Composite conductive agent, preparation method thereof, secondary battery and electric device
Patent Information
- Application Number
- CN202280094475.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-01
- Publication Date
- 2024-11-12
AI Technical Summary
Existing lithium-ion batteries have problems with low cycle life during cycling, which causes cell expansion and pole piece rebound, affecting the energy density and dynamic performance of the battery.
A composite conductive agent is used. The conductive agent is composed of organic polymers and hydroxylated carbon nanotubes. It is combined with ester groups and hydrogen bonds to form a linear polymer structure, which enhances the binding effect of the particulate matter on the counter electrode and reduces the expansion of the battery core. force and improve electrical conductivity.
It effectively improves the cycle life of the battery core and the flexibility of the pole piece, reduces the expansion force of the battery core, and improves the dynamic performance and processability of the battery.
Smart Images

Figure CN118946986A_ABST
Abstract
Description
Composite conductive agent and preparation method thereof, secondary battery and electrical device Technical Field
[0001] The present application belongs to the field of electrochemical technology, and in particular relates to a composite conductive agent and a preparation method thereof, a secondary battery, and an electrical device. Background Art
[0002] In recent years, the application of secondary batteries, represented by lithium-ion batteries, has become increasingly widespread. They are widely used in energy storage systems such as hydropower, thermal, wind, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. With the rapid development of secondary batteries, higher requirements have been placed on their energy density, cycle performance, and safety performance. However, current secondary batteries, represented by traditional lithium-ion batteries, generally suffer from a short cycle life due to phenomena such as cell expansion during cycling, making them unable to meet practical application requirements.
[0003] Summary of the Invention
[0004] The purpose of this application is to provide a composite conductive agent and a preparation method thereof, a secondary battery and an electrical device, which can improve the cycle life of the secondary battery.
[0005] In order to achieve the above-mentioned purpose of the invention, the first aspect of the present application provides a composite conductive agent, comprising: an organic polymer; and hydroxylated carbon nanotubes combined with the organic polymer, wherein the organic polymer comprises a polymer having the structural formula shown in formula (1),
[0006]
[0007] In formula (1), m is an integer from 2500 to 20000, and R1 is a polymer structure containing an ester group and a nitrile group.
[0008] In the embodiment of the present application, the composite conductive agent includes an organic polymer and hydroxylated carbon nanotubes combined with the organic polymer, wherein the organic polymer includes a linear polymer structure of the structural formula shown in the above formula (1), and the hydroxylated carbon nanotubes are also linear structures. The composite conductive agent formed by combining the two can fully realize linear polymerization. Therefore, when the composite conductive agent is used as an additive for preparing electrode slurry, compared with traditional acrylic binders, the composite conductive agent can give full play to the coating effect of linear polymerization, enhance the bonding and binding effect on other particulate matter (for example, silicon-based active material particles) in the slurry, improve the inhibitory effect on the volume expansion of other particulate matter (especially silicon-based active material particles) during the cycle process, reduce the rebound of the electrode, reduce the expansion force during the cycle of the battery cell, and improve the cycle life of the battery cell.
[0009] In some embodiments of the present application, the polymeric structure includes a polymeric structure represented by formula (2),
[0010]
[0011] In formula (2), ** represents the connection site of the polymer structure, p is an integer from 1000 to 5000, q is an integer from 1000 to 15000, f is an integer from 500 to 4000, 2≤n≤200, each R2 is independently selected from and One of the following, * indicates the connection site of R2, M + Selected from Na + , K + 、Li + and NH4 + One of them.
[0012] Compared with traditional single-type monomer linear polymers, the composite conductive agent of the present application has a linear structure of molecular chains containing more side chains composed of a variety of different functional groups. These side chains can reduce the brittleness of the composite conductive agent and enhance its flexibility, thereby enhancing the flexibility of the electrode. Therefore, after cold pressing at a high compaction density, the ductility of the electrode can be improved, which can effectively reduce the occurrence of edge overvoltage. At the same time, it can also improve the phenomenon that the electrode under high density is prone to brittle fracture during subsequent processing, thereby improving the processability of the electrode.
[0013] In some embodiments of the present application, the composite conductive agent satisfies at least one of the following conditions:
[0014] (1) The hydroxylated carbon nanotubes are bonded to the organic polymer via ester groups and / or hydrogen bonds; alternatively, the hydroxylated carbon nanotubes are bonded to the organic polymer via ester groups;
[0015] (2) The surface of the hydroxylated carbon nanotube is connected with at least one hydroxyl group.
[0016] After the ester groups are formed between the hydroxylated carbon nanotubes and the organic polymers, the carboxyl functional groups in the organic polymers can be reduced, thereby reducing the hydrogen bonding effect between the molecules on the long polymer chains, effectively reducing the mutual agglomeration between the long polymer chains, improving the dispersion uniformity in the slurry, reducing the electrode resistance, and thus improving the dynamic performance of the battery cell.
[0017] In some embodiments of the present application, the composite conductive agent satisfies at least one of the following conditions:
[0018] (1) In the composite conductive agent, the mass percentage of the organic polymer is 50% to 90%, and optionally 65% to 80%;
[0019] (2) In the composite conductive agent, the mass percentage of the hydroxylated carbon nanotubes is 10% to 50%, and optionally 20% to 35%; and
[0020] (3) The hydroxylated carbon nanotubes include hydroxylated single-walled carbon nanotubes and / or hydroxylated multi-walled carbon nanotubes.
[0021] The appropriate mass percentage of the organic polymer in the composite conductive agent not only provides the composite conductive agent with sufficient linear polymeric structure, ensuring full performance of the organic polymer, improving the cycle life of the battery cell and the processability of the electrode, but also ensures that the composite conductive agent has high electrical conductivity. The appropriate mass percentage of hydroxylated carbon nanotubes in the composite conductive agent not only ensures high electrical conductivity, but also allows a sufficient number of ester groups to form between the organic polymer and the hydroxylated carbon nanotubes, effectively reducing the carboxyl functional groups in the organic polymer, reducing agglomeration between long polymer chains due to hydrogen bonding, improving dispersion uniformity, and enhancing the dynamic performance of the battery cell.
[0022] A second aspect of the present application provides a method for preparing a composite conductive agent, comprising:
[0023] reacting acrylate with acrylic acid and hydroxylated carbon nanotubes to obtain a pre-reacted mixture; and
[0024] The pre-reacted mixture is polymerized with acrylonitrile and acrylic polyether polyol monoester to form an organic polymer combined with the hydroxylated carbon nanotubes to obtain a composite conductive agent, wherein the composite conductive agent includes the organic polymer and the hydroxylated carbon nanotubes, and the organic polymer includes a polymer having a structure represented by formula (1).
[0025]
[0026] In formula (1), m is an integer from 2500 to 20000, and R1 is a polymer structure containing an ester group and a nitrile group.
[0027] In the method provided in the present application, acrylate is first pre-reacted with acrylic acid and hydroxylated carbon nanotubes to achieve pre-polymerization of acrylate, acrylic acid and hydroxylated carbon nanotubes, so that part of acrylate and acrylic acid form oligomers through pre-polymerization, and at the same time, part of hydroxylated carbon nanotubes are grafted onto the oligomers through esterification reaction to obtain a pre-reacted mixture; then the pre-reacted mixture is polymerized with acrylonitrile and acrylic acid polyether polyol monoester to achieve linear polymerization of the pre-reacted mixture, acrylonitrile and acrylic acid polyether polyol monoester to form an organic polymer including the structural formula shown in formula (1), and more hydroxylated carbon nanotubes are grafted onto the organic polymer through esterification reaction, thereby combining with the organic polymer to obtain a composite conductive agent. Among them, polyacrylic acid and polyacrylonitrile formed after the polymerization of acrylic acid and acrylonitrile both have good bonding effects. The polymerization of the two can play a reinforcing role, which is conducive to fully exerting the coating effect of the composite conductive agent, enhancing the bonding and binding effect on other particulate matter in the slurry (for example, silicon-based active material particles), improving the inhibitory effect on the volume expansion of other particulate matter (especially silicon-based active material particles) during the cycle process, reducing the rebound of the electrode, reducing the expansion force during the cycle of the battery cell, and improving the cycle life of the battery cell.
[0028] In some embodiments of the present application, the step of reacting acrylate with acrylic acid and hydroxylated carbon nanotubes comprises:
[0029] Under the action of a polymerization aid, the acrylate, the acrylic acid and the hydroxylated carbon nanotubes are contacted and reacted.
[0030] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0031] (1) the acrylate comprises at least one of sodium acrylate, potassium acrylate, lithium acrylate and ammonium acrylate; and
[0032] (2) The polymerization aid includes sodium lauryl sulfonate and / or sodium lauryl sulfate.
[0033] While acting as a surfactant, the polymerization aid can also break the hydrogen bonds within and between molecules, which is beneficial to promoting the prepolymerization reaction.
[0034] In some embodiments of the present application, the step of allowing the acrylate, the acrylic acid, and the hydroxylated carbon nanotubes to contact and react under the action of a polymerization aid comprises:
[0035] contacting and mixing the polymerization aid, the acrylate, the acrylic acid, and the hydroxylated carbon nanotubes in water to form a first mixed solution; and
[0036] The first mixed liquid is subjected to a first heat treatment to cause a prepolymerization reaction between the acrylate, the acrylic acid and the hydroxylated carbon nanotubes.
[0037] After the first mixed liquid consisting of the polymerization aid, acrylate, acrylic acid and hydroxylated carbon nanotubes is subjected to the first heat treatment, part of the acrylate and acrylic acid can be prepolymerized to form oligomers, and at the same time, part of the hydroxylated carbon nanotubes can be grafted onto the oligomers through an esterification reaction to obtain a pre-reacted mixture.
