System and method for depositing separator material

Through the spraying and processing technology of polymer-polymer-solvent liquid mixture, a separator film with a set pore network is formed, which solves the problem of separator material thickness and pore control in the battery, and improves the ion transmission efficiency and safety of the battery .

CN118947002AActive Publication Date: 2024-11-12MILLIBATT INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380033910.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-13
Filing Date
2023-04-13
Publication Date
2024-11-12
Estimated Expiration
2043-04-13

AI Technical Summary

Technical Problem

In the existing battery technology, it is difficult to achieve accurate control of uniform thickness and pore networks in the method of depositing separator materials, which affects the ion transmission efficiency of the battery and the safety of the battery cells.

Method used

Using polymer-polymer-solvent liquid mixture as the partition material, a partition film with a set pore network is formed on the substrate through a combination of spraying, heating, washing and electron beam irradiation to ensure uniformity of the ion transmission channel. and battery safety.

Benefits of technology

The uniformity and rapidity of ion transmission in the battery are achieved, while preventing electrical short circuits in the battery cell, improving the performance and reliability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118947002A_ABST
    Figure CN118947002A_ABST
Patent Text Reader

Abstract

One variation of a method includes: receiving a portion of a substrate strip including a substrate within a cladding region; depositing a series of droplets of separator material on the first substrate, each droplet of the series of droplets of separator material comprising a first solvent, a first polymer, and a second polymer; heating the substrate and a proportion of the separator material to a first temperature; dissolving a second polymer out of the series of separator material droplets by washing the series of separator material droplets and the substrate with a second solvent to provide an open pore network having pores; and irradiating the series of droplets of separator material to cross-link the first polymer and form a discrete separator layer having an open pore network of pores sized to transport ions through the discrete separator layer.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims the benefit of U.S. Provisional Application No. 63 / 330,763, filed on April 13, 2022, which is incorporated by reference in its entirety. Technical Field

[0002] The present invention relates generally to the field of battery technology, and more particularly to new and useful systems and methods for depositing separator materials in the field of battery technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0003] Figure 1 is a flow chart representation of a method; Figure 2 is a flowchart representation of a variation of the method; Figure 3 is a flowchart representation of a variation of the method; Figure 4 is a flowchart representation of a variation of the method; and Figure 5 is a flowchart representation of a variation of the method. Description of the implementation plan

[0004] The following description of embodiments of the present invention is not intended to limit the present invention to these embodiments, but to enable those skilled in the art to make and use the present invention. The variations, configurations, implementations, example implementations, and examples described herein are optional and do not exclude the variations, configurations, implementations, example implementations, and examples they describe. The present invention described herein may include any and all combinations of these variations, configurations, implementations, example implementations, and examples.

[0005] 1. Methods like Figure 1-Figure 5 As shown, method S100 includes: during a first time period: in frame S110, receiving a first substrate in a coating area; in frame S120, spraying a series of separator material droplets (a constellation of separator material droplets) on the first substrate, each droplet in the series of separator material droplets containing a first solvent, a first polymer miscible in the first solvent, and a second polymer miscible in the first solvent; and in frame S122, reaching a target substrate temperature below the boiling point of the first solvent.

[0006] Method S100 also includes, during a second time period after the first time period: in frame S130, heating the first substrate and a series of separator material droplets to a target substrate temperature to evaporate the first solvent from the series of separator material droplets and promote phase separation of the second polymer from the first polymer; in frame S140, washing the series of separator material droplets with a second solvent to dissolve the second polymer from the series of separator material droplets and provide an open-celled network of pores within the series of separator material droplets; and in frame S150, irradiating the series of separator material droplets and the first substrate to cross-link the first polymer and form a separator membrane on the first substrate, the separator membrane defining an open-celled network of pores, the open-celled network of pores being sized to transmit ions.

[0007] 1.1 Variant: thickness of partition A variation of method S100 includes: during a first time period: in frame S110, receiving a substrate within a coating area; in frame S112, defining a target liquid temperature range for a separator material; in frame S114, at a nozzle facing the substrate and connected to a reservoir volume of liquid separator material, heating the nozzle toward the target liquid temperature range; in frame S116, detecting a first temperature of the separator material at the nozzle; in frame S120, in response to the first temperature of the separator material falling within the target liquid temperature range, spraying a first volume of separator material on the substrate via the nozzle, the separator material comprising a first solvent, a first polymer miscible in the first solvent, and a second polymer miscible in the first solvent; and in frame S122, reaching a target substrate temperature below the boiling point of the first solvent.

[0008] This variation of method S100 also includes: during a second time period after the first time period: in frame S130, heating the substrate and the first volume of separator material to a target substrate temperature to evaporate the first solvent from the first volume of separator material; in frame S140, dissolving the second polymer from the first volume of separator material to provide an open pore network having pores; and in frame S150, irradiating the first volume of separator material to cross-link the first polymer and form a separator film having a separator thickness close to the target separator thickness.

[0009] 1.2 Variant: Discrete partition A variation of method S100 includes: during a first time period: in frame S110, receiving a section of a substrate strip including a first substrate in a coating area; and in frame S120, depositing a series of separator material droplets on the first substrate, each droplet in the series of separator material droplets comprising a first solvent, a first polymer, and a second polymer.

[0010] This variation of method S100 includes: during a second time period after the first time period: in frame S130, heating the first substrate and the series of separator material droplets to a first temperature; in frame S140, washing the series of separator material droplets and the first substrate with a second solvent to dissolve the second polymer from the series of separator material droplets and provide an open network with pores within the series of separator material droplets; and in frame S150, irradiating the series of separator material droplets to crosslink the first polymer and form a discrete separator layer having an open network with pores, the open network with pores being sized to transmit ions through the discrete separator layer.

[0011] 2. Application Typically, a substrate supply station, a spray system, a refilling station, a washing station, and an irradiation station (hereinafter referred to as "system 100") can collaborate to execute the frame of method S100 to deposit the separator material as an aerosol (or a "series" of separator material droplets, a "mist" or a "cloud" of separator material droplets) on a substrate (e.g., an electrode, a cathode, an anode) and form a thin separator film (e.g., a discrete separator layer, a permeable separator film) of uniform thickness on the substrate.

[0012] More specifically, the separator material includes a uniform polymer-polymer-solvent liquid mixture, the mixture comprising: a first solvent; a first polymer miscible in the first solvent; and a second polymer miscible in the first solvent. In one example, the first solvent includes an organic ketone such as butanone; the first polymer includes a copolymer such as poly(vinylidene fluoride-hexafluoropropylene) (or "PVDF-HFP"); and the second polymer includes a polyether such as polyethylene oxide (or "PEO"), poly(ethylene oxide) (or "POE") or polyethylene glycol (or "PEG"). In this example, a first polymer (e.g., PVDF-HFP) and a second polymer (e.g., PEG) are mixed in a first solvent (e.g., butanone) to form a homogeneous polymer-polymer-solvent liquid mixture showing greater than 80% by weight of the first solvent.

[0013] Thus, system 100 can execute the blocks of method S100 during a processing cycle to: spray a volume of separator material on a substrate; upon contact with the substrate, heat the substrate to quickly dry the volume of separator material and evaporate a first solvent (e.g., butanone) from the volume of separator material; dissolve a second polymer (e.g., PEG) from the volume of separator material by washing or rinsing the substrate in a chemical bath of a second solvent including an alcohol (e.g., isopropyl alcohol) to provide an open network having pores; and irradiate the volume of separator material with an electron beam to further crosslink the first polymer (e.g., PVDF-HFP) and form a separator membrane of uniform thickness, the separator membrane defining a network of open pores, the network of open pores being sized to transport ions (e.g., lithium ions) through the separator membrane.

