] The binder is appropriately used in an amount of 1 to 50 parts by mass, and particularly, the amount is preferably approximately 1.5 to 20 parts by mass, relative to 100 parts by mass of the nonvolatile material of the composition.

[0113] The invention further relates to a method for producing a rechargeable battery electrode, wherein the battery electrode is produced using a composition for producing an electrode for a rechargeable battery.

[0114] The composition is suitably used in the form of a paste. The electrode paste can be obtained by kneading the components of the composition. Known devices such as a ribbon mixer, a screw-type kneader, a Spartan granulator, a Loedige mixer, a planetary mixer or a universal mixer can be used for kneading. The electrode paste can be formed into a sheet shape, a pellet shape, etc.

[0115] A solvent may be used during kneading. Examples of the solvent include known solvents such as dimethylformamide and isopropyl alcohol; in the case of a fluorine-based polymer, toluene and N-methylpyrrolidone; in the case of SBR, water. In the case of an adhesive using water as a solvent, a thickener is preferably used together. The amount of the solvent is adjusted to obtain a viscosity that allows the paste to be easily applied to the current collector.

[0116] The electrode can be formed by molding the electrode paste mentioned above. For example, the electrode is obtained by applying the electrode paste to a current collector, followed by drying and pressure molding.

[0117] Examples of current collectors include foils and meshes of aluminum, nickel, copper, stainless steel, etc. The coating thickness of the paste is generally 40 to 200 μm. There is no particular limitation on the paste coating method, and one example of the coating method includes a method involving coating with a doctor blade or a rod coater, followed by molding by roll pressing, etc.

[0118] Examples of pressure molding include roll molding, compression molding, etc. The pressure used for pressure molding is preferably about 1 to 3 t / cm 2 As the electrode density increases, the battery capacity per unit volume generally increases. However, if the electrode density increases too much, the cycle characteristics generally deteriorate. If the electrode paste in the preferred embodiment of the present invention is used, the cycle characteristics deteriorate little even if the electrode density is increased. Generally, the electrode density is between 1.0 and 4.0 g / cm 3In some embodiments, the electrode density of the cathode is between 2.0 and 3.5 g / cm 3 The density of the anode is between 1.2 and 2.0 g / cm 3 within the range. Example

[0119] Potassium carbonate: (Sigma-Aldrich)

[0120] (Dowanol)PMA:1-methoxy-2-propyl acetate (DOW Chemicals)

[0121] SMA 2000: Styrene-maleic anhydride copolymer (styrene / maleic anhydride molar ratio = 2 / 1) (Polyscope)

[0122] Jeffamine M 2070: Amine terminated EO / PO polyether (Huntsman)

[0123] Lutensol AO11: fatty alcohol (carbon number: 13-15) ethoxylate (polyethylene glycol repeating unit = 11) (BASF)

[0124] DMAPA: N,N-dimethylaminopropylamine (Huntsman)

[0125] Grilonit RV 1814: Alkyl (C13-15) glycidyl ether (EMS-GRILTECH)

[0126] Benzoic acid: (Sigma-Aldrich)

[0127] AMP: 95% 2-amino-2-methyl-propanol and 5% water (Sigma-Aldrich)

[0128] NMP: N-methylpyrrolidone (BASF)

[0129] Tetraisopropyl orthotitanate: (Thermo Fisher)

[0130] Benzenesulfonic acid, dodecyl-:(Akzo Nobel)

[0131] ε-Caprolactone:(BASF)

[0132] Lauric acid: (Merck KGaA)

[0133] Zirconium (IV) Butoxide Solution: (ABCR)

[0134] Polyimine 2000: 1,2-Ethylenediamine, polymer with aziridine (BASF)

[0135] Cardura E10: Neodecanoic acid, ethylene oxide methyl ester (Hexion)

[0136] MPEG 350: Poly(oxy-1,2-ethanediyl), α-methyl-ω-hydroxy-(Clariant)

[0137] δ-Valerolactone:(BASF)

[0138] Ethanol, 2-(dibutylamino)-:(BASF)

[0139] Breox B 35: Poly[oxy(methyl-1,2-ethanediyl)], α-butyl-w-hydroxy-(BASF)

[0140] Desmodur N 3400: Hexane 1,6-diisocyanate, homopolymer (Covestro)

[0141] DBTL: Dibutyltin dilaurate (Sigma Aldrich)

[0142] Epomin SP-003: N1-(2-aminoethyl)-1,2-ethylenediamine, polymer with aziridine (Sumitomo)

[0143] 2-Ethylhexyl acrylate:(Novasol)

[0144] Measurement of non-volatile matter content (solid content)

[0145] The sample (2.0±0.2 g of the test substance) is accurately weighed into a pre-dried aluminum pan and dried in a varnish drying cabinet at 150° C. for 20 minutes, cooled in a desiccator and then weighed again. The residue corresponds to the solids content in the sample (ISO 3251).

