Alkaline battery and method for manufacturing gasket for alkaline battery

By using polyamide resin with a weight average molecular weight higher than 40,000 and washer waste reuse technology, the problem of washer cracking during the riveting process of airtight NiMH secondary battery is solved, and the quality and yield of the battery are improved.

CN118947011APending Publication Date: 2024-11-12FDK CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030480.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-02-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The gasket of the sealed nickel-hydrogen secondary battery is prone to break during the riveting process, resulting in poor sealing, reducing battery quality and yield, especially when reusing resin, it is even more serious.

Method used

Polyamide resin with a weight average molecular weight of 40,000 or more is used as the washer material, and molding is performed by reusing washer waste material to control the compression ratio of the washer to improve toughness and prevent rivet fracture.

Benefits of technology

It effectively suppresses the gasket crack caused by rivet pressure, improves the seal reliability and quality of the battery, and improves the yield rate of battery production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118947011A_ABST
    Figure CN118947011A_ABST
Patent Text Reader

Abstract

A nickel-hydrogen secondary battery (2) according to the present invention is provided with: an outer can (10) having an opening at the upper end thereof; an electrode group (22) accommodated in the outer can (10) together with the alkaline electrolyte; and a sealing body (11) which is caulked and fixed at the opening portion of the outer can (10) with a gasket (12) interposed therebetween, the gasket (12) containing a polyamide resin having a weight-average molecular weight of 40,000 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an alkaline battery and a method for manufacturing a gasket for an alkaline battery, and more particularly to a sealed alkaline battery and a method for manufacturing a gasket for an alkaline battery. Background Art

[0002] As one type of alkaline battery, a sealed nickel-hydrogen secondary battery is known. In the sealed nickel-hydrogen secondary battery, an electrode group including a positive electrode and a negative electrode overlapped with a separator is contained in an outer can having an opening together with an alkaline electrolyte, and the opening of the outer can is hermetically sealed by a sealing body with a gasket (for example, refer to Patent Document 1).

[0003] The assembly operation steps of the sealed nickel-hydrogen secondary battery are as follows. First, the electrode group is contained in the outer can, and the alkaline electrolyte is injected into the outer can. On the other hand, in another process, a combination of annular gaskets is manufactured on the entire circumference of the periphery of the sealing body. Further, the combination is fitted into the opening of the outer can, and the peripheral wall of the outer can is appropriately bent and fixed by riveting. Thus, the above-mentioned combination is fixed to the opening of the outer can, thereby sealing the outer can. Here, the operation steps of riveting are described in detail. First, the specified position between the opening of the outer can and the upper part of the electrode group at the peripheral wall of the outer can is stamped toward the radial inner side of the outer can to bend and reduce the diameter. Thus, a neck is formed in the outer can. By forming the neck, a snap-fitting convex portion protruding into the inner side of the outer can is formed on the entire circumference of the peripheral wall of the outer can located on the upper side of the electrode group. Further, the above-mentioned combination is placed on the snap-fitting convex portion of the above-mentioned outer can. Then, in the outer can, the peripheral wall of the opening portion above the engaging protrusion is bent radially inward of the outer can, thereby the sealing body is fixed to the opening portion of the outer can by caulking through the gasket.

[0004] At this time, the peripheral edge of the sealing body is sandwiched between the engaging protrusion of the outer can and the folded peripheral wall of the opening of the outer can via the gasket, thereby hermetically sealing the outer can.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 5-226001 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] However, when the peripheral wall of the outer can is riveted and the peripheral edge of the sealing body is clamped through the gasket as described above, the gasket may crack and cause poor sealing. In particular, when the gasket contains recycled resin, the gasket may crack more easily. When poor sealing occurs in this way, the quality of the battery is reduced and the yield rate in battery production is reduced.

[0010] Therefore, in order to suppress a decrease in yield in battery production, a battery having high sealing reliability is desired.

[0011] The present invention has been accomplished based on the above situation, and its purpose is to provide a high-quality alkaline battery by suppressing the cracking of the gasket caused by caulking, and to provide a method for manufacturing a gasket for an alkaline battery.

[0012] Solutions to the problem

[0013] In order to achieve the above-mentioned object, according to the present invention, there is provided an alkaline battery, comprising: an outer can having an opening at an upper end; an electrode group contained in the outer can together with an alkaline electrolyte; and a sealing body fixed by riveting to the opening portion of the outer can via a gasket, wherein the gasket contains a polyamide resin having a weight-average molecular weight of 40,000 or more.

[0014] Furthermore, according to the present invention, there is provided a method for producing a gasket for an alkaline battery, the method comprising the step of recycling gasket waste containing a polyamide resin having a weight average molecular weight of 40,000 or more to mold a gasket.