[0014] Additionally, the system 100 can also monitor the temperature of the separator material in the gaseous environment in the container and the temperature of the liquid separator material in the reservoir of the coating supply subsystem to maintain the target vapor pressure and uniform polymer-polymer-solvent liquid mixture in the reservoir. In addition, the system 100 can use the target temperature range and target vapor pressure of the separator material to: achieve an accurate and repeatable liquid flow rate of the separator material through the nozzle of the spray system; and thereby achieve an accurate and repeatable separator material thickness on the substrate via spraying during the treatment cycle. The system 100 can also define (or reach) and achieve the time parameters and temperature parameters of the drying section of the treatment cycle to evaporate the first solvent (e.g., butanone) from the separator material of the coated substrate and control the phase separation of the first polymer (e.g., PVDF-HFP) and the second polymer (e.g., PEG).

[0015] Additionally or alternatively, the system 100 can: irradiate the volume of separator material to form a porous electrolyte structure extending beyond the perimeter of the substrate; and then fill the network of open pores with solvated ions to form an electrolyte. For example, the system 100 can perform the frame of the method to form an ion-carrying (e.g., lithium-carrying) electrolyte on the cathode and / or anode, which can then be assembled into a battery cell of a two-dimensional battery or a three-dimensional battery (e.g., for electric vehicles, wearable devices, cellular devices, or battery-operated tools). In addition, the electrolyte can be used as a buffer or electrode separator between the anode and cathode - assembled into the battery cell - to prevent the flow of electrons between the anode and cathode within the battery cell, and thereby prevent electrical short circuits within the battery.

[0016] Method S100 is described below as being performed by system 100 to: deposit (e.g., spray) a separator material on a substrate (e.g., an electrode); and form a thin film, or a discrete separator layer, or a permeable separator membrane of the separator material on the substrate via a processing cycle. However, method S100 can be similarly implemented to produce a thin film, a discrete separator layer, or a permeable separator membrane of the separator material directly on the cathode and / or anode, and / or to produce a separate, continuous non-conductive structure for subsequent assembly with the anode and cathode to form a two-dimensional battery or a three-dimensional battery, etc.

[0017] 3. System The system 100 includes: a substrate supply station 105; a spray system 110; a refill station 120; a washing station 130; and an irradiation station 140. The substrate supply station 105 includes a substrate reel (e.g., an electrode reel, an anode reel, a cathode reel) configured to deliver a substrate tape including a series of substrates to the spray system 110. The spray system 110 includes: a chassis 112; a multi-axis stage 113; a nozzle 114 and a coating supply subsystem 115 configured to selectively supply a liquid separator material (e.g., a polymer-polymer-solvent liquid mixture) from a reservoir to the nozzle 114; a gas regulator 116; a set of heaters 117; and a set of temperature sensors 118. The spray system 110 is configured to spray a volume of separator material onto a substrate.

[0018] The refilling station 120 includes a new supply of separator material (e.g., a polymer-polymer-solvent liquid mixture) and is configured to refill the reservoir of the spray system with the new supply of separator material. The washing station 130 includes a chemical bath of a second solvent such as an alcohol (e.g., isopropyl alcohol) and is configured to dissolve the second polymer out of the separator material on the substrate. The irradiation station 140 includes an electron beam configured to transmit electrons toward the substrate to crosslink the first polymer and form a separator film (e.g., a discrete separator layer, a permeable separator film) on the substrate.

[0019] 3.1 Base Supply Station In one embodiment, the substrate supply station 105 includes a substrate reel (e.g., an electrode reel, an anode reel, a cathode reel) configured to deliver a substrate tape comprising a series of substrates to the spray system 110. In particular, the substrate supply station 105 includes a substrate reel configured to deliver a cathode tape comprising a series of cathodes and / or an anode tape comprising a series of anodes from the substrate supply station to the spray system 110.

[0020] In one variation, the system 100 can trigger the substrate supply station 105 to load a cathode tape onto a substrate reel, and deliver a cathode reel including a first cathode in a series of cathodes from the substrate supply station to a coating area within the spray system 110. The system 100 can then receive a first portion of the cathode tape including a first cathode within the coating area, and implement the methods and techniques described below to spray a separator material on the first cathode occupying the coating area, dry the separator material on the first cathode, wash the first cathode with an alcohol bath, and irradiate the separator material and the first cathode with an electron beam to form a separator film on the first cathode in the first portion of the cathode tape.

[0021] Additionally or alternatively, the system 100 can trigger the substrate supply station 105 to load the anode strip onto the substrate reel, and transport the anode reel including the first anode in a series of anodes from the substrate supply station to the coating area within the spray system 110. The system 100 can then receive a first portion of the anode strip including the first anode in the coating area, and implement the methods and techniques described below to spray the separator material on the first anode occupying the coating area, dry the separator material on the first anode, wash the first anode with an alcohol bath, and irradiate the separator material and the first anode with an electron beam to form a separator film on the first anode in the first portion of the anode strip.

[0022] The system 100 may repeat these methods and techniques for each additional cathode in a series of cathodes, for each additional anode in a series of anodes, and for each additional portion of substrate tape to deliver substrate tape (eg, cathode tape, anode tape) to the spray system 110 .

[0023] 3.1 Spraying system The spray system 110 includes: a chassis 112 ; a multi-axis platform 113 ; a paint supply subsystem 115 ; a gas regulator 116 ; a set of heaters 117 ; and a set of temperature sensors 118 coupled to the paint supply subsystem 115 .

[0024] The chassis 112 defines an enclosure and is arranged around the spray system 110. The multi-axis platform 113 is configured to support a coating supply subsystem 115. The coating supply subsystem 115 is supported by the multi-axis platform 113 and includes: a container configured to contain a gaseous environment above a reservoir configured to contain a liquid separator material (e.g., a polymer-polymer-solvent liquid mixture); a first heater 117 configured to heat the reservoir of the liquid separator material; a nozzle 114 coupled to the reservoir, facing the substrate, and configured to spray a volume of the separator material from the reservoir onto the substrate; a second heater 117 coupled to the nozzle 114 and configured to heat the separator material before spraying the substrate; and a valve interposed between the reservoir and the nozzle 114.

[0025] The gas regulator 116 is coupled to the coating supply subsystem and is configured to regulate the pressure of the gas within the container of the coating supply subsystem 115. In one variation, the gas regulator 116 can increase the pressure of the gas within the container and through the nozzle 114 to remove excess separator material that may accumulate within the nozzle 114 over a period of time (e.g., one week, three weeks, one month).

[0026] The temperature sensor 118 may include a group of temperature sensors 118 configured to output signals corresponding to the temperature of the separator material at the reservoir, the temperature of the separator material at the nozzle 114, and the temperature of the substrate.

[0027] 3.1.1 Chassis + Stand (Gantry) Chassis 112 : defines an envelope and is disposed around the spray system 110 . The chassis 112 is configured to support a multi-axis platform and a coating supply subsystem 115 .

[0028] The multi-axis platform 113 includes a three-axis gantry (e.g., an X-axis, a Y-axis, and a Z-axis): the three-axis gantry is supported by the chassis 112; is arranged on a substrate occupying the encapsulation area; is configured to face a side of the substrate (e.g., arranged on a side of the substrate, under a side of the substrate, or adjacent to a side of the substrate); and is configured to support the coating supply subsystem 115 in a series of vertical positions, lateral positions, and longitudinal positions to enable the nozzle 114 to approach the edge of the substrate (e.g., an electrode) during a processing cycle.