[0038] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0039] (1) In the first mixed solution, the mass percentage of the acrylate is 3% to 25%, and can be optionally 5% to 15%;
[0040] (2) In the first mixed solution, the mass percentage of the acrylic acid is 5% to 40%, and can be optionally 15% to 25%;
[0041] (3) In the first mixed solution, the mass percentage of the hydroxylated carbon nanotubes is 1% to 10%, and can be optionally 3% to 7%;
[0042] (4) In the first mixed solution, the mass percentage of the polymerization aid is 2% to 5%, and optionally 3% to 4.5%; and
[0043] (5) The temperature of the first heat treatment is 50°C to 85°C, and can be optionally 65°C to 80°C.
[0044] The mass percentage of each component in the first mixed liquid is within an appropriate range, which not only makes the composite conductive agent have higher adhesion, but also improves the dispersion uniformity and improves the dynamic performance of the battery cell.
[0045] In some embodiments of the present application, the polymerizing the pre-reacted mixture with acrylonitrile and acrylic polyether polyol monoester comprises:
[0046] Under the action of a polymerization initiator, the pre-reacted mixture is brought into contact with the acrylonitrile and the acrylic polyether polyol monoester and polymerized to form the polymer structure, wherein the polymer structure includes a polymer structure represented by formula (2).
[0047]
[0048] In formula (2), ** represents the connection site of the polymer structure, p is an integer from 1000 to 5000, q is an integer from 1000 to 15000, f is an integer from 500 to 4000, 2≤n≤200, each R2 is independently selected from and One of the following, * indicates the connection site of R2, M + Selected from Na + , K + 、Li + and NH4 + One of them.
[0049] The polymerization under the action of a polymerization initiator is conducive to initiating and promoting the polymerization reaction, forming the polymer structure of the above formula (2) to obtain an organic polymer.
[0050] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0051] (1) the acrylic acid polyether polyol monoester comprises at least one of acrylic acid polyethylene glycol monoester, acrylic acid polypropylene glycol monoester and acrylic acid polytetramethylene glycol monoester; and
[0052] (2) The polymerization initiator includes at least one of potassium sulfate, potassium persulfate and sodium persulfate.
[0053] Selecting a suitable type of acrylic acid polyether polyol monoester can promote the polymerization reaction and obtain the polymerization structure of polyacrylic acid polyether polyol monoester in the organic polymer.
[0054] In some embodiments of the present application, the step of contacting and polymerizing the pre-reacted mixture with the acrylonitrile and the acrylic polyether polyol monoester under the action of a polymerization initiator comprises:
[0055] contacting and mixing the polymerization initiator, the acrylonitrile, and the acrylic polyether polyol monoester in the solution of the pre-reacted mixture to obtain a second mixed solution; and
[0056] The second mixed liquid is subjected to a second heat treatment to cause a polymerization reaction between the acrylonitrile, the acrylic polyether polyol monoester and the pre-reacted mixture.
[0057] The pre-reacted mixture is polymerized with acrylonitrile and acrylic polyether polyol monoester to achieve linear polymerization of the pre-reacted mixture, acrylonitrile and acrylic polyether polyol monoester to form an organic polymer, and more hydroxylated carbon nanotubes are grafted onto the organic polymer through esterification reaction, thereby combining with the organic polymer to obtain a composite conductive agent.
[0058] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0059] (1) In the second mixed solution, the mass percentage of the polymerization initiator is 1% to 3%, and can be optionally 2% to 2.5%;
[0060] (2) In the second mixed liquid, the mass percentage of acrylonitrile is 5% to 30%, and can be optionally 10% to 20%;
[0061] (3) In the second mixed solution, the mass percentage of the acrylic polyether polyol monoester is 10% to 40%, and optionally 20% to 35%; and
[0062] (4) The temperature of the second heat treatment is 50°C to 85°C, and can be optionally 70°C to 80°C.
[0063] The mass percentage of acrylic acid polyether polyol monoester in the second mixed liquid is controlled within an appropriate range, which is conducive to the formation of organic polymers and obtaining a polyacrylic acid polyether polyol monoester polymerization structure with a corresponding degree of polymerization in the organic polymer. This can not only make the electrode have better flexibility, prevent brittle fracture, and withstand deformation during processing, but also withstand deformation caused by volume changes during battery cycling, thereby improving service life.
[0064] In some embodiments of the present application, the step of preparing the acrylic polyether polyol monoester is further included:
[0065] Acrylic acid is brought into contact with polyether polyol to undergo an esterification reaction, thereby obtaining the acrylic acid polyether polyol monoester.
[0066] Acrylic acid and polyether polyol monoester are reacted to form acrylic acid polyether polyol monoester, wherein the ether bond contained in the acrylic acid polyether polyol monoester can effectively enhance the flexibility of the composite conductive agent in the final composite conductive agent, thereby enhancing the flexibility of the electrode and improving the processability of the electrode.
[0067] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0068] (1) the polyether polyol comprises at least one of polyethylene glycol, polypropylene glycol and polytetramethylene glycol; and
[0069] (2) The degree of polymerization of the polyether polyol is 2 to 200, and can be optionally 50 to 150.
[0070] The degree of polymerization of polyether polyols is mainly reflected in the length of the side chain. A suitable degree of polymerization can improve the problem of brittle electrodes caused by the linear structure of the main chain, but too long a degree of polymerization can easily lead to problems such as decreased adhesion and slurry processing.
[0071] In some embodiments of the present application, the step of contacting acrylic acid with polyether polyol and causing an esterification reaction comprises:
[0072] contacting and mixing the acrylic acid and the polyether polyol in water to form a third mixed solution; and
[0073] The third mixed liquid is subjected to a third heat treatment to obtain the acrylic polyether polyol monoester solution.
[0074] In the above steps, acrylic acid and polyether polyol can undergo esterification reaction under the action of a catalyst and a polymerization inhibitor. The esterification reaction can link the carboxyl group in acrylic acid with the hydroxyl group in polyether polyol to form acrylic acid polyether polyol monoester.
[0075] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0076] (1) the molar ratio of the acrylic acid to the polyether polyol is (5:1) to (1:1), and optionally (1.5:1) to (2.5:1); and
[0077] (2) The temperature of the third heat treatment is 50°C to 85°C, and can be optionally 65°C to 80°C.
[0078] The molar ratio of acrylic acid to polyether polyol is controlled within a suitable range, which is conducive to the occurrence of esterification reaction, thereby obtaining the target product, acrylic acid polyether polyol monoester.
[0079] In some embodiments of the present application, before the third mixed liquid is subjected to the third heat treatment, the method further comprises:
[0080] adding a catalyst and a polymerization inhibitor to the third mixed liquid;
[0081] Optionally, the catalyst comprises at least one of p-toluenesulfonic acid, sulfuric acid and aluminum oxide; and
[0082] Optionally, the polymerization inhibitor includes at least one of hydroquinone, p-hydroxyanisole and 2,6-di-tert-butyl-p-cresol.
[0083] A suitable type of catalyst can play a better catalytic role in the esterification reaction and increase the reaction rate; a suitable type of polymerization inhibitor can play a role in preventing the polymerization of acrylic acid monomers in the esterification reaction.
[0084] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0085] (1) In the third mixed solution, the mass percentage of the catalyst is 3% to 10%, and optionally 5% to 9%; and
[0086] (2) In the third mixed liquid, the mass percentage of the polymerization inhibitor is 1% to 5%, and can be optionally 3% to 4.5%.
[0087] The mass percentage of the catalyst in the third mixed solution is within an appropriate range, which can make the catalyst play a better catalytic promoting role. The mass percentage of the polymerization inhibitor in the third mixed solution is within an appropriate range, which can make the polymerization inhibitor play a better role in preventing the polymerization of acrylic acid monomers.
[0088] In some embodiments of the present application, after the third mixed liquid is subjected to the third heat treatment, the method further comprises:
[0089] The solution of the acrylic acid polyether polyol monoester is purified to obtain the acrylic acid polyether polyol monoester.
[0090] Purification treatment of the acrylic acid polyether polyol monoester solution can remove impurities in the reaction and obtain the target product acrylic acid polyether polyol monoester.
[0091] In some embodiments of the present application, the step of preparing the acrylate is further included:
[0092] Acrylic acid is contacted with an alkaline reagent to react to obtain the acrylic acid salt.
[0093] Acrylates are obtained by reacting acrylic acid with an alkaline reagent to salify the acrylic acid. Salinizing the carboxylic acid functional groups in acrylic acid reduces hydrogen bonding on the polyacrylate molecular chains during the subsequent polymerization process, weakening the mutual agglomeration between the molecular chains. This allows the resulting conductive adhesive to be evenly dispersed in the slurry, thereby improving the dynamic performance of the battery cell.
[0094] In some embodiments of the present application, the step of allowing acrylic acid to contact with an alkaline reagent comprises:
[0095] Adding an alkaline agent to a solution of acrylic acid to adjust the pH value of the solution to 7 to 8, thereby obtaining a solution of the acrylic acid salt; and
[0096] The acrylate solution is subjected to distillation and drying treatment.
[0097] By controlling the pH value of the solution, the amount of the reactants acrylic acid and alkaline reagent can be indirectly controlled. By controlling the amount of the reactants within a suitable range, the salification reaction is facilitated, thereby obtaining the target product acrylate.
[0098] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0099] (1) the alkaline reagent comprises at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide and ammonia water; and
[0100] (2) The acrylate includes at least one of sodium acrylate, potassium acrylate, lithium acrylate and ammonium acrylate.
[0101] Acrylates can achieve polymerization in the subsequent process and obtain a polymeric structure of polyacrylate in the organic polymer; alkaline reagents can salt acrylic acid and thus reduce the carboxyl groups contained in acrylic acid.
[0102] The third aspect of the present application provides a secondary battery, comprising the composite conductive agent described in the first aspect of the present application or the composite conductive agent prepared by the method described in the second aspect of the present application.
[0103] A fourth aspect of the present application provides an electrical device comprising the secondary battery described in the third aspect of the present application.
[0104] The electric device of the present application includes the secondary battery provided by the present application, and thus has at least the same advantages as the secondary battery.