[0146] Measurement of amine value

[0147] 1.5 to 3.0 g of dispersant was accurately weighed into an 80 ml beaker and dissolved with 50 ml of acetic acid. The solution was neutralized and titrated with 0.1 mol / L HClO4 acetic acid solution using an automatic titration device equipped with a pH electrode. The inflection point of the titration pH curve was used as the titration endpoint, and the amine value (DIN 16945) was obtained by the following equation.

[0148] Amine value [mg KOH / g] = (561 × 0.1 × f × V) / (W × S)

[0149] (where f: coefficient of titrant, V: titration amount at the titration endpoint [mL], W: weighed amount of dispersant sample [g], S: solid matter concentration of dispersant sample [wt%])

[0150] Acid value measurement

[0151] 1.5 to 3.0 g of dispersant was accurately weighed into an 80 ml beaker and dissolved with 50 ml of ethanol. The solution was neutralized and titrated with a 0.1 mol / L ethanol KOH solution using an automatic titration device equipped with a pH electrode. The inflection point of the titration pH curve was used as the titration endpoint, and the acid value was obtained by the following equation (DIN EN ISO 2114).

[0152] Acid value [mg KOH / g] = (561 × 0.1 × f × V) / (W × S)

[0153] (where f: coefficient of titrant, V: titration amount at the titration endpoint [mL], W: weighed amount of dispersant sample [g], S: solid matter concentration of dispersant sample [wt%])

[0154] Gel Permeation Chromatography (GPC)

[0155] The weight average molecular weight Mw was determined at 40°C according to DIN 55672-1:2007-08 using a high pressure liquid chromatography pump (WATERS 600HPLC pump) and a refractive index detector (Waters 410). As separation columns, a combination of 3 Styragel columns from WATERS was used, with dimensions of 300 mm x 7.8 mm ID / column, a particle size of 5 μm and pore sizes HR4, HR2 and HR1. The eluent used was tetrahydrofuran containing 1% by volume of dibutylamine at an elution rate of 1 ml / min. Polystyrene standards were used for routine calibration.

[0156] Synthesis of Comb Copolymer C-1

[0157] 85 g of PMA was added to the reactor. 21 g of SMA 2000 was added during stirring while the mixture was heated to 70°C. Then, 64 g of Jeffamine M 2070 and 4 g of DMAPA were added dropwise to the reactor. The reaction was carried out at 170°C for 4 hours. PMA was distilled off during the reaction. The Mw of the polymer was 30210 g / mol.

[0158] In the next step, the reactor was cooled to 120° C. Then, 9 g of Grilonit RV 1814 and 4 g of benzoic acid were added to the reactor. The reaction was carried out at 120° C. for 4 hours. Thereafter, the comb copolymer C-1 was obtained.

[0159] The comb copolymer C-1 had a solids content of 100%, an amine value of 18 mg KOH / g and an acid value of 8 mg KOH / g.

[0160] Synthesis of Comb Copolymer C-2

[0161] 85 g of PMA were added to the reactor. 21 g of SMA 2000 were added during stirring while the mixture was heated to 70° C. After the addition of 0.4 g of potassium carbonate, 43 g of Lutensol AO11 were added dropwise and the reactor was heated to 140° C. for 4 hours.

[0162] In the next step, PMA was distilled off under reduced pressure at 150° C. After cooling to 80° C., 30 g of NMP were added to the reactor. After addition of 6 g of AMP followed by homogenization, comb copolymer C-3 was obtained.

[0163] The comb copolymer C-3 has a theoretical solid content of 70% (solvent: NMP), an amine value of 37 mg KOH / g and an acid value of 27 mg KOH / g. The Mw of the comb copolymer C-3 is 9600 g / mol.