[0029] In one variation, the multi-axis platform includes a five-axis gantry (e.g., X-axis, Y-axis, Z-axis, A-axis, and B-axis): the five-axis gantry is supported by a chassis 112; is disposed on a substrate occupying a coating area; is configured to face a side of the substrate; and is configured to support a coating supply subsystem 115 in a series of vertical, lateral, longitudinal, and rotational positions to enable the nozzle 114 to approach an edge of a substrate (e.g., an electrode) during a processing cycle.

[0030] 3.1.2 Paint supply subsystem The coating supply subsystem 115 is supported by the multi-axis platform 113 and includes: a container configured to contain a gaseous environment of the separator material; a reservoir arranged in the container and configured to contain the liquid separator material; a nozzle 114, which is connected to the reservoir and faces the substrate; a first heater 117, which is configured to heat the separator material; a second heater 117, which is connected to the nozzle 114 and configured to heat the separator material before spraying the substrate; a first valve, which is between the reservoir and the nozzle 114; and a second valve, which is arranged at the proximal end of the nozzle 114.

[0031] The first valve is operable in an open position to supply the separator material in a liquid state from the reservoir to the nozzle 114, and in a closed position to maintain the separator material in a liquid state in the reservoir and maintain a gaseous environment in the container. The second valve is operable in a closed position to prevent an existing volume of the first solvent (e.g., butanone) from entering the nozzle 114, and in an open position to supply an existing volume of the first solvent (e.g., butanone) through the nozzle 114, and thereby enable the nozzle 114 to be cleaned without disassembling the coating supply subsystem 115.

[0032] 3.1.3 Temperature Sensor In one embodiment, the spray system 110 includes a set of temperature sensors 118 (e.g., PID sensors, thermocouples) coupled to the coating supply subsystem 115 and / or the substrate occupying the encapsulation area. The temperature sensors 118 are configured to output signals corresponding to the temperature of the separator material during the treatment cycle.

[0033] In one variation, the system 100 may include: a first temperature sensor 118 coupled to the container and configured to output a signal corresponding to the temperature of the separator material in the gaseous environment; a second temperature sensor 118 coupled to the nozzle 114 and configured to output a signal corresponding to the temperature of the separator material in a liquid state before exiting the nozzle 114; and a third temperature sensor 118 coupled to the spray system 110 and configured to output a signal corresponding to the temperature of the substrate. The system 100 may then: interpret the temperature of the separator material and / or substrate; monitor the temperature; and derive a correlation between the temperature and the vapor pressure of the gaseous environment prior to commencing the coating segment of the treatment cycle, as further described below.

[0034] 4. Separator material: polymer-polymer-solvent liquid mixture Typically, the separator material is a polymer-polymer-solvent liquid mixture and comprises: a first solvent; a first polymer miscible in the first solvent; and a second polymer miscible in the first solvent. The polymer-polymer-solvent liquid mixture comprises greater than 80% by weight of the first solvent and comprises a low viscosity to enable the nozzle to deposit a series of separator material droplets (e.g., aerosol) on the porous substrate and adhere to the surface of the porous substrate.

[0035] In one embodiment, the first solvent includes an organic ketone, such as butanone, and the organic ketone is characterized by a boiling point of 79.64 degrees Celsius or 175.26 degrees Fahrenheit. The first polymer includes a copolymer, such as poly (vinylidene fluoride-hexafluoropropylene) (or "PVDF-HFP"), and is characterized by a molecular weight of about 400,000 grams per mole. The second polymer includes a polyether, such as polyethylene oxide (or "PEO"), poly (ethylene oxide) (or "POE") or polyethylene glycol (or "PEG"), and is characterized by a molecular weight of about 20,000 grams per mole. In this embodiment, the first polymer (such as PVDF-HFP) and the second polymer (such as PEG) are mixed in the first solvent (such as butanone) to form a homogeneous polymer-polymer-solvent liquid mixture showing a first solvent greater than 80% by weight.

[0036] In one modification, the polymer-polymer-solvent liquid mixture comprises a first solvent (e.g., butanone), and a first polymer (e.g., PVDF-HFP) and a second polymer (e.g., PEG) mixed in the first solvent. In this modification, the system 100 can heat the polymer-polymer-solvent liquid mixture toward the target liquid temperature range, so that the polymer-polymer-solvent liquid mixture is maintained as a homogeneous mixture in the reservoir and at the nozzle of the coating supply subsystem. Additionally, the first polymer (e.g., PVDF-HFP) is immiscible with the second polymer (e.g., PEG), and vice versa.

[0037] In addition, during the treatment cycle, the system 100 sprays the polymer-polymer-solvent liquid mixture as an aerosol (or a "series" of separator material droplets, a "mist" or a "cloud" of separator material droplets) on the substrate occupying the coating area. For example, the polymer-polymer-solvent liquid mixture can show less than 20% by weight of the first solvent (e.g., between 15% and 20% by weight of butanone). Upon initial contact between the series of separator material droplets and the substrate, the system 100 further rapidly dries the series of separator material droplets, such as by using a heater coupled to the substrate, thereby promoting phase separation of the first polymer (e.g., PVDF-HFP) and the second polymer (e.g., PEG). Then, the system 100 washes, rinses or sprays the substrate with a volume of a second solvent, such as with an alcohol (e.g., isopropanol), dissolving the second polymer (e.g., PVDF-HFP) from the series of separator material droplets. The resulting series of droplets of separator material, from which the second polymer has been removed, can thereby form a continuous film (eg, an aerosol) defining a network of voids distributed throughout its volume.

[0038] The system 100 then selectively irradiates the series of separator material droplets and the substrate via an electron beam to further crosslink the molecules of the first polymer (e.g., PVDF-HFP) and form a separator membrane (e.g., a discrete separator layer, a permeable separator membrane) across the substrate. Thus, the separator membrane defines an open pore network having pores that are sized to: promote uniform and rapid ion transport; prevent defects from forming on the substrate; and thereby prevent electrical shorting between the substrate and the anode or cathode in the battery cell, such as due to dendrite growth from the anode into the separator membrane, as further described below.

[0039] 5. Processing loops At the beginning of a processing cycle (e.g., a spray deposition cycle, a spray treatment cycle), the system 100 resets the multi-axis platform to a home position facing the coating area. Then, the substrate supply station delivers a series of substrates (e.g., anodes, cathodes) to the spray system so that the substrates (e.g., anodes, cathodes) occupy the coating area. Then, the system 100 starts a processing cycle (e.g., a spray deposition cycle, a spray treatment cycle).

[0040] The system 100 washes or rinses the substrate with a second solvent to dissolve the second polymer from the separator material, thereby providing an open network with pores. The system 100 then irradiates the separator material and the substrate with an electron beam to further crosslink the first polymer and form a separator layer. The resulting separator layer is non-conductive and includes an open network with pores that are sized to transport ions (e.g., lithium ions) through the separator layer and between adjacent anodes and cathodes within the assembled battery cell.

[0041] 5.1 Coating section Once the system 100 initiates a processing cycle, the system 100 may trigger the multi-axis stage to position the coating supply subsystem to face the substrate within the encapsulation area and initiate the first encapsulation segment of the processing cycle.