[0015] Effects of the Invention

[0016] According to the present invention, it is possible to suppress the gasket from being broken by caulking, thereby providing a high-quality alkaline battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a perspective view showing a partially cutaway cylindrical nickel-hydrogen secondary battery.

[0018] Figure 2 is a cross-sectional view of the gasket.

[0019] Figure 3 It is a cross-sectional view showing a combination of a sealing body and a gasket.

[0020] Figure 4 It is a cross-sectional view schematically showing a compressed portion of the gasket.

[0021] Figure 5 This is a graph showing the relationship between the number of times a gasket is reused and the weight average molecular weight of the resin constituting the gasket.

[0022] Figure 6This is a graph showing the relationship between the weight average molecular weight of the resin constituting the gasket and the crack occurrence rate of the gasket. DETAILED DESCRIPTION

[0023] Hereinafter, a cylindrical nickel-hydrogen secondary battery (hereinafter also referred to as a “battery”) 2 of AAA size according to one embodiment will be described with reference to the drawings.

[0024] like Figure 1 As shown, the battery 2 includes an outer can 10 in a bottomed cylindrical shape with an open top. The outer can 10 is conductive, and its bottom wall 35 functions as a negative electrode terminal. The outer can 10 contains an electrode group 22 .

[0025] The electrode group 22 includes a strip-shaped positive electrode 24, a negative electrode 26 and a separator 28, which are wound into a spiral shape with the separator 28 sandwiched between the positive electrode 24 and the negative electrode 26. That is, the positive electrode 24 and the negative electrode 26 overlap each other with the separator 28 between them. Such an electrode group 22 is cylindrical as a whole. Here, the outermost periphery of the electrode group 22 is formed by a part (outermost periphery) of the negative electrode 26. That is, at the outermost periphery of the electrode group 22, there is no separator 28 and the negative electrode 26 is exposed. Therefore, the outermost negative electrode 26 of the electrode group 22 is in contact with the inner peripheral wall of the outer can 10, and the negative electrode 26 and the outer can 10 are electrically connected to each other.

[0026] In the electrode group 22, the edge of the positive electrode 24 protrudes in a spiral shape from one end surface, and the edge of the negative electrode 26 protrudes in a spiral shape from the other end surface. Here, the protruding edge of the positive electrode 24 is referred to as the positive electrode protruding edge 32, and the protruding edge of the negative electrode 26 is referred to as the negative electrode protruding edge 34. A positive electrode current collector 36 is welded to the positive electrode protruding edge 32, and thus the positive electrode current collector 36 is electrically connected to the positive electrode 24 over a wide range. On the other hand, a negative electrode current collector 38 is welded to the negative electrode protruding edge 34, and thus the negative electrode current collector 38 is electrically connected to the negative electrode 26 over a wide range.

[0027] Furthermore, a predetermined amount of alkaline electrolyte (not shown) is injected into the outer can 10. The alkaline electrolyte performs a charge-discharge reaction between the positive electrode 24 and the negative electrode 26. As the alkaline electrolyte, an alkaline electrolyte used in a general nickel-hydrogen secondary battery can be used. For example, a sodium hydroxide aqueous solution is preferably used.

[0028] A separator material commonly used in nickel-hydrogen secondary batteries can be used as the material of the separator 28. For example, a nonwoven fabric made of polyolefin fibers such as polyethylene and polypropylene is preferably used.

[0029] The positive electrode 24 includes: a conductive positive electrode substrate having a porous structure and a large number of pores; and a positive electrode mixture held in the pores and on the surface of the positive electrode substrate.

[0030] As such a positive electrode substrate, for example, foamed nickel can be used.

[0031] The positive electrode mixture includes: positive electrode active material particles, conductive material, positive electrode additive and binder. The binder plays the following role: while bonding the positive electrode active material particles, conductive material and positive electrode additive, the positive electrode mixture is bonded to the positive electrode substrate. Here, as the binder, for example, carboxymethyl cellulose can be used.

[0032] The positive electrode active material particles are nickel hydroxide particles or nickel hydroxide particles.

[0033] As the conductive material, for example, one or two or more selected from cobalt compounds such as cobalt oxide (CoO) and cobalt hydroxide (Co(OH) 2 ) and cobalt (Co) can be used.

[0034] In order to improve the characteristics of the positive electrode, a positive electrode additive appropriately selected as needed is added. Examples of the main positive electrode additive include yttrium oxide and zinc oxide.

[0035] Next, the negative electrode 26 will be described.

[0036] The negative electrode 26 includes a strip-shaped conductive negative electrode core and a negative electrode mixture held in the negative electrode core.

[0037] The negative electrode core is made of a sheet-like metal material with distributed through holes, for example, a punched metal sheet can be used. The negative electrode mixture is not only filled in the through holes of the negative electrode core, but also maintained in layers on both surfaces of the negative electrode core.