[0105] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0106] FIG1 is a schematic diagram of an embodiment of a secondary battery of the present application.
[0107] FIG2 is an exploded schematic diagram of an embodiment of a secondary battery of the present application.
[0108] FIG3 is a schematic diagram of another embodiment of the secondary battery of the present application.
[0109] FIG. 4 is a schematic diagram of another embodiment of the secondary battery of the present application.
[0110] FIG. 5 is an exploded view of FIG. 4 .
[0111] FIG6 is a schematic diagram of an embodiment of an electric device using a secondary battery as a power source according to the present application. DETAILED DESCRIPTION
[0112] To make the purpose, technical solutions, and advantages of this application more clear, the technical solutions of this application will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of this application, rather than all the embodiments. The relevant embodiments described herein are illustrative and are used to provide a basic understanding of this application. The embodiments of this application should not be interpreted as limiting this application.
[0113] For the sake of clarity, only some numerical ranges are specifically disclosed herein. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.
[0114] In the description herein, unless otherwise specified, “above” and “below” include the number itself.
[0115] Unless otherwise specified, the terms used in this application have the commonly understood meanings commonly understood by those skilled in the art. Unless otherwise specified, the numerical values of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).
[0116] A list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.
[0117] To meet market demand, the energy density of secondary batteries, particularly lithium-ion batteries, is increasing. Consequently, battery cell design requires electrodes with high coating surface density and high compaction density. Furthermore, to increase energy density, silicon-based materials are being introduced as active materials in secondary batteries. The inventors discovered during their research that silicon-based materials expand in volume during the cycling of secondary batteries. This, coupled with the high coating surface density and high compaction density, leads to a continuous accumulation of electrode rebound in the direction perpendicular to the plane (the Z direction). This can affect the amount of active material entering the battery shell in the short term, thereby impacting the battery capacity. In the long term, this electrode rebound can cause excessive cell expansion, impacting the battery's cycle life.
[0118] In addition, traditional secondary batteries, represented by lithium-ion batteries, generally use organic polymers as binders. Among them, polyacrylic acid polymers, as a single type of monomer linear polymer, are more widely used in secondary batteries due to their high adhesion and chemical stability compared to other types of binders. However, the inventors found during the research process that although the overall performance of polyacrylic acid polymers is better than other similar binders, when polyacrylic acid polymers are used alone as binders, the long polymer chains will agglomerate with each other due to the hydrogen bonding between molecules on the long polymer chains, making it difficult to effectively disperse the binder in the slurry, ultimately leading to an increase in electrode resistance, an increase in the DC resistance (DCR) of the battery cell, and lithium precipitation, and a deterioration in its kinetic performance.
[0119] In addition, the inventors also found that although polyacrylic acid polymers have excellent bonding properties, their conductivity is poor; and this single type of monomer linear polymer is generally brittle due to the relatively simple types of functional groups, and in the slurry, it usually contacts other particulate matter in the slurry in the form of a mesh surface contact. After the above slurry is coated on the current collector to form a pole piece, the linear structure of the polyacrylic acid polymer molecular chain will make the pole piece insufficiently flexible. After cold pressing at a high compaction density, the pole piece will have insufficient ductility, and stress will easily concentrate at the edge of the coating area, thereby causing edge overpressure. At the same time, the pole piece under high density is prone to brittle fracture during subsequent processing, resulting in poor machinability of the pole piece.
[0120] Furthermore, in the pursuit of high energy and power density in secondary batteries, particularly lithium-ion batteries, linear CNTs (carbon nanotubes) have become a key additive in positive and negative electrode slurry formulations due to their high conductivity. However, the inventors discovered that during the preparation of slurries containing linear CNTs, crosslinking can cause the CNTs to entangle within the slurry, leading to uneven dispersion and even gelation, thus affecting the processability of the electrode.
[0121] In order to solve the above problems, the inventors started from the aspects of linear polymer binders and linear CNT conductive agents, and through extensive research, proposed a composite conductive agent, including an organic polymer and a hydroxylated carbon nanotube combined with the organic polymer. The composite conductive agent can form a product of an organic polymer and a hydroxylated CNT (carbon nanotube) composite by combining the organic polymer with the hydroxylated carbon nanotube. During the slurry processing, the long-chain molecules of the organic polymer can be suspended in the aqueous solution, which has the effect of stabilizing other particulate matter in the slurry, thereby enhancing the thickening and stabilizing effect of the composite conductive agent, improving the distribution state of the hydroxylated CNT in the slurry, and improving the dispersion uniformity. At the same time, after combining the organic polymer with the hydroxylated CNT, the high conductivity of the hydroxylated CNT can also improve the conductive properties of the organic polymer, thereby obtaining a composite conductive agent composite product with better comprehensive performance. In addition, the organic polymer and hydroxylated CNT in the composite conductive agent also fully realize linear polymerization, thereby giving full play to the coating effect of linear polymerization, enhancing the coating effect of the composite conductive agent in the slurry on other particulate matter, improving the inhibitory effect on the expansion of silicon-based materials during the cycle, reducing the rebound of the electrode, reducing the expansion force during the cycle of the battery cell, and improving the cycle life of the battery cell.
[0122] Composite conductive agent
[0123] A first aspect of the embodiments of the present application provides a composite conductive agent, comprising an organic polymer and hydroxylated carbon nanotubes combined with the organic polymer, wherein the organic polymer comprises a polymer having the structural formula shown in formula (1),
[0124]
[0125] In formula (1), m is an integer from 2500 to 20000, and R1 is a polymer structure containing an ester group and a nitrile group.
[0126] In the embodiment of the present application, the composite conductive agent includes an organic polymer and hydroxylated carbon nanotubes combined with the organic polymer, wherein the organic polymer includes a linear polymer structure of the structural formula shown in the above formula (1), and the hydroxylated carbon nanotubes are also linear structures. The composite conductive agent formed by combining the two can fully realize linear polymerization. Therefore, when the composite conductive agent is used as an additive for preparing electrode slurry, compared with traditional acrylic binders, the composite conductive agent can give full play to the coating effect of linear polymerization, enhance the bonding and binding effect on other particulate matter (for example, silicon-based active material particles) in the slurry, improve the inhibitory effect on the volume expansion of other particulate matter (especially silicon-based active material particles) during the cycle process, reduce the rebound of the electrode, reduce the expansion force during the cycle of the battery cell, and improve the cycle life of the battery cell.
[0127] In addition, since the composite conductive agent contains organic polymers, and the organic polymer can play a good thickening and stabilizing role in the slurry, its long-chain molecules can be suspended in the aqueous solution, playing a role in stabilizing other particulate matter in the slurry. Therefore, compared with traditional linear CNTs (carbon nanotubes), the composite conductive agent can promote the stabilizing effect of the organic polymer on the linear carbon nanotubes by combining the organic polymer with the hydroxylated carbon nanotubes, reduce the cross-linking entanglement of the carbon nanotubes, improve the distribution state of the carbon nanotubes in the slurry, and improve its dispersion uniformity, thereby further improving the processability of the pole piece and improving the fast charging performance of the battery cell. At the same time, compared with traditional organic high molecular polymer binders, by combining the organic polymer with the hydroxylated carbon nanotubes, the high conductivity of the carbon nanotubes can also improve the conductive properties of the binder, thereby obtaining a composite conductive agent with better comprehensive performance.
[0128] In some embodiments, the polymeric structure includes a polymeric structure represented by formula (2),
[0129]
[0130] In formula (2), ** represents the connection site of the polymer structure, p is an integer from 1000 to 5000, q is an integer from 1000 to 15000, f is an integer from 500 to 4000, 2≤n≤200, each R2 is independently selected from and One of the following, * indicates the connection site of R2, M + Selected from Na + , K + 、Li + and NH4 + One of them.
[0131] It can be seen from the above formula (2) that compared with the traditional single-type monomer linear polymer, the composite conductive agent of the present application has a linear structure of the molecular chain containing more side chains composed of multiple different functional groups. These side chains can reduce the brittleness of the composite conductive agent and enhance its flexibility, thereby enhancing the flexibility of the electrode. Therefore, after cold pressing at a high compaction density, the ductility of the electrode can be improved, which can effectively reduce the occurrence of edge overvoltage. At the same time, it can also improve the phenomenon that the electrode under high density is prone to brittle fracture during subsequent processing, thereby improving the processability of the electrode.
[0132] In some embodiments, in the above-mentioned organic polymer structural formula (1) and formula (2), the degree of polymerization m, p, q, and f of each polymer structure will affect the adhesiveness and solubility and dispersibility of the composite conductive agent in the slurry. When the degree of polymerization of each polymer structure is relatively low, the adhesiveness of the composite conductive agent is likely to decrease; when the degree of polymerization of each polymer structure is relatively high, the solubility and dispersibility of the composite conductive agent in the slurry is likely to decrease. By controlling the degree of polymerization m, p, q, and f of each polymer structure within an appropriate range, the composite conductive agent can have both high adhesive properties and good solubility and dispersibility in the slurry.
[0133] As a non-limiting example of the composite conductive agent, the schematic structural formula of the composite conductive agent may include any one of the following formulas (3) to (8):
[0134]
[0135] In some embodiments, the hydroxylated carbon nanotubes are bonded to the organic polymer via ester groups and / or hydrogen bonds. Alternatively, the hydroxylated carbon nanotubes are bonded to the organic polymer via ester groups.
[0136] It is understood that the ester groups can be derived from the esterification reaction between the hydroxyl groups in the hydroxylated carbon nanotubes and the carboxyl groups in the organic polymer. The ester groups formed between the hydroxylated carbon nanotubes and the organic polymer can reduce the carboxyl groups in the organic polymer, thereby reducing hydrogen bonding between molecules in the long polymer chains. This effectively reduces aggregation between the long polymer chains, improves dispersion uniformity in the slurry, reduces electrode sheet resistance, and thus improves the dynamic performance of the battery cell.