[0042] Prior to initiating the first coating segment of the process cycle, the system 100 can reach a target gas temperature range for the separator material in the gaseous environment in the container, a target liquid temperature range for the separator material in the liquid state at the nozzle, and a target substrate temperature for the substrate in the drying segment of the process cycle. Then, during the first coating segment of the process cycle, the system 100 can deposit (or "spray") a volume of separator material (or "a series of separator material droplets") as an aerosol via the nozzle across all surfaces and / or edges of the substrate (e.g., anode, cathode) occupying the coating area.

[0043] In particular, the system 100 can: configure a valve arranged in the coating supply subsystem to an open position to deliver a liquid separator material (e.g., a polymer-polymer-solvent liquid mixture) from a reservoir to a nozzle; and spray a series of separator material droplets on the substrate in the coating area, so that each droplet in the series of separator material droplets contains a molecule of a first polymer (e.g., PVDF-HFP) defining a small cross-sectional width: the small cross-sectional width is greater than the minimum cross-sectional width of lithium ions; and is less than the minimum cross-sectional width of the substrate thickness (e.g., 50 microns, 100 microns). Therefore, the series of separator material droplets can encapsulate the edge of the substrate (e.g., anode, cathode). In addition, in box S120, the system 100 can spray a series of separator material droplets on the substrate, each droplet in the series of separator material droplets containing a first solvent (e.g., butanone), a first polymer miscible in the first solvent (e.g., PVDF-HFP), and a second polymer miscible in the first solvent (e.g., PEG).

[0044] In addition, the system 100 can detect a minimum volume of separator material in liquid form within the reservoir and track the volume of separator material exiting the nozzle for each coating segment of the process cycle. The system 100 can then derive a correlation between the total volume of separator material exiting the nozzle for each coating segment and, in response to the total volume of separator material exceeding the minimum volume of separator material, trigger the refill station to refill the reservoir with a new volume of separator material.

[0045] 5.1.1 Temperature and pressure adjustment of partition material Before spraying the separator material onto the substrate occupying the coating area, the system 100 can define a target gas temperature range for the first solvent of the gaseous environment of the container and a target liquid temperature range for the separator material of the reservoir, which produces a target flow rate of the separator material through the nozzle. The system 100 can then monitor the temperature of the separator material in the container and the reservoir based on signals from a set of temperature sensors connected to the coating supply subsystem. In addition, the system 100 can adjust the temperature of the gaseous environment and the separator material to the target temperature range with a heater connected to the coating supply subsystem and the nozzle to maintain the target flow rate of the separator material through the nozzle.

[0046] In one embodiment, the system 100 can define a target gas temperature range corresponding to a target vapor pressure of a first solvent in a gaseous environment within a container. In particular, the system 100 can: reach a target gas temperature range proportional to the vapor pressure of a separator material (e.g., a polymer-polymer-solvent liquid mixture) in a gaseous environment within a container; detect a temperature of the first solvent in the gaseous environment; and initiate a coating segment of a treatment cycle based on the temperature.

[0047] For example, the system 100 may: define a target gas temperature range for the first solvent; heat the gaseous environment toward the target gas temperature range at a container containing the gaseous environment above a reservoir of separator material in a liquid state; and interpret a first temperature of the gaseous environment within the container based on a first signal from a first temperature sensor coupled to a coating supply subsystem. Then, in response to the first temperature of the gaseous environment falling within the target gas temperature range, the system 100 may initiate a coating segment of a processing cycle and spray a series of separator material droplets through a nozzle and onto a substrate.

[0048] In another embodiment, the system 100 may similarly define a target liquid temperature range for the separator material to maintain a homogeneous polymer-polymer-solvent liquid mixture within the reservoir; detect the temperature of the separator material in a liquid state at the nozzle; and based on the temperature, initiate a coating segment of the treatment cycle. For example, the system 100 may: define a target liquid temperature range for the separator material; at a nozzle coupled to a reservoir of the separator material in a liquid state and facing the substrate, heat the nozzle toward the target liquid temperature range; and interpret a first temperature of the separator material at the nozzle based on a signal from a temperature sensor coupled to a coating supply subsystem. Then, in response to the first temperature of the separator material falling within the target liquid temperature range, the system 100 may initiate the coating segment of the treatment cycle and spray a series of separator material droplets onto the substrate via the nozzle.

[0049] Additionally, the system 100 may define a target gas temperature range for the first solvent that is equivalent to a target liquid temperature range for the separator material, detect the temperature of the separator material in a liquid state at the nozzle and the temperature in the gaseous environment, and then initiate a coating segment of the treatment cycle based on these temperatures of the separator material in a liquid state and the first solvent in the gaseous environment. For example, the system 100 may: define a target gas temperature range for the first solvent corresponding to a target vapor pressure for the separator material in a gaseous state; heat the gaseous environment toward the target gas temperature range at a container containing the gaseous environment above a reservoir of the separator material in a liquid state; interpret the first temperature of the gaseous environment based on a first signal from a first temperature sensor coupled to a coating supply subsystem; define a target liquid temperature range for the separator material; heat the nozzle toward the target liquid temperature range at a nozzle coupled to a reservoir of the separator material in a liquid state and facing the substrate; and interpret a second temperature of the separator material in a liquid state at the nozzle based on a second signal from a second temperature sensor coupled to the coating supply subsystem. Then, in response to a first temperature of the gaseous environment falling within a target gas temperature range and in response to a second temperature of the separator material falling within a target liquid temperature range, the system 100 can spray a series of separator material droplets onto the substrate via the nozzle.

[0050] Alternatively, in response to the first temperature of the gaseous environment falling outside the target gas temperature range and in response to the second temperature of the separator material falling outside the target liquid temperature range, the system 100 may: heat the gaseous environment toward the target gas temperature range via a first heater coupled to the container; heat the separator material in a liquid state toward the target liquid temperature range via a second heater coupled to the nozzle; interpret a third temperature of the gaseous environment based on a signal from the first temperature sensor; and interpret a fourth temperature of the separator material in a liquid state at the nozzle based on a signal from the second temperature sensor. Then, in response to the third temperature of the gaseous environment falling within the target gas temperature range and in response to the fourth temperature of the separator material falling within the target liquid temperature range, the system 100 may spray a series of separator material droplets on the substrate via the nozzle.

[0051] Thus, the system 100 can monitor the temperature of the first solvent in the gaseous environment and in the liquid state to maintain a target vapor pressure and a homogeneous polymer-polymer-solvent liquid mixture in the reservoir. Additionally, the system 100 can utilize a target temperature range and a target vapor pressure to achieve an accurate and repeatable flow rate of the separator material through the nozzle to spray the separator material on the substrate during the coating section of the processing cycle.

[0052] 5.1.2 Thickness of partition In one embodiment, the system 100 can trigger the multi-axis platform to position the nozzle of the spray system at a target offset distance relative to the substrate within the encapsulation area. More specifically, the system 100 can receive a target separator thickness of a separator film (e.g., a discrete separator layer, a permeable separator film) formed during the irradiation of a series of separator material droplets, and select a target offset distance between the nozzle and the substrate that is proportional to the target separator thickness.

[0053] In one variation, system 100 can set a target offset distance for the nozzle based on battery specifications (e.g., multi-cell batteries for electric vehicles, single-cell batteries for wearable devices) and corresponding mechanical properties, electrical properties, optical properties, and / or physical properties of a separator film formed on a substrate (e.g., anode, cathode).