[0038] The negative electrode mixture includes: particles of hydrogen storage alloy, negative electrode additive, conductive material and adhesive. Here, the hydrogen storage alloy is an alloy that can absorb and release hydrogen as the negative electrode active material. There is no special limitation on the type of hydrogen storage alloy, but it is preferred to use a rare earth-Mg-Ni type hydrogen storage alloy containing rare earth elements, Mg and Ni. The above-mentioned adhesive plays the following role: while bonding the particles of the hydrogen storage alloy, the negative electrode additive and the conductive material to each other, the negative electrode mixture is bonded to the negative electrode core. Here, a hydrophilic or hydrophobic polymer can be used as a binder, and carbon black, graphite, nickel powder, etc. can be used as a conductive material.

[0039] In order to improve the characteristics of the negative electrode, a negative electrode additive appropriately selected according to needs is added.

[0040] The positive electrode 24 and the negative electrode 26 as described above are wound into a spiral shape with the separator 28 interposed therebetween, thereby forming the electrode group 22. In detail, during winding, the positive electrode 24 and the negative electrode 26 are arranged in a state slightly offset from each other in the following direction, which is the direction along the axial direction of the electrode group 22, and the separator 28 of a specified size is arranged at a specified position between these positive electrodes 24 and negative electrodes 26, and the winding operation is performed in this state. As a result, a cylindrical electrode group 22 is obtained. The morphology of the obtained electrode group 22 is as follows, one end side of the electrode group 22 is a state in which the positive electrode protruding end edge portion 32 of the positive electrode 24 protrudes relative to the negative electrode 26 adjacent to the separator 28, and the other end side of the electrode group 22 is a state in which the negative electrode protruding end edge portion 34 of the negative electrode 26 protrudes relative to the positive electrode 24 adjacent to the separator 28.

[0041] The positive electrode 24 , the negative electrode 26 , and the separator 28 of the electrode group 22 are formed by winding a winding core having a predetermined outer diameter. The winding core is pulled out after the winding operation, so a central through hole 40 is formed in the center of the electrode group 22 to penetrate the center.

[0042] In the electrode group 22 , a positive electrode current collector 36 is welded to a positive electrode protruding edge portion 32 located at one end of the cylindrical shape of the electrode group 22 .

[0043] The positive electrode current collector 36 includes, for example, a main body 42 that is circular in plan view and is made of a metal thin plate, and a lead portion 44 that extends from a portion of the periphery of the main body 42 .

[0044] The main body 42 of the prepared positive electrode current collector 36 is welded to the positive electrode protruding edge portion 32 at one end of the electrode group 22. Here, the material of the positive electrode current collector 36 is not particularly limited, but a nickel-plated steel plate obtained by plating nickel with a thickness of 2 μm on a thin steel plate equivalent to so-called SPCC (cold-rolled steel plate) can be exemplified as a preferred material.

[0045] In addition, in the electrode group 22 , a negative electrode current collector 38 is welded to a negative electrode protruding edge portion 34 located at the other end of the cylindrical shape of the electrode group 22 .

[0046] For example, a metal thin plate having a circular shape in plan view is used as the negative electrode current collector 38. Here, the material of the negative electrode current collector 38 is not particularly limited, but a nickel-plated steel plate obtained by plating nickel with a thickness of 2 μm on a thin steel plate equivalent to so-called SPCC (cold-rolled steel plate) can be exemplified as a preferred material.

[0047] The electrode group 22 to which the positive electrode collector 36 and the negative electrode collector 38 are welded is housed in the outer can 10. Here, the negative electrode collector 38 is welded to the bottom wall 35 of the outer can 10, which serves as a negative electrode terminal. Therefore, the negative electrode 26 is in contact with the outer can 10 not only at the outermost periphery of the electrode group 22, but also in contact with the bottom wall 35 of the outer can 10 via the negative electrode collector 38. Therefore, the negative electrode 26 is in contact with the outer can 10 over a wide range, and the current collection efficiency is further improved.

[0048] An alkaline electrolyte is injected into the outer can 10 containing the electrode group 22. A sealing body 11 is fixed to the opening of the outer can 10 containing the electrode group 22 together with the alkaline electrolyte via an insulating gasket 12. The sealing body 11 includes a cover plate 14, a valve body 18, and a cap member 20. The cap member 20 also serves as a positive electrode terminal.