[0137] In some embodiments, in the composite conductive agent, the mass percentage of the organic polymer is 50% to 90%. For example, the mass percentage of the organic polymer can be 60%, 65%, 70%, 75%, 80%, 85%, or any range thereof. Alternatively, the mass percentage of the organic polymer is 65% to 80%.
[0138] In the embodiment of the present application, the mass percentage of the organic polymer in the composite conductive agent is within an appropriate range, which can not only provide sufficient linear polymerization structure for the composite conductive agent, ensure that the performance of the organic polymer is fully exerted, and improve the cycle life of the battery cell and the processability of the electrode; but also ensure that the composite conductive agent has high conductivity.
[0139] In some embodiments, the weight percentage of the hydroxylated carbon nanotubes in the composite conductive agent is 10% to 50%. For example, the weight percentage of the hydroxylated carbon nanotubes can be 15%, 20%, 25%, 30%, 35%, 40%, 45%, or any range thereof. Alternatively, the weight percentage of the hydroxylated carbon nanotubes is 20% to 35%.
[0140] In the embodiment of the present application, the mass percentage of hydroxylated carbon nanotubes in the composite conductive agent is within an appropriate range, which can not only ensure that the composite conductive agent has a high conductivity, but also form a sufficient number of ester groups between the organic polymer and the hydroxylated carbon nanotubes, thereby effectively reducing the carboxyl functional groups in the organic polymer, reducing the agglomeration formed by hydrogen bonding between long polymer chains, improving dispersion uniformity, and improving the dynamic performance of the battery cell.
[0141] The mass percentages of the organic polymer and hydroxylated carbon nanotubes in the composite conductive agent are well known in the art and can be measured using instruments and methods known in the art. For example, the organic portion can be separated by acid washing to obtain a CNT solid phase, and the percentages can be calculated.
[0142] In some embodiments, at least one hydroxyl group is connected to the surface of the hydroxylated carbon nanotube. Optionally, the hydroxylated carbon nanotube includes a hydroxylated single-walled carbon nanotube and / or a hydroxylated multi-walled carbon nanotube.
[0143] It should be noted that the hydroxylated carbon nanotubes described herein are carbon nanotubes containing at least one hydroxyl group on their surface. These hydroxyl groups may be attached to the surface of the carbon nanotubes by methods including, but not limited to, grafting. As non-limiting examples of hydroxylated carbon nanotubes, the hydroxylated carbon nanotubes may be commercially available or obtained by acid-washing carbon nanotubes.
[0144] A second aspect of the present application provides a method for preparing a composite conductive agent, comprising the following steps:
[0145] S10, reacting acrylate with acrylic acid and hydroxylated carbon nanotubes to obtain a pre-reacted mixture; and
[0146] S20, polymerizing the pre-reacted mixture with acrylonitrile and acrylic polyether polyol monoester to form an organic polymer combined with the hydroxylated carbon nanotubes to obtain a composite conductive agent, wherein the composite conductive agent includes the organic polymer and the hydroxylated carbon nanotubes, and the organic polymer includes a polymer having the structural formula shown in formula (1).
[0147]
[0148] In formula (1), m is an integer from 2500 to 20000, and R1 is a polymer structure containing an ester group and a nitrile group.
[0149] In the method provided in the present application, acrylate is first pre-reacted with acrylic acid and hydroxylated carbon nanotubes to achieve pre-polymerization of acrylate, acrylic acid and hydroxylated carbon nanotubes, so that part of acrylate and acrylic acid form oligomers through pre-polymerization, and at the same time, part of hydroxylated carbon nanotubes are grafted onto the oligomers through esterification reaction to obtain a pre-reacted mixture; then the pre-reacted mixture is polymerized with acrylonitrile and acrylic acid polyether polyol monoester to achieve linear polymerization of the pre-reacted mixture, acrylonitrile and acrylic acid polyether polyol monoester to form an organic polymer including the structural formula shown in formula (1), and more hydroxylated carbon nanotubes are grafted onto the organic polymer through esterification reaction, thereby combining with the organic polymer to obtain a composite conductive agent. Among them, polyacrylic acid and polyacrylonitrile formed after the polymerization of acrylic acid and acrylonitrile both have good bonding effects. The polymerization of the two can play a reinforcing role, which is conducive to fully exerting the coating effect of the composite conductive agent, enhancing the bonding and binding effect on other particulate matter in the slurry (for example, silicon-based active material particles), improving the inhibitory effect on the volume expansion of other particulate matter (especially silicon-based active material particles) during the cycle process, reducing the rebound of the electrode, reducing the expansion force during the cycle of the battery cell, and improving the cycle life of the battery cell.
[0150] In some implementations, step S10 may include the following steps:
[0151] S100, contacting and mixing the polymerization aid, the acrylate, the acrylic acid, and the hydroxylated carbon nanotubes in water to form a first mixed solution; and
[0152] S110 , performing a first heat treatment on the first mixed solution to cause a prepolymerization reaction between the acrylate, the acrylic acid, and the hydroxylated carbon nanotubes.
[0153] In steps S100 to S101, after the first mixed solution consisting of the polymerization aid, acrylate, acrylic acid, and hydroxylated carbon nanotubes is subjected to a first heat treatment, a portion of the acrylate and acrylic acid undergo a prepolymerization reaction to form oligomers. Simultaneously, a portion of the hydroxylated carbon nanotubes are grafted onto the oligomers via an esterification reaction, resulting in a pre-reacted mixture. Structurally, in the pre-reaction, the hydroxylated carbon nanotubes primarily bridge with the acrylic acid. The purpose of the pre-polymerization reaction is to pre-react the relevant components separately, strengthening this bridge effect and preventing interference from subsequent components that could weaken the bonding strength and cause unstable bridge structures. Because acrylate and acrylic acid have similar structures, polymerization is facilitated, and thus the acrylate is introduced simultaneously for the pre-polymerization reaction.
[0154] In some embodiments, the type of the acrylate is not particularly limited, as long as the prepolymerization reaction can be achieved and a polymer structure of the polyacrylate can be obtained in the organic polymer. For example, the acrylate can include at least one of sodium acrylate, potassium acrylate, lithium acrylate, and ammonium acrylate.
[0155] In some embodiments, the weight percentage of the acrylate in the first mixed solution is 3% to 25%. For example, the weight percentage of the acrylate can be 5%, 7%, 11%, 13%, 15%, 17%, 19%, 21%, 23%, or any range thereof. Alternatively, the weight percentage of the acrylate is 5% to 15%. The acrylate and acrylic acid monomers in the first mixed solution have similar molecular structures, and simultaneous polymerization helps improve the reaction efficiency of the overall preparation process while avoiding the introduction of too many types of monomer molecules into the subsequent polymerization reaction.
[0156] In some embodiments, the weight percentage of acrylic acid in the first mixed solution is 5% to 40%. For example, the weight percentage of acrylic acid can be 10%, 15%, 20%, 25%, 30%, 35%, or any range thereof. Alternatively, the weight percentage of acrylic acid is 15% to 25%. A weight percentage of acrylic acid in the first mixed solution within a suitable range is beneficial for obtaining a polyacrylic acid polymer structure with a corresponding degree of polymerization in the organic polymer, thereby enabling the composite conductive agent to have higher bonding properties and better solubility and dispersibility in the slurry.
[0157] In some embodiments, in the first mixed solution, the mass percentage of the hydroxylated carbon nanotubes is 1% to 10%. For example, the mass percentage of the hydroxylated carbon nanotubes can be 3%, 5%, 7%, 9% or within the range of any of the above values. Optionally, the mass percentage of the hydroxylated carbon nanotubes is 3% to 7%. The mass percentage of the hydroxylated carbon nanotubes in the first mixed solution is within a suitable range, which is conducive to consuming the carboxyl functional groups in the mixed solution through the esterification reaction, thereby effectively reducing the carboxyl functional groups contained in the organic polymer finally formed, reducing the agglomeration formed by hydrogen bonding between long polymer chains, improving the dispersion uniformity, and improving the dynamic performance of the battery cell.
[0158] In some embodiments, the type of polymerization aid is not particularly limited, as long as it can act as a surfactant in the prepolymerization reaction and can break intramolecular and intermolecular hydrogen bonds. For example, the polymerization aid can include sodium dodecyl sulfonate and / or sodium dodecyl sulfate.
[0159] In the first mixed solution, the mass percentage of the polymerization aid is 2% to 5%. For example, the mass percentage of the polymerization aid can be 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, or any range thereof. Alternatively, the mass percentage of the polymerization aid is 3% to 4.5%. When the mass percentage of the polymerization aid in the first mixed solution is within a suitable range, it can not only act as a surfactant but also break intramolecular and intermolecular hydrogen bonds, thereby promoting the prepolymerization reaction.
[0160] In some embodiments, the temperature of the first heat treatment is 50° C. to 85° C., and optionally 65° C. to 80° C. The temperature of the first heat treatment is controlled within a suitable range, which is beneficial to further promote the prepolymerization reaction.
[0161] As a non-limiting example of step S10, sodium dodecyl sulfate, acrylic acid, sodium acrylate, and hydroxylated CNTs may be added to 1 kg of distilled water, stirred evenly, and then heated to 70°C to obtain a pre-reacted mixture.
[0162] In some implementations, step S20 may include the following steps:
[0163] S200, contacting and mixing a polymerization initiator, the acrylonitrile, and the acrylic polyether polyol monoester in the solution of the pre-reacted mixture to obtain a second mixed solution; and
[0164] S210, performing a second heat treatment on the second mixed liquid to cause a polymerization reaction between the acrylonitrile, the acrylic polyether polyol monoester and the pre-reacted mixture to form the polymer structure, wherein the polymer structure includes a polymer structure represented by formula (2).
[0165]
[0166] In formula (2), ** represents the connection site of the polymer structure, p is an integer from 1000 to 5000, q is an integer from 1000 to 15000, f is an integer from 500 to 4000, 2≤n≤200, each R2 is independently selected from and One of the following, * indicates the connection site of R2, M + Selected from Na + , K + 、Li + and NH4 + One of them.