[0054] For example, a user may require a separator film with a target separator thickness for a multi-cell battery for an electric vehicle, and define a battery specification for the multi-cell battery that exhibits low resistance, large ion flux, target conductivity, and high mechanical strength to withstand forces applied during subsequent assembly into a battery cell. The system 100 can then: receive a battery specification that defines a target separator thickness (e.g., 10 microns) for the separator film; select a target offset distance of the nozzle relative to the substrate based on the target separator thickness; and detect a first distance between the nozzle and the substrate within the coating area by interpreting a signal from a depth sensor coupled to a coating supply subsystem. Then, in response to the target offset distance exceeding the first distance between the nozzle and the substrate, the system 100 can: trigger the multi-axis to adjust the nozzle from the first distance to the target offset distance; and spray a series of separator material droplets on a first portion of the substrate via the nozzle at the target offset distance. The system 100 can then spray a second series of separator material droplets onto a second portion of the substrate and implement the methods and techniques described below to form a separator membrane - exhibiting low electrical resistance, large ion flux, and high mechanical strength - where the separator thickness is close to the target separator thickness (e.g., 10 microns + / - 0.01 microns, 10 microns + / - 0.1 microns).

[0055] Thus, system 100 can spray discrete portions or sections of a substrate with separator material via nozzles located at a target offset distance from the substrate to form a thin separator film of a target separator thickness according to specific battery specifications, such as defined by an operator.

[0056] 5.1.3 Refilling the reservoir with separator material In one embodiment, system 100 can detect a minimum volume of liquid separator material in a reservoir and track the volume of separator material exiting the nozzle for each coating segment of a processing cycle to trigger a refill station to refill the reservoir with a new volume of separator material.

[0057] For example, during a first coating segment of a processing cycle, the system 100 may: detect a minimum volume of separator material in a liquid state in a reservoir; receive a first substrate in a coating zone; define a target liquid temperature range for the separator material in a liquid state in the reservoir; detect a first temperature of the separator material at a nozzle; and in response to a second temperature of the separator material falling within the target liquid temperature range, spray a first volume of separator material on the first substrate via the nozzle. Then, during a second coating segment of the processing cycle, the system 100 may: receive a second substrate in the coating zone; heat the nozzle toward the target liquid temperature range; detect a second temperature of the separator material at the nozzle; and in response to the second temperature of the separator material falling within the target liquid temperature range, spray a second volume of separator material on the second substrate via the nozzle. Then, the system 100 may: calculate a total volume of separator material on the first substrate and the second substrate based on a combination of the first volume of separator material and the second volume of separator material; and in response to the minimum volume of separator material exceeding the total volume of separator material, refill the reservoir with a third volume of separator material in a liquid state that is greater than the minimum volume of separator material.

[0058] Thus, system 100 may track the volume of separator material exiting the nozzle during each coating segment of a processing cycle and refill the reservoir with a volume of liquid separator material if the minimum volume of separator material exceeds the total volume of separator material exiting the nozzle.

[0059] 5.2 Drying section: removal of the first solvent + phase separation During the second drying segment of the processing cycle, the system 100 can quickly and simultaneously dry each of the series of separator material droplets after the series of separator material droplets contact the substrate. In addition, the system 100 can heat the substrate and the series of separator material droplets to a temperature within a target temperature range proportional to the boiling point of the first solvent for a period of time. During the drying segment, the system 100 can also evaporate the first solvent from each of the series of separator material droplets and promote phase separation of the second polymer (e.g., PEG) and the first polymer (e.g., PVDF-HFP) on the substrate.

[0060] In one embodiment, the system 100 can set the time parameters and temperature parameters of the drying section of the processing cycle to control the phase separation of the first polymer (e.g., PVDF-HFP) and the second polymer (e.g., PEG). In particular, in box S122, the system 100 can reach a target substrate temperature range proportional to the boiling point of the first solvent (e.g., butanone). Then, in box S130, the system 100 can heat the substrate and the series of separator material droplets for a duration (e.g., 10 seconds, 30 seconds) to evaporate the first solvent from the separator material. More specifically, the system 100 can reach a target substrate temperature range, such as between 74 degrees Celsius and 79 degrees Celsius; between 77 degrees Celsius and 79 degrees Celsius; and / or between 78.9 degrees Celsius and 79.4 degrees Celsius, etc. Then, the system 100 can start the drying section of the processing cycle and heat the series of separator material droplets and the substrate to a temperature within the target substrate temperature range.

[0061] For example, the system 100 can spray a series of separator material droplets on the substrate during the coating section of the processing cycle. In this example, each droplet in the series of separator material droplets includes: a first solvent, which includes a first volume of an organic ketone solvent (e.g., butanone); a first polymer, which is miscible in the first volume of the organic ketone solvent and includes a second volume of a copolymer (e.g., PVDF-HFP); and a second polymer, which is miscible in the first volume of the organic ketone solvent and includes a third volume of a polyether (e.g., PEG). The system 100 can then: reach a target substrate temperature that is below the boiling point of the organic ketone solvent (e.g., between 77 degrees Celsius and 79 degrees Celsius); initiate a drying segment of a processing cycle; and heat the substrate and the series of separator material droplets to a temperature within the target substrate temperature range (e.g., 78 degrees Celsius) via a heater coupled to the substrate to evaporate a first volume of the organic ketone solvent (e.g., butanone) from the series of separator material droplets and promote phase separation of the second polymer (e.g., PEG) from the first polymer (e.g., PVDF-HFP).

[0062] However, the series of separator material droplets and the substrate may be processed for any other duration or at any other temperature during the second drying segment of the processing cycle.

[0063] The system 100 can then transport the substrate to a washing assembly to wash or rinse the series of separator material droplets with a second solvent to dissolve the second polymer from the series of separator material droplets and thereby provide an open pore network having pores.

[0064] 5.3 Washing section: Removal of the second polymer During the third washing section of the treatment cycle, the system 100 can dissolve the second polymer (e.g., PEG) from the series of separator material droplets by washing or rinsing the series of separator material droplets with a chemical bath containing a second solvent (e.g., alcohol) to provide an open-pore network with pores. In addition, in block S140, the system 100 can wash the substrate and the series of separator material droplets with a second solvent to form an open-pore network with pores distributed throughout the series of separator material droplets.

[0065] In one embodiment, the system 100 can receive a series of separator material droplets and a substrate from a spray system in a wash station, each droplet comprising a first volume of a first polymer (e.g., PVDF-HFP) and a second volume of a second polymer (e.g., PEG). At the wash station, the system 100 can then dissolve the second volume of the second polymer (e.g., PEG) from the series of separator material droplets to provide an open pore network with pores by washing the series of separator material droplets with a second solvent comprising a third volume of an alcohol (e.g., isopropanol), wherein the second solvent can completely swell the substrate, dissolve the second polymer (e.g., PEG) from the pores in the separator material to provide open channels for transporting ions through the separator material.

[0066] In one variation, the system 100 can perform the blocks of method S100 to rinse the series of separator material droplets and substrates with a second solvent (e.g., isopropyl alcohol) to provide an open pore network having pores; and project an air stream onto the series of separator material droplets and substrates to remove excess isopropyl alcohol remaining from the chemical bath from the series of separator material droplets and substrates. For example, the substrate can be immersed in a heated bath of the second solvent (e.g., isopropyl alcohol) and stirred for a duration, removed from the bath and dried to remove the second polymer (e.g., PEG) from the separator material.

[0067] Furthermore, the system 100 can then transport the substrate to an irradiation station, which then irradiates the series of separator material droplets on the substrate, thereby promoting cross-linking of the first polymer (eg, PVDF-HFP) to form a separator membrane having an open network with pores.