[0049] The cover plate 14 is a conductive disc-shaped member having an inner surface 14a located inside the battery 2 and an outer surface 14b located outside the battery 2 on the opposite side to the inner surface 14a (see FIG. Figure 3 ). In addition, the cover plate 14 also includes a through hole serving as a vent. In the present embodiment, a central through hole 16 serving as the above-mentioned vent is opened in the center of the cover plate 14. In addition, a rubber valve body 18 is arranged on the outer surface 14b of the cover plate 14 to block the central through hole 16. Furthermore, a metal cap member 20 (positive terminal) in a cylindrical shape with a flange is electrically connected to the outer surface 14b of the cover plate 14 in a manner covering the valve body 18. The cap member 20 presses the valve body 18 toward the cover plate 14. It should be noted that a vent hole 21 (refer to Figure 3 ).

[0050] Normally, the central through hole 16 is hermetically closed by the valve body 18. On the other hand, if gas is generated in the outer can 10 and the internal pressure thereof increases, the valve body 18 is compressed by the internal pressure to open the central through hole 16, and as a result, the gas is discharged from the inner part of the outer can 10 to the outside through the central through hole 16 and the exhaust hole 21 of the positive terminal 20. That is, the central through hole 16, the valve body 18, and the cap member 20 (positive terminal) form a safety valve for the battery 2.

[0051] Here, the lead portion 44 of the positive electrode current collector 36 is connected to the inner surface 14a of the cover plate 14. That is, the positive electrode 24 is electrically connected to the cover plate 14. Thus, the positive electrode 24 and the cap member 20 (positive electrode terminal) are electrically connected to each other via the positive electrode current collector 36 and the cover plate 14.

[0052] The opening of the outer can 10 is sealed by the sealing body 11 and the gasket 12. Specifically, the opening 15 of the outer can 10 is sealed by caulking and fixing the assembly 46 of the sealing body 11 and the gasket 12 to a predetermined position of the peripheral wall 13 of the outer can 10.

[0053] The gasket 12 contains a polyamide resin, preferably polyamide 66 (hereinafter also referred to as "PA66"). PA66 has the advantages of excellent alkali resistance and low cost. The gasket 12 preferably contains a polyamide resin as a main component.

[0054] At least a portion of the polyamide resin is preferably a recycled resin of gasket waste. Gasket waste refers to a molded product (gasket 12) obtained in the process of molding the gasket 12 or unnecessary parts such as runners discharged in the process, used gaskets 12, etc. The recycled resin refers to a resin obtained by crushing these gasket wastes, recovering them, and reusing them.

[0055] The shape of the gasket 12 is, for example, annular as a whole. Figure 2 As shown, it includes: a disc-shaped base end wall 50; and a side peripheral wall 52 extending upright from the outer peripheral portion of the base end wall 50.

[0056] The base end wall 50 is a portion that contacts the inner surface 14a of the cover plate 14 of the sealing body 11, and has a cover plate receiving surface 54 located on the sealing body 11 side and a lower surface 56 located on the opposite side of the cover plate receiving surface 54 and on the electrode group 22 side. A stepped step 58 is provided on the cover plate receiving surface 54 in a manner consistent with the shape of the cover plate 14. An engaging portion 60 is provided on the lower surface 56 to engage with the peripheral wall 13 of the curved outer can 10 during caulking.

[0057] The side peripheral wall 52 includes an outer peripheral edge contact portion 62 that contacts the outer peripheral edge of the cover plate 14 , and a restriction portion 64 that is covered on the outer surface 14 b of the cover plate 14 and restricts the cover plate 14 during caulking.

[0058] like Figure 3 As shown, the sealing body 11 is fitted between the side peripheral walls 52 of the gasket 12. In this way, a combination 46 of the sealing body 11 and the gasket 12 is formed.

[0059] Here, the compression rate of the gasket 12 during riveting is preferably set to 10% or more. If the compression rate of the gasket 12 is 10% or more, the air tightness and liquid tightness of the outer can 10 are fully maintained. The compression rate of the gasket 12 is more preferably 30% or more. In the present embodiment, it is confirmed that the air tightness and liquid tightness of the outer can 10 are fully maintained until the compression rate of the gasket 12 reaches 60%.

[0060] Below, reference Figure 4The compression rate of the gasket 12 in this embodiment will be described.

[0061] Figure 4 , the right side of the caulking portion is schematically enlarged and shown relative to the cross-sectional shape of the outer can 10. It should be noted that in this figure, the cap member 20 is omitted.

[0062] If the Figure 4 As shown, the length between P1 and P2 before and after compression changes in percentage, where P1 is the portion in contact with the engaging protrusion 17 of the outer can 10 at the lower surface 56 of the base end wall 50 of the gasket 12, and P2 is the portion in contact with the inner surface 14a of the cover plate 14 at the cover plate receiving surface 54 of the base end wall 50 of the gasket 12. Specifically, when the length between P1 and P2 after compression is defined as A and the length between P1 and P2 before compression is defined as B, the compression rate T is obtained by the following formula (I).