[0167] In the above steps S200 to S210, the pre-reacted mixture is polymerized with acrylonitrile and acrylic polyether polyol monoester, which can achieve linear polymerization of the pre-reacted mixture, acrylonitrile and acrylic polyether polyol monoester to form a polymer structure including the structural formula shown in formula (2), thereby obtaining an organic polymer, and more hydroxylated carbon nanotubes are grafted onto the organic polymer through an esterification reaction, thereby combining with the organic polymer to obtain a composite conductive agent.
[0168] In some embodiments, the type of the acrylic acid polyether polyol monoester is not particularly limited, as long as a polymerization reaction can be achieved and a polymer structure of the acrylic acid polyether polyol monoester is obtained in the organic polymer. For example, the acrylic acid polyether polyol monoester may include at least one of polyethylene glycol acrylate monoester, polypropylene glycol acrylate monoester, and polytetramethylene glycol acrylate monoester.
[0169] In some embodiments, in the second mixed liquid, the mass percentage of the acrylic polyether polyol monoester is 10% to 40%. For example, the mass percentage of the acrylic polyether polyol monoester can be 15%, 20%, 25%, 30%, 35% or within the range of any of the above values. Optionally, the mass percentage of the acrylic polyether polyol monoester is 20% to 35%. The mass percentage of the acrylic polyether polyol monoester in the second mixed liquid is controlled within a suitable range, which is conducive to the formation of organic polymers and obtaining a polyacrylic polyether polyol monoester polymerization structure with a corresponding degree of polymerization in the organic polymer, thereby making the electrode have better flexibility, preventing brittle fracture, and being able to withstand deformation during processing. At the same time, it can also withstand deformation caused by volume changes during battery cycling, thereby improving service life.
[0170] In some embodiments, the mass percentage of acrylonitrile in the second mixed liquid is 5% to 30%. For example, the mass percentage of acrylonitrile can be 10%, 15%, 20%, 25%, or any range thereof. Alternatively, the mass percentage of acrylonitrile is 10% to 20%.
[0171] The mass percentage of acrylonitrile in the second mixed liquid is within an appropriate range, which is conducive to obtaining a polyacrylonitrile polymerization structure with a corresponding degree of polymerization in the organic polymer, thereby enabling the composite conductive agent to have higher bonding properties and better solubility and dispersibility in the slurry. In addition, the polyacrylonitrile formed after the polymerization of acrylonitrile also has a good bonding effect, which can enhance the bonding properties of the polyacrylic acid polymerization structure in the organic polymer, thereby facilitating full play of the coating effect of the composite conductive agent, enhancing the bonding and binding effect on other particulate matter in the slurry, improving the inhibitory effect on the volume expansion of other particulate matter (especially silicon-based active material particles) during the cycle, reducing the rebound of the pole piece, reducing the expansion force of the battery cell during the cycle, and improving the cycle life of the battery cell.
[0172] In some embodiments, the type of polymerization initiator is not particularly limited, as long as it can play a role in initiating the polymerization reaction. For example, the polymerization initiator can include at least one of potassium sulfate, potassium persulfate, sodium persulfate, and ammonium persulfate.
[0173] In the second mixed solution, the weight percentage of the polymerization initiator is 1% to 3%. For example, the weight percentage of the polymerization initiator can be 1.5%, 2%, 2.5%, or any range thereof. Alternatively, the weight percentage of the polymerization aid is 2% to 2.5%. The weight percentage of the polymerization initiator in the second mixed solution is within a suitable range, which is conducive to initiating and promoting the polymerization reaction.
[0174] In some embodiments, the temperature of the second heat treatment is 50° C. to 85° C., and optionally 65° C. to 80° C. The temperature of the second heat treatment is controlled within a suitable range, which is beneficial to further promote the polymerization reaction.
[0175] As a non-limiting example of step S20, potassium sulfate can be added to the solution of the pre-reacted mixture, and polyethylene glycol monoacrylate and acrylonitrile are simultaneously and evenly added, and simultaneously heated to 70°C and stirred for 2 to 3 hours; during the reaction process, each reagent can be slowly added in equal proportion according to the required mass percentage, and the composite conductive agent can be obtained after purification by removing the supernatant by centrifugation.
[0176] In some embodiments, before obtaining the composite conductive agent, the method of the present application may further include the following step S30 of preparing the acrylic polyether polyol monoester:
[0177] S30, contacting acrylic acid with polyether polyol to cause an esterification reaction to obtain the acrylic acid polyether polyol monoester.
[0178] Acrylic acid and polyether polyol monoester are reacted to form acrylic acid polyether polyol monoester, wherein the ether bond contained in the acrylic acid polyether polyol monoester can effectively enhance the flexibility of the composite conductive agent in the final composite conductive agent, thereby enhancing the flexibility of the electrode and improving the processability of the electrode.
[0179] In some embodiments, the type of the polyether polyol is not particularly limited, as long as it can undergo esterification reaction with acrylic acid and includes an ether bond in its molecular structure. For example, the polyether polyol may include at least one of polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.
[0180] In some embodiments, the degree of polymerization of the polyether polyol is 2 to 200, and optionally 50 to 150. The degree of polymerization of the polyether polyol is mainly reflected in the length of the side chain. A suitable degree of polymerization can improve the problem of brittle electrode caused by the linear structure of the main chain, but too long can easily lead to problems such as decreased adhesion and slurry processing.
[0181] In some implementations, the above step S30 may further include the following steps:
[0182] S300, contacting and mixing the acrylic acid and the polyether polyol in water to form a third mixed solution;
[0183] S310, adding a catalyst and a polymerization inhibitor to the third mixed liquid;
[0184] S320, performing a third heat treatment on the third mixed liquid to obtain a solution of acrylic polyether polyol monoester;
[0185] S330, purifying the solution of the acrylic acid polyether polyol monoester to obtain the acrylic acid polyether polyol monoester.
[0186] In the above steps S300 to S330, acrylic acid and polyether polyol may undergo esterification reaction under the action of a catalyst and a polymerization inhibitor. The esterification reaction may link the carboxyl group in acrylic acid with the hydroxyl group in polyether polyol to form acrylic acid polyether polyol monoester.
[0187] In some embodiments, the molar ratio of acrylic acid to polyether polyol is from (5:1) to (1:1), and can be optionally from (1.5:1) to (2.5:1). Controlling the molar ratio of acrylic acid to polyether polyol within a suitable range is conducive to the occurrence of an esterification reaction, thereby obtaining the target product, acrylic acid polyether polyol monoester.
[0188] In some embodiments, the type of the catalyst is not particularly limited, as long as it can catalyze the esterification reaction and increase the reaction rate. For example, the catalyst can include at least one of p-toluenesulfonic acid, sulfuric acid, and aluminum chloride.
[0189] In some embodiments, the weight percentage of the catalyst in the third mixed solution is 3% to 10%. For example, the weight percentage of the catalyst can be 4%, 5%, 6%, 7%, 8%, 9%, or any range thereof. Alternatively, the weight percentage of the catalyst is 5% to 9%. When the weight percentage of the catalyst in the third mixed solution is within a suitable range, the catalyst can achieve a better catalytic promoting effect.
[0190] In some embodiments, the type of the polymerization inhibitor is not particularly limited, as long as it can prevent the polymerization of acrylic acid monomers during the esterification reaction. For example, the polymerization inhibitor can include at least one of hydroquinone, p-hydroxyanisole, and 2,6-di-tert-butyl-p-cresol.
[0191] In some embodiments, the weight percentage of the polymerization inhibitor in the third mixed solution is 1% to 5%. For example, the weight percentage of the polymerization inhibitor can be 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, or any range thereof. Alternatively, the weight percentage of the polymerization inhibitor is 3% to 4.5%. When the weight percentage of the polymerization inhibitor in the third mixed solution is within a suitable range, the polymerization inhibitor can better inhibit the polymerization of the acrylic acid monomer.
[0192] In some embodiments, the temperature of the third heat treatment is 60° C. to 85° C., and optionally 70° C. to 80° C. The temperature of the third heat treatment is controlled within a suitable range, which is conducive to promoting the esterification reaction.
[0193] As a non-limiting example of the esterification reaction in step S30, the reaction process can be represented by any one of the following reaction formulas (I) to (III):
[0194]
[0195] As a non-limiting example of step S30, polyethylene glycol and acrylic acid can be added to distilled water in a molar ratio of 1:1 to obtain a 20% solution. A catalyst and a polymerization inhibitor are then added, stirred evenly, and heated to 70°C to obtain a polyethylene glycol monoacrylate solution. The polyethylene glycol monoacrylate solution is then dissolved in dichloromethane, washed with 5% sodium hydroxide, separated to remove the aqueous solution, then washed with saturated sodium chloride solution, separated to remove excess polyether, and finally distilled to remove the solvent to obtain the polyethylene glycol monoacrylate monomer.
[0196] In some embodiments, before obtaining the composite conductive agent, the method of the present application may further include the following step S40 of preparing the acrylate:
[0197] S40, allowing acrylic acid to contact and react with an alkaline reagent to obtain the acrylic acid salt.
[0198] Acrylates are obtained by reacting acrylic acid with an alkaline reagent to salify the acrylic acid. Salinizing the carboxylic acid functional groups in acrylic acid reduces hydrogen bonding on the polyacrylate molecular chains during the subsequent polymerization process, weakening the mutual agglomeration between the molecular chains. This allows the resulting conductive adhesive to be evenly dispersed in the slurry, thereby improving the dynamic performance of the battery cell.
[0199] In some implementations, the above step S40 may further include the following steps:
[0200] S400, adding an alkaline agent to the acrylic acid solution to adjust the pH value of the solution to 7 to 8, thereby obtaining the acrylate solution;
[0201] S410, performing distillation and drying treatment on the acrylate solution.