[0068] 5.4 Irradiation section: thin film During the fourth irradiation segment of the processing cycle, in block S150, the system 100 can irradiate the series of separator material droplets and the substrate to crosslink the first polymer and form a separator membrane (e.g., a discrete separator layer, a permeable separator membrane) on the substrate, the separator membrane having an open pore network with pores, the open pore network with pores being sized to transmit ions through the separator membrane. In particular, the system 100 can selectively expose the substrate to an electron beam to further crosslink the molecules within the first polymer (e.g., PVDF-HFP) and form a separator membrane.

[0069] In one embodiment, the irradiation station includes an electron beam configured to transmit electrons toward the series of separator material droplets and the substrate to cross-link the molecules within the first polymer (e.g., PVDF-HFP) to form a polymer matrix, to flash dry any remaining solvent from the substrate, and to form a separator film on the substrate.

[0070] In one variation, the system 100 may receive a first substrate including a cathode at an irradiation station, and then receive a second substrate including an anode from a cleaning station at the irradiation station. In this variation, the system 100 may receive a cathode and an anode, wherein a second polymer (e.g., PEG) is removed from the series of separator material droplets; and electrons are transmitted toward the cathode and the anode via an electron beam to form a continuous non-conductive structure extending beyond the perimeter of the cathode and beyond the perimeter of the anode.

[0071] For example, the system 100 can receive a first substrate including a cathode at an irradiation station, and irradiate the series of separator material droplets and the cathode with an electron beam to crosslink the first polymer (e.g., PVDF-HFP) and form a continuous non-conductive structure: define a separator membrane, the separator membrane has an open network with pores, the open network with pores is sized to transmit ions through the separator membrane; and extends beyond the perimeter of the cathode. Then, the system 100 can receive a second substrate including an anode at an irradiation station, and irradiate the series of separator material droplets and the anode with an electron beam to crosslink the molecules within the first polymer (e.g., PVDF-HFP) and form a continuous non-conductive structure: define a separator membrane, the separator membrane has an open network with pores, the open network with pores is sized to transmit ions through the separator membrane; and extends beyond the perimeter of the anode. Therefore, after the anode and cathode are subsequently assembled into a battery cell for post-processing, the continuous non-conductive structure can prevent the flow of electrons between the anode and the cathode, such as preventing an electrical short circuit in the battery cell.

[0072] Additionally or alternatively, the system 100 can irradiate the series of separator material droplets and the cathode and / or anode via an electron beam to crosslink the first polymer and form a separator membrane on the cathode and / or anode, the separator membrane comprising a permeable separator membrane having an open network of pores, the open network of pores being sized to transmit ions through the permeable separator membrane.

[0073] Thus, system 100 can irradiate the series of separator material droplets after quickly drying and washing the substrate to form a rigid, continuous non-conductive structure of uniform thickness on the substrate, and thereby form a separator material film exhibiting target mechanical properties, electrical properties, optical properties, and physical properties.

[0074] 6. Post-processing of battery components: introduction of solvated ions In one variation, the separator membrane can form a porous electrolyte structure extending beyond the periphery of the substrate (e.g., cathode, anode) during the last irradiation segment of the treatment cycle. The system 100 can then expose the electrolyte structure to a solvent (e.g., an organic solvent) and ions to fill a network of open pores in the electrolyte structure with solvated ions to form an electrolyte. In this variation, the system 100 can introduce solvated ions (e.g., lithium ions) into the electrolyte structure to fill the network of open pores, and thereby enable the electrolyte structure to be used as an electrolyte carrying ions (e.g., carrying lithium ions) in a subsequently assembled battery cell for an electric vehicle or wearable device.

[0075] Thus, the system 100 can perform a processing cycle to form a porous electrolyte structure extending beyond the perimeter of the anode or cathode, and then fill the network of open pores with solvated ions to form an electrolyte. Alternatively, the electrolyte can be used as a buffer or electrode separator between the anode and cathode, and then assembled into a battery cell to prevent the flow of electrons between the anode and cathode inside the battery cell (i.e., to prevent electrical short circuits).

[0076] 7. Variant: Parallel nozzles In one variation, the coating supply subsystem may include a set of nozzles coupled in parallel by a valve so that each nozzle in the set of nozzles can simultaneously spray the diaphragm material onto the substrate to obtain a diaphragm film exhibiting a uniform target thickness across the substrate. In this variation, the valve may include a chemically resistant solenoid valve that tolerates a first solvent (e.g., butanone) in the polymer-polymer-solvent liquid mixture, operable in an open position and a closed position to maintain the vapor pressure of the polymer-polymer-solvent liquid mixture within each nozzle of the coating supply subsystem.

[0077] For example, the coating supply subsystem may include a set (e.g., 3) of nozzles: connected in parallel by a solenoid valve; defining a coating zone; and configured to simultaneously spray the separator material onto the substrate within the coating zone. At a first time, the system 100 may: receive a first portion of a substrate strip including a first substrate within the coating zone; spray a first series of separator material droplets onto the first portion of the first substrate via a first nozzle; spray a second series of separator material droplets onto the second portion of the first substrate via a second nozzle; and spray a third series of separator material droplets onto a third portion of the first substrate, the third portion being between the first portion and the second portion of the first substrate, via a third nozzle.

[0078] At a second time after the first time, the system 100 can implement the methods and techniques described above to: heat the first substrate to a target substrate temperature to simultaneously and quickly dry the first series of separator material droplets, the second series of separator material droplets, and the third series of separator material droplets on the first substrate to evaporate the first solvent (e.g., butanone) from the first series of separator material droplets, the second series of separator material droplets, and the third series of separator material droplets; wash the first series of separator material droplets, the second series of separator material droplets, and the third series of separator material droplets with a second solvent (e.g., isopropyl alcohol); The invention relates to a method for coating a first substrate and a second substrate. The method comprises the steps of: coating a first substrate and a third substrate; dissolving a second polymer (e.g., PEG) from the first substrate, the second substrate and the third substrate; and irradiating the first substrate, the second substrate and the third substrate with an electron beam to crosslink the first polymer (e.g., PVDF-HFP) to form a membrane of the membrane material extending beyond the periphery of the first substrate (e.g., encapsulating all sides of the first substrate). Thus, each nozzle in the coating supply subsystem can spray a corresponding portion of the substrate to obtain a membrane of uniform target thickness.

[0079] Additionally or alternatively, the coating supply subsystem may include a set (e.g., 3) of nozzles: connected in parallel by a solenoid valve; defining a set (e.g., 3) of enveloping zones; and configured to spray the separator material onto a corresponding substrate in a series of substrates within each enveloping zone. In this variation, the system 100 may batch process a series of substrates simultaneously during a processing cycle.

[0080] For example, at a first time, the system 100 may: receive a first portion of the substrate strip including the first substrate in a first coating zone; receive a second portion of the substrate strip including the second substrate in a second coating zone; and receive a third portion of the substrate strip including the third substrate in a third coating zone. At about the first time, the system 100 may: spray a first series of separator material droplets on the first substrate via a first nozzle; spray a second series of separator material droplets on the second substrate via a second nozzle; and spray a third series of separator material droplets on the third substrate via a third nozzle. At a second time after the first time, system 100 can implement the methods and techniques described above to: heat the first substrate, the second substrate, and the third substrate to a target substrate temperature to simultaneously and quickly dry the first series of separator material droplets, the second series of separator material droplets, and the third series of separator material droplets on the first substrate, the second substrate, and the third substrate to evaporate the first solvent (e.g., butanone) from the first series of separator material droplets, the second series of separator material droplets, and the third series of separator material droplets; wash the first series of separator material droplets, the second series of separator material droplets, and the third series of separator material droplets and the first substrate, the second substrate, and the third substrate with a second solvent (e.g., isopropyl alcohol); The invention relates to a method for coating a plurality of substrates, wherein the first series of separator material droplets, the second series of separator material droplets, and the third series of separator material droplets are coated with a first separator material film extending beyond the periphery of the first substrate (e.g., encapsulating all sides of the first substrate), a second separator material film extending beyond the periphery of the second substrate, and a third separator material film extending beyond the periphery of the third substrate. Thus, each nozzle in the coating supply subsystem can spray a corresponding substrate in a series of substrates to obtain a separator material film of uniform target thickness on a series of substrates in a batch coating process.