[0164] Synthesis of Comb Copolymer C-3

[0165] The polyacrylates used for the aminolysis are prepared by generally known methods, such as by free-radical polymerization. More specialized production methods, such as anionic polymerization or group transfer polymerization are also possible.

[0166] 1450 grams of n-butyl polyacrylate (Mw about 12,000) was mixed with 177 grams of DMAPA. In addition, 0.5 grams of dodecylbenzene sulfonic acid was added as a catalyst. The reaction mixture was heated to reflux (about 180° C.) under nitrogen. Due to the n-butanol released during the reaction, the boiling point dropped to about 130° C. After about 15-17 hours, the reaction was complete and the released n-butanol was distilled off. At the same time, 35.32 grams of MPEG 350 were added. The reaction mixture was heated to 100° C. under nitrogen. Now 0.33 grams of tetraisopropyl orthotitanate were added and stirred at 200° C. for 2 hours. Then another 0.33 grams of tetraisopropyl orthotitanate were added and stirred at 200° C. for another 2 hours. The released n-butanol was distilled off. Then 0.17 grams of tetraisopropyl orthotitanate were added and stirred at 200° C. for 1 hour. The released n-butanol was distilled off.

[0167] The comb copolymer C-3 has a solid content of 100% and an amine value of 32 mg KOH / g. The Mw of the comb copolymer C-3 is 17000 g / mol.

[0168] Synthesis of branched polymer C-4

[0169] 25.6 g of lauric acid and 160.3 g of ε-caprolactone were mixed and heated to 100° C. under nitrogen with stirring. 0.1 g of zirconium (IV) butoxide solution was then added and further heated to 190° C. under nitrogen. Stirring was continued at this temperature until a solid content of >99% was reached. The reaction temperature was reduced to 100° C. 11.6 g of Polyimin 2000 and 2.4 g of Cardura E10 were added. The reaction mixture was heated to 140° C. for 5 hours. After cooling, branched polymer C-4 was obtained.

[0170] The branched polymer C-4 had a solid content of 100%. The amine value was 39 mg KOH / g, the acid value was 5 mg KOH / g, and the Mw of the branched polymer was 16000 g / mol.

[0171] Synthesis of branched polymer C-5

[0172] 13.21 g MPEG 350, 8.30 g ε-caprolactone and 4.87 g δ-valerolactone were mixed and heated to 160° C. under nitrogen with stirring. 0.04 g dodecylbenzenesulfonic acid was added and further heated to 160° C. under nitrogen. 0.02 g 2-(dibutylamino)-ethanol was then added and stirring was continued until a solid content of >97% was reached. The resulting monofunctional polyester was cooled to room temperature.

[0173] 105.69 g of Breox B 35 and 43.26 g of Desmodur N 3400 were combined with the monofunctional polyester obtained above. The mixture was heated to 80° C. and 0.01 g of DBTL was added. The reaction mixture was stirred until the NCO content was less than 0.1%. 5.44 g of 2-phenoxyethanol was then added and the mixture was homogenized. 11.26 g of Epomin SP-003 was added and the mixture was stirred until the amine value was 63% of the initial value. 7.93 g of 2-ethylhexyl 2-acrylate was added and the mixture was stirred for 1 hour. After cooling, branched polymer C-5 was obtained.

[0174] Branched polymer C-5 had a solid content of 100%, an amine value of 47 mg KOH / g, and a hydroxyl value of 34 mg KOH / g.

[0175] Preparation of dispersant compositions and comparative dispersant compositions

[0176] The polymers (C-1 to C-5), AMP or ethanolamine (EA) and hydroxypropylmethylcellulose (HPMC) or ethylcellulose (EC) stored in sealed boxes were dissolved in NMP in 140 ml glass bottles. Carbon nanotubes (CNT, FT 7320 produced by CNANO) and 150 grams of 2 mm zirconium oxide beads were then added. A paint shaking disperser DAS200 (LAU GmbH) was used to prepare the dispersion. The dispersion time was 12 hours at 30 ° C to obtain respective CNT dispersions D-1 to D-11 (details are described in Table 1).