[0202] In the above steps S400 to S410, the amount of the reactants acrylic acid and alkaline reagent can be indirectly controlled by controlling the pH value of the solution. By controlling the amount of the reactants within a suitable range, the salification reaction is facilitated, thereby obtaining the target product acrylate.
[0203] In some embodiments, the type of acrylate is not particularly limited, as long as a polymerization reaction can be achieved in a subsequent reaction process to obtain a polymeric structure of the polyacrylate in the organic polymer. For example, the acrylate can include at least one of sodium acrylate, potassium acrylate, lithium acrylate, and ammonium acrylate.
[0204] In some embodiments, the type of the alkaline agent is not particularly limited, as long as it can salt the acrylic acid and reduce the carboxyl groups contained in the acrylic acid. For example, the alkaline agent includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide and ammonia water.
[0205] As a non-limiting example of the salification reaction in step S40, the reaction process can be represented by the following reaction formula (IV):
[0206]
[0207] As a non-limiting example of step S40, sodium hydroxide solution may be slowly added dropwise to an aqueous solution of acrylic acid, and the solution may be stirred during the addition process until the pH value of the solution reaches 7 to 8, and then distilled and dried to obtain sodium acrylate particles.
[0208] Pole
[0209] A third aspect of the embodiments of the present application provides a pole piece, comprising the composite conductive agent of the first aspect of the present application or the composite conductive agent prepared by the method of the second aspect of the present application.
[0210] In some embodiments, the electrode sheets may include negative and / or positive electrode sheets. The electrode sheets include a composite conductive agent, which improves the dispersion and uniformity of the slurry and reduces the occurrence of slurry gelation. Applying the slurry containing the composite conductive agent to the electrode sheets increases the post-drying cold pressing window and improves the processing performance of the electrode sheets. Furthermore, the composite conductive agent can suppress electrode sheet rebound during cycling, reduce the increase in battery cell expansion force, and increase the cycle life of the battery cells.
[0211] It should be noted that the composite conductive agent of the present application, when used in an electrode, can be used alone as a conductive agent or adhesive, or can be mixed with other conventional adhesives or conductive agents.
[0212] In some embodiments, the negative electrode sheet may include the composite conductive agent of the first aspect of the present application or the composite conductive agent prepared by the method of the second aspect of the present application.
[0213] In some embodiments, the positive electrode sheet may include the composite conductive agent of the first aspect of the present application or the composite conductive agent prepared by the method of the second aspect of the present application.
[0214] It should be noted that when the conductive binder of the present application is used for a positive electrode sheet, the active material in the positive electrode sheet needs to be a positive electrode material that is insensitive to moisture, for example, a lithium iron phosphate positive electrode material.
[0215] secondary batteries
[0216] A fourth aspect of the embodiments of the present application provides a secondary battery, including any device in which an electrochemical reaction occurs to convert chemical energy into electrical energy, for example, a lithium ion secondary battery or a sodium ion secondary battery.
[0217] In some embodiments, the secondary battery of the present application includes the electrode sheet of the third aspect of the present application, wherein the electrode sheet includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte. During the battery charging and discharging process, active ions are intercalated and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte acts as an ion conductor between the positive electrode sheet and the negative electrode sheet. The separator is disposed between the positive electrode sheet and the negative electrode sheet, primarily to prevent a short circuit between the positive and negative electrodes while allowing ions to pass through.
[0218] [Positive electrode]
[0219] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector. The positive electrode film layer includes a positive electrode active material. For example, the positive electrode current collector has two opposing surfaces in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.
[0220] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc. Polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0221] In some embodiments, the positive electrode active material may include a positive electrode active material for a battery that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0222] In some embodiments, the positive electrode active material may also include at least one of the following materials: a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound. However, this application is not limited to these materials; other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more.
[0223] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Sodium transition metal oxide is, for example, Na x MO2, wherein M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.
[0224] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n- A class of compounds with anionic units. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be at least one of P, S and Si; n represents (YO4) n- valence.
[0225] Polyanionic compounds can also be sodium ions, transition metal ions, tetrahedral (YO4) n-A class of compounds containing anion units and halogen anions. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y can be at least one of P, S, and Si, and n represents (YO4) n- valence state; the halogen may be at least one of F, Cl and Br.
[0226] Polyanionic compounds can also be sodium ions, tetrahedral (YO4) n- Anion unit, polyhedron unit (ZO y ) m+ and an optional halogen anion. Y can be at least one of P, S and Si, and n represents (YO4) n- valence state; Z represents a transition metal, which may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce, and m represents (ZO y ) m+ valence state; the halogen may be at least one of F, Cl and Br.
[0227] Polyanionic compounds include NaFePO4, Na3V2(PO4)3 (sodium vanadium phosphate, abbreviated as NVP), Na4Fe3(PO4)2(P2O7), NaM'PO4F (M' is one or more of V, Fe, Mn and Ni) and Na3(VOy)2(PO4)2F 3-2y At least one of (0≤y≤1).
[0228] Prussian blue compounds can be sodium ions, transition metal ions and cyanide ions (CN - ) compounds. The transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Prussian blue compounds are, for example, Na a Me b Me' c (CN)6, wherein Me and Me' are each independently at least one of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.
[0229] In some embodiments, the positive electrode film layer may optionally further include the composite conductive agent of the first aspect of the present application or the composite conductive agent prepared according to the method of the second aspect of the present application.
[0230] In some embodiments, the positive electrode film layer does not exclude other conventional conductive agents in addition to the composite conductive agent provided herein. As an example, other conventional conductive agents may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0231] In some embodiments, the positive electrode film layer does not exclude other conventional binders besides the composite conductive agent provided herein. As an example, other conventional binders may include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and at least one of fluorine-containing acrylate resin.
[0232] The positive electrode sheets in this application can be prepared according to conventional methods in the art. For example, the positive electrode film layer is typically formed by coating a positive electrode slurry onto a positive electrode current collector, drying, and cold pressing. The positive electrode slurry is typically formed by dispersing the positive electrode active material, an optional composite conductive agent, optional other conventional conductive agents, optional other conventional binders, and any other components in a solvent and stirring them uniformly. The solvent can be, but is not limited to, N-methylpyrrolidone (NMP).
[0233] The positive electrode sheet of the present application does not exclude other additional functional layers in addition to the positive electrode film layer. For example, in some embodiments, the positive electrode sheet of the present application further includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the positive electrode current collector and the positive electrode film layer and disposed on the surface of the positive electrode current collector. In other embodiments, the positive electrode sheet of the present application further includes a protective layer covering the surface of the positive electrode film layer.
[0234] [Negative electrode]
[0235] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector. The negative electrode film layer includes a negative electrode active material. For example, the negative electrode current collector has two opposing surfaces in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposing surfaces of the negative electrode current collector.
[0236] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver and silver alloys, etc., and the polymer material substrate includes but is not limited to polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE) and other substrates.
[0237] In some embodiments, the negative electrode active material may adopt the negative electrode active material for secondary batteries known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0238] In some embodiments, the negative electrode film layer may optionally further include the composite conductive agent of the first aspect of the present application or the composite conductive agent prepared according to the method of the second aspect of the present application.
[0239] In some embodiments, the negative electrode film layer does not exclude other conventional binders besides the composite conductive agent provided herein. Other conventional binders may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0240] In some embodiments, the negative electrode film layer does not exclude other conventional conductive agents in addition to the composite conductive agent provided herein. Other conventional conductive agents can be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0241] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0242] In some embodiments, the negative electrode sheet can be prepared by the following method: the above-mentioned components for preparing the negative electrode sheet, such as the negative electrode active material, the optional composite conductive agent, the optional other conventional conductive agent, the optional other conventional binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0243] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0244] [Electrolyte]
[0245] The electrolyte plays a role in conducting active ions between the positive electrode and the negative electrode. The electrolyte that can be used in the secondary battery of the present application can be an electrolyte known in the prior art.
[0246] In some embodiments, the electrolyte includes an organic solvent, an electrolyte salt, and optional additives. The types of the organic solvent, electrolyte salt, and additives are not particularly limited and can be selected according to needs.
[0247] In some embodiments, the electrolyte salt may be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0248] In some embodiments, the electrolyte salt may include, but is not limited to, at least one of NaPF6, NaClO4, NaBCl4, NaSO3CF3, and Na(CH3)C6H4SO3. The above electrolyte salts may be used alone or in combination of two or more.
[0249] In some embodiments, as an example, the organic solvent includes but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE). The above organic solvents can be used alone or in combination. Alternatively, two or more organic solvents are used in combination.
[0250] In some embodiments, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0251] As an example, the additive includes but is not limited to at least one of fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinyl ethylene carbonate (VEC), diethylene sulfate (DTD), propylene sulfate, vinyl sulfite (ES), 1,3-propane sultone (PS), 1,3-propene sultone (PST), sulfonate cyclic quaternary ammonium salt, succinic anhydride, succinonitrile (SN), adiponitrile (AND), tris(trimethylsilyl) phosphate (TMSP), and tris(trimethylsilyl) borate (TMSB).
[0252] The electrolyte solution can be prepared according to conventional methods in the art. For example, an organic solvent, an electrolyte salt, and optional additives can be uniformly mixed to obtain the electrolyte solution. The order in which the materials are added is not particularly limited. For example, the electrolyte salt and optional additives can be added to the organic solvent and mixed uniformly to obtain the electrolyte solution; alternatively, the electrolyte salt can be first added to the organic solvent, and then the optional additives can be added to the organic solvent and mixed uniformly to obtain the electrolyte solution.
[0253] [Isolation film]
[0254] The separator is placed between the positive and negative electrodes to prevent short circuits between the positive and negative electrodes while allowing active ions to pass through. This application does not impose any particular restrictions on the type of separator; any known porous separator with good chemical and mechanical stability can be used.
[0255] In some embodiments, the material of the isolation membrane can be selected from one or more of, but not limited to, glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different. In some embodiments, the isolation membrane can also be provided with a ceramic coating or a metal oxide coating.