[0081] 8. Application of other partition materials Typically, the above describes a method S100 for manufacturing a conformable rigid separator membrane in a 2D or 3D lithium-ion battery for an electric vehicle, such as by manufacturing a separator membrane of uniform thickness on a planar anode, and then assembling a planar cathode on the separator membrane. However, in the case of manufacturing a 3D battery on a silicon wafer, similar methods and techniques can be implemented to produce a conformable rigid separator membrane. Similarly, these methods, techniques, and materials can be implemented to produce a 2D or 3D hydrogen fuel cell comprising a separator membrane, the separator membrane defining a controlled density and distribution of relatively large pores, which can improve hydrogen ion conduction through the fuel cell. In addition, these methods, techniques, and materials can be implemented to produce a 2D or 3D nickel metal hydride battery comprising a separator membrane, the separator membrane defining a controlled density and distribution of relatively large pores, which can improve hydrogen ion conduction through the nickel metal hydride battery.

[0082] However, the separator material can be applied and processed in any other manner to form a conformable rigid separator membrane. Similarly, method S100 can be implemented in any other manner to manufacture a conformable rigid separator membrane, such as manufacturing a conformable rigid separator membrane directly on an electrode or manufacturing a conformable rigid separator membrane separately from an electrode.

[0083] The system 100 and method described herein may be at least partially embodied and / or implemented as a machine configured to receive a computer-readable medium storing computer-readable instructions. Instructions may be performed by a computer-executable component integrated with an application, applet, host, server, network, website, communication service, communication interface, hardware / firmware / software element of a user's computer or mobile device, wristband, smart phone, or any suitable combination thereof. Other systems 100 and methods of the embodiment may be at least partially embodied and / or implemented as a machine configured to receive a computer-readable medium storing computer-readable instructions. Instructions may be performed by a computer-executable component integrated with a computer-executable component integrated with the above-mentioned type of device and network. Computer-readable media may be stored on any suitable computer-readable medium, such as RAM, ROM, flash memory, EEPROM, optical device (CD or DVD), hard drive, floppy disk drive, or any suitable device. The computer-executable component may be a processor, but any suitable dedicated hardware device may (optionally or additionally) execute instructions.

[0084] As those skilled in the art will recognize from the previous detailed description and from the accompanying drawings and claims, modifications and variations may be made to the embodiments of the invention without departing from the scope of the invention as defined in the appended claims.

Claims

1. A method for depositing a separator material, comprising: During the first period: receiving a first substrate in the encapsulation region; spraying a series of separator material droplets on the first substrate, each droplet in the series of separator material droplets comprising a first solvent, a first polymer miscible in the first solvent, and a second polymer miscible in the first solvent; and reaching a target substrate temperature below the boiling point of the first solvent; and During a second time period following said first time period: heating the first substrate and the series of separator material droplets to the target substrate temperature to evaporate the first solvent from the series of separator material droplets and promote phase separation of the second polymer from the first polymer; washing the series of separator material droplets with a second solvent to dissolve the second polymer from the series of separator material droplets and provide an open pore network having pores within the series of separator material droplets; and The series of separator material droplets and the first substrate are irradiated to crosslink the first polymer and form a separator membrane on the first substrate, the separator membrane defining the open network of pores sized to transmit ions.

2. The method according to claim 1: Also included is, during the first time period: defining a target gas temperature range for the first solvent, the target gas temperature range corresponding to a target vapor pressure of the separator material in a gaseous environment; at a container containing a gaseous environment of the first solvent above a reservoir of separator material in a liquid state, heating the gaseous environment toward the target gas temperature range; and detecting a second temperature of the gaseous environment; and Wherein spraying the series of separator material droplets on the first substrate includes spraying the series of separator material droplets on the first substrate in response to the second temperature of the separator material falling within the target gas temperature range.

3. The method according to claim 1: Also included is, during the first time period: defining a target liquid temperature range for the separator material; at a nozzle coupled to a reservoir of separator material in a liquid state and facing the first substrate, heating the nozzle toward the target liquid temperature range; and detecting a second temperature of the partition material at the nozzle; and Wherein spraying the series of separator material droplets on the first substrate includes spraying the series of separator material droplets on the first substrate via the nozzle in response to the second temperature falling within the target liquid temperature range.

4. The method according to claim 3: Also included is, during the first time period: receiving a target separator thickness for the separator film; selecting a target offset distance between the nozzle and the first substrate based on the target diaphragm thickness; detecting a first distance between the nozzle and the first substrate in the encapsulation area; and in response to the target offset distance exceeding the first distance between the nozzle and the first substrate, adjusting the first distance to the target offset distance between the nozzle and the first substrate; wherein spraying the series of separator material droplets on the first substrate comprises spraying the series of separator material droplets on the first substrate via the nozzle at the target offset distance; and Wherein irradiating the series of separator material droplets and the first substrate includes irradiating the series of separator material droplets and the first substrate to crosslink the first polymer and form a separator film exhibiting a separator thickness close to the target separator thickness.

5. The method according to claim 1: wherein receiving the first substrate comprises receiving the first substrate including a cathode in the encapsulation region; wherein spraying the series of separator material droplets on the first substrate comprises spraying the series of separator material droplets on the cathode; and wherein irradiating the series of separator material droplets and the first substrate comprises irradiating the series of separator material droplets and the cathode with an electron beam to crosslink the first polymer and form a continuous non-conductive structure: The continuous non-conductive structure defines the separator membrane having an open pore network having pores, the open pore network having pores being sized to transmit ions through the separator membrane; and The continuous non-conductive structure extends beyond the perimeter of the cathode.

6. The method according to claim 1: wherein receiving the first substrate comprises receiving the first substrate including an anode within the encapsulation region; wherein spraying the series of separator material droplets on the first substrate comprises spraying the series of separator material droplets on the anode; and wherein irradiating the series of separator material droplets and the first substrate comprises irradiating the series of separator material droplets and the anode with an electron beam to crosslink the first polymer and form a continuous non-conductive structure: The continuous non-conductive structure defines the separator membrane having an open pore network having pores, the open pore network having pores being sized to transmit ions through the separator membrane; and The continuous non-conductive structure extends beyond the perimeter of the anode.

7. The method according to claim 1: Also included is defining, during the first time period, a target separator thickness corresponding to a target conductivity of the separator film; and Wherein irradiating the series of separator material droplets and the first substrate to crosslink the first polymer and form the separator film includes irradiating the series of separator material droplets and the first substrate to crosslink the first polymer and form the separator film having a separator thickness close to the target separator thickness.

8. The method according to claim 1: Also included is receiving, during the first time period, a target separator thickness for the separator film; Wherein spraying the series of separator material droplets comprises: spraying the series of separator material droplets on the first substrate at a first nozzle coupled to a reservoir of separator material in liquid form and facing the first substrate; Also included is spraying a second series of separator material droplets on the first substrate at a second nozzle coupled to a reservoir of the separator material during the second time period, each droplet in the second series of separator material droplets comprising the first solvent, the first polymer, and the second polymer; and Wherein irradiating the series of separator material droplets and the first substrate to cross-link the first polymer and form the separator film includes irradiating the series of separator material droplets, the second series of separator material droplets and the first substrate to cross-link the first polymer and form the separator film having a separator thickness close to the target separator thickness.