[0177] Table 1

[0178]

[0179]

[0180] Comparative examples are marked with *

[0181] Preparation of compositions and comparative compositions for preparing electrodes for rechargeable batteries

[0182] The electrode material Li 1+x (Ni 0.5 Co 0.2 Mn 0.3 ) 1-x O2 (NCM), polyvinylidene fluoride (PVDF) as a binder and CNT dispersion as a conductive auxiliary agent were added to N-methyl-2-pyrrolidone. In the electrode material paste, the mass ratio was NCM:CNT:PVdF=97.5:0.5:2 based on non-volatile materials, and the components were mixed together to prepare an electrode material paste.

[0183] The electrode material paste is applied to the surface of 180 μm thick polyethylene terephthalate (PET) sheet to form a coating, and the coating is dried to form a cathode layer on the surface of the PET sheet. After that, this PET sheet with a cathode layer is cut into 3 cm width to measure the volume resistivity of the cathode layer. The viscosity of the CNT dispersion is measured by using BROOKFIELDVISCOMETER DV-II+, and the volume resistivity of the electrode coating is measured by a four-point measurement method using a low resistivity meter (Mitsubishi Chemical Corporation product, model: Loresta-AX) at 25 ° C. These are described in Table 2.

[0184] Table 2

[0185]

[0186] Comparative examples are marked with *

[0187] It can be inferred from Table 2 that the carbon nanotube dispersions prepared with the dispersant composition according to the invention exhibit significantly lower viscosity changes upon storage than the dispersions prepared with the comparative dispersant composition. The volume resistivity was at acceptable levels in all cases.

Claims

1. A dispersant composition comprising a) 30 to 80% by weight of at least one first polymer, b) 10 to 60% by weight of at least one amine having a molecular weight of up to 250 g / mol, and c) 5 to 20 wt. % of at least one second polymer which is different from the first polymer, wherein the wt. % is based on the total weight of a), b) and c).

2. The composition according to claim 1, wherein the composition comprises a) 40 to 75% by weight of the at least one first polymer, b) 15 to 55% by weight of the at least one amine having a molecular weight of up to 250 g / mol, and c) 7 to 15 wt. % of the at least one second polymer which is different from the first polymer.

3. The composition according to claim 1 or 2, wherein the at least one first polymer is selected from linear polymers having a linear polymer chain without polymer side chains or polymer branches.

4. The composition according to claim 3, wherein the at least one first polymer is selected from polyvinyl pyrrolidone, modified cellulose or mixtures thereof.

5. The composition of claim 4, wherein the modified cellulose comprises hydroxymethylpropyl cellulose.

6. The composition according to any one of the preceding claims, wherein the at least one amine having a molecular weight of up to 250 g / mol has one amine group and one hydroxyl group.

7. The composition according to any one of the preceding claims, wherein the at least one second polymer is selected from comb polymers, branched polymers, hyperbranched polymers and mixtures thereof.

8. The composition of claim 7, wherein the at least one second polymer comprises a comb polymer having a polymer backbone comprising polymerized units of styrene and maleic anhydride and side chains comprising ether groups.

9. The composition of claim 8, wherein the at least one second polymer further comprises neutralized carboxylic acid groups.

10. The composition according to any one of the preceding claims, wherein the composition further comprises at least one organic solvent in an amount of 10 to 90 wt. %, based on the total weight of the composition.

11. The composition of claim 10, wherein the at least one organic solvent comprises an amide group.

12. The composition according to any one of the preceding claims, wherein the composition further comprises a conductive carbon-based material.

13. The composition of claim 12, wherein the conductive carbon-based material comprises at least one of carbon black, carbon nanotubes, graphite, carbon fibers, graphene, and fullerene.

14. Use of the composition according to any one of the preceding claims 1 to 11 as a dispersant for conductive carbon-based materials.

15. Use of a composition according to any one of the preceding claims 1 to 11 for reducing the viscosity of a composition for the preparation of an electrode for a rechargeable battery.

16. A composition for preparing an electrode of a rechargeable battery, comprising i) cathode active material, ii) Conductive carbon-based materials, iii) a polymer binder different from the polymer comprised in the composition according to any one of the preceding claims 1 to 11, and iv) A composition according to any one of the preceding claims 1 to 11.

17. A method for preparing a dispersion of a conductive carbon-based material, comprising i) providing a conductive carbon-based material, ii) providing a composition according to any one of the preceding claims 1 to 11, iii) mixing the components provided in steps i) and ii) and applying shear force to prepare a dispersion.

18. A method for preparing a rechargeable battery electrode, wherein the battery electrode is prepared using the composition according to claim 12 or 16.