[0063] T[%]=(BA) / B × 100…(I)

[0064] It should be noted that after riveting, the outer diameter of the battery is sometimes drawn (outer diameter drawing). Even in this case, the compression rate will hardly change depending on whether the outer diameter drawing is performed, or even if it changes, the compression rate is further improved by the outer diameter drawing.

[0065] However, the gasket 12 may be broken during caulking, and when the gasket 12 is broken, it may cause a poor sealing of the outer can 10. Such a break may occur even when caulking is performed at a normal compression rate of about 30%.

[0066] Therefore, the inventors of the present application conducted an in-depth study on the cause of the breakage of the gasket 12. In the course of the study, it was found that there is a correlation between the weight average molecular weight of the polyamide resin contained in the gasket 12 and the occurrence rate of the breakage of the gasket 12. Specifically, the following knowledge was obtained: when the weight average molecular weight of the polyamide resin is less than 40,000, the breakage occurs in the gasket 12.

[0067] In particular, it was found that when the gasket 12 is obtained by recycling gasket waste, the weight average molecular weight of the polyamide resin decreases as the number of times of recycling increases. Further, the following insight was obtained: when the weight average molecular weight of the recycled polyamide resin is less than 40,000, the gasket is prone to cracking during riveting.

[0068] Based on these findings, in the present embodiment, the weight average molecular weight of the polyamide resin is set to be greater than or equal to 40,000. Although the mechanism by which the cracking of the gasket 12 is suppressed by setting the weight average molecular weight of the polyamide resin to be greater than or equal to 40,000 is not clear, it is presumed that this is because the toughness of the gasket 12 is improved. The upper limit of the weight average molecular weight of the polyamide resin is not particularly limited as long as it is within a range that does not impair the moldability, and can be set to 60,000, for example.

[0069] Here, the weight average molecular weight of the polyamide resin can be measured by GPC (Gel Permeation Chromatography) method. Specifically, it can be measured by the following operation procedure.

[0070] 1) A portion of the gasket 12 is dissolved in an eluent to prepare a sample solution, and the obtained sample solution is filtered with a membrane filter (pore size 0.2 μm) as a pretreatment for analysis. The filtered sample solution is passed through a chromatographic column of a GPC measuring device, and the molecular size in the sample solution flowing out of the chromatographic column is detected with a detector to obtain a chromatogram of the molecular size in the sample solution. The measurement conditions of the GPC method can be set as follows.

[0071] (Measurement conditions)

[0072] GPC measuring apparatus: GPC-104 manufactured by Shoko Scientific Co., Ltd. (using RI detector)

[0073] Chromatographic column: Two Shodex GPC LF-404 columns manufactured by Showa Denko K.K. connected together

[0074] Eluent: a solution of 10 mmol / L sodium trifluoroacetate (CF3COONa) added to hexafluoroisopropanol (HFIP)

[0075] Sample concentration: 0.2w / v%

[0076] Injection volume: 10 μL

[0077] Flow rate of sample liquid in the chromatographic column: 0.3mL / min

[0078] Column temperature: 40°C

[0079] 2) On the other hand, the same measurement was performed in advance using a standard substance (polymethyl methacrylate (PMMA)) with a known molecular weight, and a calibration curve (logarithm of detection time versus molecular weight) was prepared.

[0080] 3) Further, the molecular weight at a certain detection time is determined from the chromatogram of the sample obtained in 1) using the calibration curve obtained in 2). Thus, the weight average molecular weight of the polyamide resin contained in the gasket 12 is measured.

[0081] As an operation procedure for manufacturing the gasket 12, first, prepare resin particles that are finely crushed into granular particles from the raw material of the polyamide resin. At this time, a polyamide resin with a weight average molecular weight of more than 40,000 is prepared. Alternatively, a polyamide resin with a weight average molecular weight of more than 55,000 can also be prepared. The prepared resin particles are sent to the inside of the barrel through the hopper of the injection molding machine. Since the barrel is heated by the heater, the resin particles are melted in the barrel. The molten resin is mixed by the screw rotating in the barrel. Then, the screw is pushed out to the mold side, whereby the molten resin is injected into the mold. Further, the resin is maintained in the mold until it is cooled and solidified. Then, the mold is opened and the molded product is discharged. At this time, the discharged molded product is in a state where multiple gaskets are connected by a runner, so the gasket 12 is obtained by cutting from the runner.

[0082] When manufacturing the gasket 12 in this manner, if a polyamide resin having a weight average molecular weight of 40,000 or more is prepared as the polyamide resin to be prepared, the gasket 12 capable of suppressing the occurrence of cracks can be obtained.