9. The method according to claim 1: Wherein spraying the series of separator material droplets on the first substrate includes spraying the series of separator material droplets on the first substrate, each droplet in the series of separator material droplets comprising: the first solvent, the first solvent comprising a first volume of an organic ketone solvent; the first polymer, the first polymer being miscible in the first volume of the organic ketone solvent and comprising a second volume of a copolymer; and the second polymer, the second polymer being miscible in the first volume of the organic ketone solvent and comprising a third volume of the polyether; wherein reaching the target substrate temperature comprises reaching the target substrate temperature below the boiling point of the organic ketone solvent; and Wherein heating the first substrate and the series of separator material droplets to the target substrate temperature to evaporate the first solvent includes heating the first substrate and the series of separator material droplets to the target substrate temperature to evaporate the first volume of organic ketone solvent from the series of separator material droplets and promote phase separation of the second polymer from the first polymer.

10. The method of claim 9, wherein washing the series of separator material droplets with the second solvent comprises washing the series of separator material droplets with the second solvent comprising a fourth volume of alcohol to dissolve the third volume of polyether from the series of separator material droplets and provide the open pore network having pores within the series of separator material droplets.

11. The method of claim 1 , wherein spraying the series of separator material droplets on the first substrate comprises spraying the series of separator material droplets on the first substrate, each droplet in the series of separator material droplets comprising molecules of the first polymer defining a small cross-sectional width: The small cross-sectional width is greater than the minimum cross-sectional width of a lithium ion; and The small cross-sectional width is smaller than the minimum cross-sectional width of the substrate thickness.

12. The method according to claim 1: wherein receiving the first substrate within the encapsulation region comprises receiving a first portion of a substrate strip including the first substrate within the encapsulation region; Also included is, during a third time period after the first time period: receiving a second portion of the substrate strip including a second substrate within the encapsulation region; and spraying a second series of separator material droplets on the second substrate, each droplet in the second series of separator material droplets comprising the first solvent, the first polymer miscible in the first solvent, and the second polymer miscible in the first solvent; and Also included is that, during a fourth time period after the third time period: heating the second substrate and the second series of separator material droplets to the target substrate temperature to evaporate the first solvent from the second series of separator material droplets and promote phase separation of the second polymer from the first polymer; washing the series of separator material droplets with a second solvent to dissolve the second polymer from the second series of separator material droplets and provide the open pore network having pores within the second series of separator material droplets; and The second series of separator material droplets and the second substrate are irradiated to crosslink the first polymer and form a second separator film on the second substrate having a separator thickness that approximates a target separator thickness.

13. The method of claim 1 , wherein irradiating the series of separator material droplets and the first substrate comprises irradiating the series of separator material droplets and the first substrate via an electron beam to crosslink the first polymer and form the separator membrane on the first substrate, the separator membrane comprising a permeable separator membrane having an open network of pores, the open network of pores being sized to transmit ions through the permeable separator membrane.

14. The method of claim 1, wherein dissolving the second polymer from the series of separator material droplets comprises: flushing the series of separator material droplets and the first substrate with the second solvent to provide an open pore network having pores; and A stream of air is projected onto the series of spacer material droplets and the first substrate to remove the second solvent from the series of spacer material droplets and the first substrate.

15. The method of claim 1, wherein spraying the series of separator material droplets on the first substrate comprises spraying the series of separator material droplets on the first substrate, each droplet in the series of separator material droplets comprising between 15% and 20% by weight of the first solvent comprising an organic ketone.

16. A method for depositing a separator material, comprising: During the first period: receiving a substrate within the encapsulation region; defining a target liquid temperature range for the separator material; at a nozzle facing the substrate and coupled to a reservoir of separator material in a liquid state, heating the nozzle toward the target liquid temperature range; detecting a first temperature of the baffle material at the nozzle; spraying a first volume of a separator material onto the substrate via the nozzle in response to the first temperature of the separator material falling within the target liquid temperature range, the separator material comprising a first solvent, a first polymer miscible in the first solvent, and a second polymer miscible in the first solvent; and reaching a target substrate temperature below the boiling point of the first solvent; and During a second time period following said first time period: heating the substrate and the first volume of the separator material to the target substrate temperature to evaporate the first solvent from the volume of separator material; dissolving the second polymer from the first volume of separator material to provide an open-pore network having pores; and The first volume of separator material is irradiated to crosslink the first polymer and form a separator film having a separator thickness that approximates a target separator thickness.

17. The method according to claim 16: Also included is, during the first time period: defining a target gas temperature range for the separator material, the target gas temperature corresponding to a target vapor pressure of the separator material in a gaseous state; heating the gaseous environment toward the target gas temperature range at a container containing a gaseous environment above a reservoir of separator material in a liquid state; and detecting a second temperature of the gaseous environment; and Wherein spraying the volume of separator material on the substrate includes spraying the first volume of separator material on the first substrate via the nozzle in response to the first temperature of the separator material falling within the target liquid temperature range and in response to the second temperature of the separator material falling within the target gas temperature range.

18. The method according to claim 16, further comprising: detecting a minimum volume of separator material in liquid form in the reservoir during the first time period; and During a third time period following the second time period: receiving a second substrate within the encapsulation region; heating the nozzle toward the target liquid temperature range; detecting a second temperature of the partition material at the nozzle; spraying a second volume of separator material on the second substrate via the nozzle in response to the second temperature of the separator material falling within the target liquid temperature range, the separator material comprising the first solvent, the first polymer, and the second polymer; calculating a total volume of separator material on the first substrate and the second substrate based on a combination of the first volume of separator material and the second volume of separator material; and In response to the total volume of the separator material exceeding the minimum volume of the separator material, the reservoir is refilled with a third volume of separator material in a liquid state that is greater than the minimum volume of the separator material.

19. A method for depositing a separator material, comprising: During the first period: receiving a portion of the substrate strip including the first substrate within the encapsulation region; and depositing a series of separator material droplets on the first substrate, each droplet in the series of separator material droplets comprising a first solvent, a first polymer, and a second polymer; as well as During a second time period following said first time period: heating the first substrate and the series of separator material droplets to a first temperature; washing the series of separator material droplets and the first substrate with a second solvent to dissolve the second polymer from the series of separator material droplets and provide an open pore network having pores within the series of separator material droplets; and The series of separator material droplets are irradiated to crosslink the first polymer and form a discrete separator layer on the first substrate, the discrete separator layer defining the open pore network having pores sized to transmit ions through the discrete separator layer.

20. The method of claim 19, wherein depositing the series of separator material droplets on the first substrate comprises spraying a series of monodisperse separator material droplets on the first substrate, each droplet in the series of separator material droplets being sized to prevent defects from forming in the discrete separator layer on the first substrate.

Citation Information

Patent Citations

  • Lithium ion battery composite isolation membranes

    CN102810655A

  • Preparation method of P(VDF-HFP) (Poly(Vinyl Fluoride-Hexafluoropropylene)) inorganic compound porous nano fiber lithium ion battery separator

    CN103258978A

  • Non-woven type power lithium battery diaphragm and preparation method thereof

    CN105070862A

  • Polymer composite membrane as well as preparation method and lithium ion battery with same

    CN107785519A

  • Separator and electrochemical device comprising same

    CN111373571A