[0256] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0257] In some embodiments, the secondary battery cell may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0258] In some embodiments, the outer packaging of the secondary battery cell can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery cell can also be a soft package, such as a bag-type soft package. The soft package can be made of plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0259] The present application has no particular limitation on the shape of the secondary battery cell, which can be cylindrical, square or any other shape. FIG1 shows a secondary battery 5 with a square structure as an example.
[0260] In some embodiments, referring to FIG2 , the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the separator may be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 may be one or more, which can be adjusted according to demand.
[0261] In some embodiments, the secondary battery may also be a battery module assembled from a plurality of battery cells. The battery module may contain multiple secondary battery cells, and the specific number may be adjusted according to the application and capacity of the battery module.
[0262] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple secondary battery cells 5 may be arranged sequentially along the length of the battery module 4. Of course, they may also be arranged in any other manner. Furthermore, the multiple secondary battery cells 5 may be secured together using fasteners.
[0263] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of secondary battery cells 5 are accommodated in the accommodation space.
[0264] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0265] In some embodiments, the battery cells mentioned above may also be directly assembled into a battery pack, and the number of battery cells contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0266] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 covers the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the battery box.
[0267] Electrical equipment
[0268] The fifth aspect of the embodiment of the present application provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack of the present application. The secondary battery, battery module, or battery pack can be used as a power source for the device, and can also be used as an energy storage unit for the device. The device can be, but is not limited to, a mobile device, an electric vehicle, an electric train, a ship and a satellite, an energy storage system, etc. For example, it can be a laptop computer, a pen-input computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery, etc.
[0269] The device can select a secondary battery, a battery module or a battery pack according to its usage requirements.
[0270] Figure 6 shows an example device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the device's requirements for high power and high energy density, a battery pack or battery module can be used.
[0271] Example
[0272] The following examples describe the present disclosure in more detail and are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and used directly without further processing, and all instruments used in the examples are commercially available.
[0273] Example 1
[0274] Preparation of composite conductive agent
[0275] (1) Sodium hydroxide solution (mass percentage concentration is 10%) was slowly added dropwise to an acrylic acid aqueous solution (mass percentage concentration is 15%), and the solution was stirred during the addition process until the pH value of the solution was 7.5. The solution was distilled and dried to obtain sodium acrylate particles.
[0276] (2) Polyethylene glycol and acrylic acid were added to distilled water in a molar ratio of 2:1 to prepare a 20% mass percent solution, 5% mass percent toluenesulfonic acid and 3% mass percent hydroquinone were added, and the mixture was stirred and heated to 70° C. to obtain an aqueous solution of polyethylene glycol monoacrylate.
[0277] (3) The product of (2) is dissolved in dichloromethane, washed with a sodium hydroxide solvent having a mass percentage concentration of 5%, separated to remove the aqueous solution, then washed with a saturated sodium chloride solution, separated to remove excess polyether substances, and finally distilled to remove the solvent to obtain acrylic acid polyethylene glycol monoester.
[0278] (4) Sodium dodecyl sulfate and acrylic acid, and the sodium acrylate prepared in step (1), were added to redistilled water at concentrations of 3%, 20%, and 10% by mass to obtain an aqueous solution. Hydroxylated CNTs (5% by mass) were added to the solution, stirred evenly, and heated to 70°C.
[0279] (5) Potassium sulfate with a mass percentage concentration of 2% is added to (4), and the acrylic acid polyethylene glycol monoester (mass percentage 30%) and acrylonitrile (mass percentage 15%) prepared in (3) are uniformly added simultaneously, and the mixture is heated to 70° C. and stirred continuously for 2 to 3 hours; during the reaction, reagents can be slowly added in equal proportions, and the target product, a composite conductive agent, is obtained after removing the supernatant by centrifugal washing.
[0280] Preparation of positive electrode
[0281] The positive electrode active material NCM, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are dissolved in the solvent N-methylpyrrolidone (NMP) in a weight ratio of 96.5:1.5:2, and the mixture is fully stirred and mixed to obtain a positive electrode slurry; the positive electrode slurry is then evenly coated on the positive electrode collector, and then dried, cold pressed, and cut to obtain a positive electrode sheet.
[0282] Preparation of negative electrode sheet
[0283] The active material graphite, silicon, conductive agent acetylene black, composite conductive agent, thickener sodium carboxymethyl cellulose (CMC), and binder (SBR) are dissolved in solvent deionized water in a weight ratio of 90:5:1:2:1, and then evenly mixed with deionized water to prepare a negative electrode slurry. The slurry is coated on copper foil, dried, and then cold-pressed and cut to obtain a negative electrode sheet.
[0284] Preparation of electrolyte
[0285] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent; LiPF6 is dissolved in the above organic solvent, and then fluoroethylene carbonate (FEC) is added and mixed evenly to obtain an electrolyte; wherein the concentration of LiPF6 is 1 mol / L.
[0286] Preparation of isolation membrane
[0287] PE porous film is used as the isolation membrane.
[0288] Preparation of lithium-ion batteries
[0289] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrodes to provide insulation. The cells are then wound to form a bare cell. The tabs are then welded to the bare cell and placed in an aluminum shell. The shell is then baked at 80°C to remove moisture. The electrolyte is then injected and sealed to create an uncharged battery. The uncharged battery then undergoes a series of processes, including resting, hot and cold pressing, formation, shaping, and capacity testing, to produce a lithium-ion battery.
[0290] Examples 2 to 25
[0291] The preparation method of the lithium-ion battery is similar to that of Example 1, except that the composite conductive agent and the relevant parameters in the preparation process are adjusted. The specific parameters are detailed in Table 1 below. Wherein, “ / ” indicates that the corresponding parameter does not exist.
[0292] Among them, the negative electrode plate of Example 24 contains conventional conductive agent acetylene black and composite conductive agent, but does not contain conventional binder SBR; the negative electrode plate of Example 25 contains conventional binder SBR and composite conductive agent, but does not contain conventional conductive agent acetylene black.
[0293] Comparative Example 1
[0294] In the negative electrode sheet of Comparative Example 1, carbon nanotubes are used instead of the composite conductive agent.
[0295] Comparative Example 2
[0296] The method for preparing the composite conductive agent in Comparative Example 2 is similar to that in Example 1, except that no hydroxylated carbon nanotubes are added during the preparation process, and carbon nanotubes are used in the negative electrode to replace the conductive agent acetylene black.
[0297] Comparative Example 3
[0298] The method for preparing the composite conductive agent in Comparative Example 3 is similar to that in Example 1, except that no hydroxylated carbon nanotubes are added during the preparation process.
[0299] Comparative Example 4
[0300] The method for preparing the composite conductive agent in Comparative Example 4 is similar to that in Example 1, except that an excess of hydroxylated carbon nanotubes is used during the preparation process.
[0301] Test section
[0302] (1) Machinability test of slurry or electrode
[0303] Stability test of slurry: take an appropriate amount of stirred slurry in a beaker, seal it with plastic wrap, and check the slurry sedimentation or gelation after standing for 24 hours: open the plastic wrap, gently move the slurry surface with a steel ruler to check whether there is any abnormality on the slurry surface; slowly extend the steel ruler vertically along the edge of the beaker to the bottom of the beaker, scrape the slurry at the bottom and then pull out the steel ruler to check the sedimentation brought out by the steel ruler.
[0304] Electrode Adhesion Test: Take the electrode to be tested and cut a sample of appropriate length and width with a blade. Apply special double-sided tape to a steel plate, keeping the tape width constant. Attach the cut electrode sample to the double-sided tape with the test surface facing down. After compacting with a roller, use a tensile testing machine to test the force corresponding to the maximum peel strength. Convert to N / m based on the tape width.
[0305] Toughness of the electrode: Take an appropriate amount of cold-pressed electrode sample, fold the sample in half along the TD direction, place it on the flat surface of the laboratory table, roll it once with a 2kg cylindrical roller, and then fold it again once to check whether there is light transmission or breakage at the crease. If so, it is NG. If not, repeat the above test, check the light transmission once, add 1 to the toughness, and record the maximum number of non-NG toughness.
[0306] (2) Lithium-ion battery cycle life test
[0307] The cycle test temperature is 25°C. The battery is charged at a constant current of 0.33C to the upper limit voltage, then charged at a constant voltage of 0.05C. After standing for 5 minutes, it is discharged at 0.33C to the lower limit voltage. The capacity obtained in this step is the initial capacity. A 0.33C charge / 0.33C discharge cycle test is performed until the capacity decays to 80% SOH. The corresponding cycle number is recorded to obtain the corresponding life data.
[0308] (3) Battery cell expansion force test
[0309] Before the test (2), the battery cell is fixed in the fixture of the pressure sensor and clamped with a fixed pressure. The capacity calibration and cycle test are carried out according to the process in (2). The change of expansion force is monitored during the cycle. The ratio of the expansion force increment when the capacity decays to 80% to the initial expansion force is the expansion force change.
[0310] (4) Lithium-ion battery dynamic performance test
[0311] DC resistance (DCR) test: Charge the cell to the nominal voltage at 0.33C, then charge at constant voltage until the current is ≤ 0.05C, recording the capacity at 100% SOC. Wait for 5 minutes. Discharge the cell to 50% SOC at a constant current rate of 0.33C. After conditioning, measure the lithium-ion battery voltage and record it as V1. Discharge the cell at a constant current rate of 4C (denoted as I) for 10 seconds. After discharge, measure the lithium-ion battery voltage and record it as V2. Calculate the DC resistance using the formula: DCR = (V1 - V2) / I.
[0312] Table 2 below shows the performance test results of Examples 1 to 24 and Comparative Examples 1 to 4.