[0083] However, from the viewpoint of effective utilization of resources, it is not preferred to directly discard the runner remaining after removing the gasket 12, which also leads to an increase in the environmental load. Therefore, the remaining runner is crushed again to make resin particles as the raw material of the gasket 12. Usually, such reuse is carried out. However, as the number of such reuses increases, the weight-average molecular weight of the polyamide resin decreases, and when the weight-average molecular weight is lower than 40,000, cracks are likely to occur in the obtained gasket. Therefore, before the weight-average molecular weight is lower than 40,000, a gasket 12 that is not easy to crack even if it is reused can be obtained, so the weight-average molecular weight of the polyamide resin can also be used as a standard for the number of reuses.

[0084] That is, the method for producing a gasket for an alkaline battery according to one embodiment preferably includes a step of molding the gasket 12 by recycling gasket scraps containing a polyamide resin having a weight average molecular weight of 40,000 or more.

[0085] There is no particular limitation on the method for recycling the gasket waste containing the polyamide resin having a weight average molecular weight of 40,000 or more. For example, the weight average molecular weight of the polyamide resin in the gasket waste discharged in the step of forming the gasket 12 may be measured, and if the weight average molecular weight is 40,000 or more, the gasket waste may be recovered and reused in the above-mentioned gasket forming step. Alternatively, information indicating the relationship between the weight average molecular weight of the polyamide resin contained in the gasket waste and the number of reuses may be obtained in advance (for example, as described later). Figure 5According to the information, in the above-mentioned gasket forming process, the gasket waste containing the polyamide resin with a weight average molecular weight of 40000 or more is used. For example, according to the above-mentioned information, the gasket waste can be repeatedly reused within the range of the weight average molecular weight of the polyamide resin not less than 40000.

[0086] As described above, according to this embodiment, by controlling the weight average molecular weight of the polyamide resin to be above 40000, the gasket rupture caused by riveting can be suppressed. Therefore, according to this embodiment, a high-quality battery with high sealing reliability can be obtained, and the yield rate in battery production can be improved.

[0087] Example

[0088] 1. Battery manufacturing

[0089] (Example 1)

[0090] (1) Manufacturing of gaskets

[0091] As the polyamide resin, pellets of polyamide 66 having a weight average molecular weight of about 50,000 are prepared. The prepared pellets of polyamide 66 are loaded into the hopper of the injection molding machine and sent from the hopper to the inside of the barrel. The barrel is heated to 300°C by a heater, and the pellets of polyamide 66 are melted in the barrel. The molten polyamide 66 is kneaded by the screw rotating in the barrel. Then, the screw is pushed out to the mold side, whereby the molten resin is injected into the mold. Further, the resin is retained in the mold until it is cooled and solidified. Then, the mold is opened and the molded product is discharged. The discharged molded product is a state in which a plurality of gaskets are connected by a runner, so the gasket 12 is obtained by cutting it from the runner. The obtained gasket 12 is Figure 2 The circular shape shown.

[0092] Next, the obtained gasket 12 is placed in silica gel to be dried and stored in an absolutely dry state.

[0093] Here, a sample for determining the weight average molecular weight is extracted from a part of the obtained multiple gaskets 12, and the weight average molecular weight is determined by the GPC method. In detail, the sample is dissolved in an eluent to prepare a sample solution, and the obtained sample solution is filtered with a membrane filter (pore size 0.2μm) as an analysis pretreatment. The filtered sample solution is passed through the chromatographic column of the GPC analysis device, and the molecular size in the sample solution flowing out of the chromatographic column is detected by a detector to obtain a chromatogram of the molecular size in the sample solution. On the other hand, the same measurement is performed in advance using a standard substance with a known molecular weight to prepare a calibration curve (logarithm of the detection time to the molecular weight). Furthermore, using this calibration curve, the molecular weight at a certain detection time is determined by the chromatogram of the sample. In this way, the weight average molecular weight of the gasket 12 is measured.

[0094] The analysis conditions of the above-mentioned GPC method are as follows. The eluent is a solution of sodium trifluoroacetate (CF3COONa) added to hexafluoroisopropanol (HFIP) at 10 mmol / L, the standard substance is polymethyl methacrylate (PMMA), the sample concentration is 0.2 w / v%, the injection volume is 10 μL, the flow rate of the sample solution in the chromatographic column is 0.3 mL / min, the chromatographic column temperature is 40°C, the GPC analysis device is GPC-104 manufactured by Showa Science Co., Ltd. (using RI detector), and the chromatographic column is a chromatographic column formed by connecting two Shodex GPC LF-404 manufactured by Showa Denko K.K.

[0095] Here, the weight average molecular weight of the polyamide 66 constituting the gasket 12 of Example 1 is 52,000.

[0096] (2) Assembly of AAA-size cylindrical nickel-metal hydride secondary batteries

[0097] First, if Figure 3 As shown, the valve body 18 is accommodated in the interior of the cap member 20, and the cap member 20 is welded to the outer surface 14b of the cover plate 14. At this time, the valve body 18 is arranged at a position to block the central through hole 16 of the cover plate 14. In this way, the sealing body 11 is completed.

[0098] Then, if Figure 3 The obtained sealing body 11 and the gasket 12 obtained as described above are combined as shown to form a combination 46 of the sealing body 11 and the gasket 12 .

[0099] Next, the positive electrode 24 and the negative electrode 26 used for a general AAA size nickel-hydrogen secondary battery are wound into a spiral shape with a separator 28 made of a nonwoven fabric made of polypropylene fibers sandwiched therebetween to produce an electrode group 22. The positive electrode collector 36 and the negative electrode collector 38 are welded at predetermined positions of the electrode group 22.

[0100] The obtained electrode group 22 is housed in an outer can 10 with a bottomed cylindrical shape for AAA size. At this time, the negative electrode collector 38 and the bottom wall 35 of the outer can 10 are welded. Furthermore, the lead portion 44 of the positive electrode collector 36 and the inner surface 14a of the cover plate 14 are welded. Then, an alkaline electrolyte composed of an aqueous sodium hydroxide solution is injected into the outer can 10. Next, the above-mentioned assembly 46 is fitted into the opening portion of the outer can 10, and the peripheral wall of the outer can 10 is appropriately bent and fixed by riveting. Here, the compression rate of the gasket 12 during riveting is 60%.

[0101] Next, the battery 2 whose sealing body 11 has been riveted and fixed is subjected to outer diameter drawing. It is confirmed that the compression rate remains unchanged even after the outer diameter drawing. Thus, a battery 2 of AAA size is manufactured. It is noted that 20 batteries 2 are manufactured by the same operation steps as the above operation steps.

[0102] (Example 2)

[0103] A battery was manufactured in the same manner as in Example 1 except that pellets obtained by collecting and crushing the runners remaining when manufacturing the gasket 12 of Example 1 were used as pellets of polyamide 66.

[0104] Here, the weight average molecular weight of the polyamide 66 constituting the gasket of Example 2 is 49000. The number of times of reuse of the gasket 12 of Example 2 is counted as one.

[0105] (Example 3)

[0106] A battery was manufactured in the same manner as in Example 1 except that pellets obtained by collecting and crushing the runners remaining when manufacturing the gasket 12 of Example 2 were used as pellets of polyamide 66.

[0107] Here, the weight average molecular weight of the polyamide 66 constituting the gasket 12 of Example 3 is 45000. The number of times the gasket 12 of Example 3 was reused was counted as 2 times.

[0108] (Example 4)

[0109] A battery was manufactured in the same manner as in Example 1 except that pellets obtained by collecting and crushing the runners remaining when manufacturing the gasket 12 of Example 3 were used as pellets of polyamide 66.

[0110] Here, the weight average molecular weight of the polyamide 66 constituting the gasket 12 of Example 4 is 43000. The number of times the gasket 12 of Example 4 was reused was counted as three times.

[0111] (Example 5)

[0112] A battery was manufactured in the same manner as in Example 1 except that pellets obtained by collecting and crushing the runners remaining when manufacturing the gasket 12 of Example 4 were used as pellets of polyamide 66.

[0113] Here, the weight average molecular weight of the polyamide 66 constituting the gasket 12 of Example 5 is 40000. The number of times the gasket 12 of Example 5 was reused was counted as 4 times.

[0114] (Comparative Example 1)

[0115] A battery was manufactured in the same manner as in Example 1 except that pellets obtained by collecting and crushing the runners remaining when manufacturing the gasket 12 of Example 5 were used as pellets of polyamide 66.

[0116] Here, the weight average molecular weight of the polyamide 66 constituting the gasket 12 of Comparative Example 1 is 39000. The number of times the gasket 12 of Comparative Example 1 was reused was counted as 5 times.

[0117] (Comparative Example 2)

[0118] A battery was manufactured in the same manner as in Example 1 except that pellets obtained by collecting and crushing the runners remaining when manufacturing the gasket 12 of Comparative Example 1 were used as pellets of polyamide 66.

[0119] Here, the weight average molecular weight of the polyamide 66 constituting the gasket 12 of Comparative Example 2 is 35000. The number of times the gasket 12 of Comparative Example 2 was reused was counted as 6 times.

[0120] (Comparative Example 3)

[0121] A battery was manufactured in the same manner as in Example 1 except that pellets obtained by collecting and crushing the runners remaining when manufacturing the gasket 12 of Comparative Example 2 were used as pellets of polyamide 66.

[0122] Here, the weight average molecular weight of the polyamide 66 constituting the gasket 12 of Comparative Example 3 is 31000. The number of times of reuse of the gasket 12 of Comparative Example 3 is counted as 7 times.