[0313] Comparison of the Examples and Comparative Examples demonstrates that the composite conductive agent obtained by combining an organic polymer with hydroxylated carbon nanotubes can effectively improve the processability of electrode sheets, reduce the expansion force of battery cells, and enhance the cycle life and dynamic performance of lithium-ion batteries. By controlling the relevant parameters during the composite conductive agent preparation process, the various properties of the electrode sheets, battery cells, and lithium-ion batteries can be adjusted, thereby achieving lithium-ion batteries with superior overall performance based on actual application requirements.
[0314] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0315] The above description is merely a specific embodiment of the present application, but the scope of protection of the present application is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in this application, and such modifications or substitutions should be included in the scope of protection of this application. Therefore, the scope of protection of this application should be based on the scope of protection of the claims, and the description and drawings can be used to interpret the scope of protection of the claims.
[0316]
[0317]
[0318] Table 2
[0319]
Claims
1. A composite conductive agent comprising: organic polymers; and Hydroxylated carbon nanotubes combined with the organic polymer, wherein the organic polymer includes a polymer having the structural formula shown in formula (1), In formula (1), m is an integer from 2500 to 20000, and R1 is a polymer structure containing an ester group and a nitrile group.
2. The composite conductive agent according to claim 1, wherein The polymer structure includes a polymer structure of the formula (2), In formula (2), ** represents the connection site of the polymer structure, p is an integer from 1000 to 5000, q is an integer from 1000 to 15000, f is an integer from 500 to 4000, 2≤n≤200, each R2 is independently selected from and One of the following, * indicates the connection site of R2, M + Selected from Na + , K + 、Li + and NH4 + One of them.
3. The composite conductive agent according to claim 1 or 2, wherein The composite conductive agent satisfies at least one of the following conditions: (1) the hydroxylated carbon nanotubes are bonded to the organic polymer via ester groups and / or hydrogen bonds. Optionally, the hydroxylated carbon nanotubes are bonded to the organic polymer via ester groups; and (2) The surface of the hydroxylated carbon nanotube is connected with at least one hydroxyl group.
4. The composite conductive agent according to any one of claims 1 to 3, wherein The composite conductive agent satisfies at least one of the following conditions: (1) In the composite conductive agent, the mass percentage of the organic polymer is 50% to 90%, and optionally 65% to 80%; and (2) The hydroxylated carbon nanotubes include hydroxylated single-walled carbon nanotubes and / or hydroxylated multi-walled carbon nanotubes.
5. A method for preparing a composite conductive agent, comprising: reacting acrylate with acrylic acid and hydroxylated carbon nanotubes to obtain a pre-reacted mixture; and The pre-reacted mixture is polymerized with acrylonitrile and acrylic polyether polyol monoester to form an organic polymer combined with the hydroxylated carbon nanotubes to obtain a composite conductive agent, wherein the composite conductive agent includes the organic polymer and the hydroxylated carbon nanotubes, and the organic polymer includes the structural formula shown in formula (1). In formula (1), m is an integer from 2500 to 20000, and R1 is a polymer structure containing an ester group and a nitrile group.
6. The method according to claim 5, wherein: The step of reacting acrylate with acrylic acid and hydroxylated carbon nanotubes comprises: Under the action of a polymerization aid, the acrylate, the acrylic acid and the hydroxylated carbon nanotubes are contacted and reacted.
7. The method according to claim 6, wherein: The method satisfies at least one of the following conditions: (1) the acrylate comprises at least one of sodium acrylate, potassium acrylate, lithium acrylate and ammonium acrylate; and (2) The polymerization aid includes sodium lauryl sulfonate and / or sodium lauryl sulfate.
8. The method according to claim 6 or 7, wherein: The step of causing the acrylate, the acrylic acid and the hydroxylated carbon nanotubes to contact and react under the action of a polymerization aid comprises: contacting and mixing the polymerization aid, the acrylate, the acrylic acid, and the hydroxylated carbon nanotubes in water to form a first mixed solution; and The first mixed liquid is subjected to a first heat treatment to cause a prepolymerization reaction between the acrylate, the acrylic acid and the hydroxylated carbon nanotubes.
9. The method according to claim 8, wherein The method satisfies at least one of the following conditions: (1) In the first mixed solution, the mass percentage of the acrylate is 3% to 25%, and can be optionally 5% to 15%; (2) In the first mixed solution, the mass percentage of the acrylic acid is 5% to 40%, and can be optionally 15% to 25%; (3) In the first mixed solution, the mass percentage of the hydroxylated carbon nanotubes is 1% to 10%, and can be optionally 3% to 7%; (4) In the first mixed solution, the mass percentage of the polymerization aid is 2% to 5%, and optionally 3% to 4.5%; and (5) The temperature of the first heat treatment is 50°C to 85°C, and can be optionally 65°C to 80°C.
10. The method according to any one of claims 5 to 9, wherein: The process of polymerizing the pre-reacted mixture with acrylonitrile and acrylic acid polyether polyol monoester comprises: Under the action of a polymerization initiator, the pre-reacted mixture is brought into contact with the acrylonitrile and the acrylic polyether polyol monoester and polymerized to form the polymer structure, wherein the polymer structure includes a polymer structure represented by formula (2). In formula (2), ** represents the connection site of the polymer structure, p is an integer from 1000 to 5000, q is an integer from 1000 to 15000, f is an integer from 500 to 4000, 2≤n≤200, each R2 is independently selected from and One of the following, * indicates the connection site of R2, M + Selected from Na + , K + 、Li + and NH4 + One of them.
11. The method according to claim 10, wherein: The method satisfies at least one of the following conditions: (1) the acrylic acid polyether polyol monoester comprises at least one of acrylic acid polyethylene glycol monoester, acrylic acid polypropylene glycol monoester and acrylic acid polytetramethylene glycol monoester; and (2) The polymerization initiator includes at least one of potassium sulfate, potassium persulfate and sodium persulfate.
12. The method according to claim 10 or 11, wherein: The method of bringing the pre-reacted mixture into contact with the acrylonitrile and the acrylic polyether polyol monoester and polymerizing the mixture under the action of a polymerization initiator comprises: contacting and mixing the polymerization initiator, the acrylonitrile, and the acrylic polyether polyol monoester in the solution of the pre-reacted mixture to obtain a second mixed solution; and The second mixed liquid is subjected to a second heat treatment to cause a polymerization reaction between the acrylonitrile, the acrylic polyether polyol monoester and the pre-reacted mixture.
13. The method according to claim 12, wherein: The method satisfies at least one of the following conditions: (1) In the second mixed solution, the mass percentage of the polymerization initiator is 1% to 3%, and can be optionally 2% to 2.5%; (2) In the second mixed liquid, the mass percentage of acrylonitrile is 5% to 30%, and can be optionally 10% to 20%; (3) In the second mixed solution, the mass percentage of the acrylic polyether polyol monoester is 10% to 40%, and can be optionally 20% to 35%; and (4) The temperature of the second heat treatment is 50°C to 85°C, and can be optionally 65°C to 80°C.
14. The method according to any one of claims 5 to 13, wherein: The invention also includes the steps of preparing the acrylic acid polyether polyol monoester: Acrylic acid is brought into contact with polyether polyol to undergo an esterification reaction, thereby obtaining the acrylic acid polyether polyol monoester.
15. The method according to claim 14, wherein The method satisfies at least one of the following conditions: (1) the polyether polyol comprises at least one of polyethylene glycol, polypropylene glycol and polytetramethylene glycol; and (2) The degree of polymerization of the polyether polyol is 2 to 200, and can be optionally 50 to 150.
16. The method according to claim 14 or 15, wherein: The method of contacting acrylic acid with polyether polyol and causing esterification reaction comprises: contacting and mixing the acrylic acid and the polyether polyol in water to form a third mixed solution; and The third mixed liquid is subjected to a third heat treatment to obtain the acrylic polyether polyol monoester solution.
17. The method according to claim 16, wherein: The method satisfies at least one of the following conditions: (1) the molar ratio of the acrylic acid to the polyether polyol is (5:1) to (1:1), and optionally (1.5:1) to (2.5:1); and (2) The temperature of the third heat treatment is 50°C to 85°C, and can be optionally 65°C to 80°C.
18. The method according to claim 16 or 17, wherein Before performing the third heat treatment on the third mixed liquid, the method further comprises: adding a catalyst and a polymerization inhibitor to the third mixed liquid; Optionally, the catalyst comprises at least one of p-toluenesulfonic acid, sulfuric acid and aluminum oxide; and Optionally, the polymerization inhibitor includes at least one of hydroquinone, p-hydroxyanisole and 2,6-di-tert-butyl-p-cresol.
19. The method according to claim 18, wherein The method satisfies at least one of the following conditions: (1) In the third mixed solution, the mass percentage of the catalyst is 3% to 10%, and optionally 5% to 9%; and (2) In the third mixed liquid, the mass percentage of the polymerization inhibitor is 1% to 5%, and can be optionally 3% to 4.5%.
20. The method according to any one of claims 16 to 19, wherein After the third mixed liquid is subjected to the third heat treatment, the method further comprises: The solution of the acrylic acid polyether polyol monoester is purified to obtain the acrylic acid polyether polyol monoester.
21. The method according to any one of claims 5 to 20, wherein: The invention also includes the steps of preparing the acrylate: Acrylic acid is contacted with an alkaline reagent to react to obtain the acrylic acid salt.
22. The method according to claim 21, wherein The step of making acrylic acid contact with an alkaline reagent for reaction comprises: Adding an alkaline agent to a solution of acrylic acid to adjust the pH value of the solution to 7 to 8, thereby obtaining a solution of the acrylic acid salt; and The acrylate solution is subjected to distillation and drying treatment.
23. The method according to claim 21 or 22, wherein: The method satisfies at least one of the following conditions: (1) the alkaline reagent comprises at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide and ammonia water; and (2) The acrylate includes at least one of sodium acrylate, potassium acrylate, lithium acrylate and ammonium acrylate. 24 . A secondary battery comprising the composite conductive agent according to claim 1 or the composite conductive agent prepared according to the method according to claim 5 .
25. An electric device comprising the secondary battery according to claim 24.