[0123] 2. Evaluation

[0124] (1) Relationship between the number of reuses and weight average molecular weight

[0125] Regarding the washers of Examples 1 to 5 and Comparative Examples 1 to 3, the relationship between the number of reuses and the weight average molecular weight is as follows: Figure 5 as shown in the chart.

[0126] Depend on Figure 5 As can be seen from the graph, the weight average molecular weight of polyamide 66 constituting the gasket decreases as the number of reuses increases.

[0127] (2) Check whether the gasket is broken

[0128] The state of the gasket portion of the batteries of Examples 1 to 5 and Comparative Examples 1 to 3 was observed, and the number of batteries with cracks was counted. Furthermore, the percentage of the number of batteries with cracks in the gasket among the total number of batteries (20) was calculated, and the percentage was taken as the occurrence rate of gasket cracks. Based on the obtained results, the relationship between the weight average molecular weight of polyamide 66 and the occurrence rate of gasket cracks is as follows: Figure 6 as shown in the chart.

[0129] (3) Investigation

[0130] The relationship between the weight average molecular weight of polyamide 66 and the cracking rate of the gasket is shown in Figure 2. Figure 6 It can be seen that when the weight average molecular weight of polyamide 66 is between 52,000 and 40,000, the gasket rupture caused by riveting does not occur, and the high sealing quality is maintained. On the other hand, when the weight average molecular weight of polyamide 66 is lower than 40,000, the gasket rupture begins to occur. It can be seen that if the weight average molecular weight of polyamide 66 is set to 40,000 or more, the occurrence of gasket rupture is suppressed even if riveting is performed. Therefore, it can be said that controlling the weight average molecular weight of polyamide 66 to 40,000 or more is important for the stable production of high-quality batteries.

[0131] As described above, according to the present invention, by controlling the weight average molecular weight of the polyamide resin contained in the gasket to 40,000 or more, it is possible to suppress the gasket from being broken by caulking, thereby providing a high-quality alkaline battery.

[0132] In addition, the relationship between the number of reuses and the weight average molecular weight is shown by Figure 5 It can be seen that when the number of reuses exceeds 4 times, the weight average molecular weight of polyamide 66 is less than 40000. When the weight average molecular weight of polyamide 66 is less than 40000, the quality of the battery is deteriorated, so it can be understood that it is preferable to set the number of reuses to 4 times or less in order to maintain the quality of the battery at a certain level or above. That is, it is easy to grasp the criterion for achieving a balance between the number of reuse operations for suppressing environmental load and maintaining the quality of the battery at a certain level or above.

[0133] It should be noted that the present invention is not limited to the above-mentioned one embodiment and example, and various modifications can be made. For example, the type of battery is not limited to nickel-hydrogen secondary batteries, but can also be other alkaline secondary batteries such as nickel-cadmium secondary batteries. In addition, it is not limited to alkaline secondary batteries, but can also be alkaline primary batteries. Furthermore, the shape of the battery is not limited to cylindrical, but can also be a square battery.

[0134] This application claims the priority based on Japanese Patent Application No. 2022-051905 filed on March 28, 2022. The contents described in the specification and drawings of that application are incorporated herein by reference in their entirety.

[0135] Industrial Applicability

[0136] According to the present invention, cracking of the gasket caused by caulking can be suppressed, thereby providing a high-quality alkaline battery. In addition, a method for producing a gasket for an alkaline battery can be provided.

[0137] Description of Reference Numerals

[0138] 2Nickel-metal hydride secondary battery

[0139] 10 external cans

[0140] 11 Sealing body

[0141] 12 washers

[0142] 14 Cover

[0143] 18 Valve body

[0144] 20 Cap member (positive terminal)

[0145] 24 positive electrode

[0146] 26 negative electrode

[0147] 28 Diaphragm

[0148] 50 base end wall

[0149] 52 side wall

Claims

1. An alkaline battery comprising: an outer can having an opening at an upper end; an electrode group contained in the outer can together with an alkaline electrolyte; and A sealing body is fixed to the opening of the outer can by riveting through a gasket, in, The gasket includes a polyamide resin having a weight average molecular weight of 40,000 or more.

2. The alkaline battery according to claim 1, wherein The sealing body includes a cover plate, which is a circular plate-shaped cover plate that seals the opening of the outer can, and has an inner surface located inside the outer can and an outer surface located outside the outer can. The gasket is in the shape of a ring that fits in with the outer peripheral edge of the cover plate, and includes a base end wall and a side peripheral wall, wherein the base end wall is in contact with the inner surface of the cover plate, and the side peripheral wall extends upright from the outer peripheral portion of the base end wall and is bent at the outer peripheral edge portion of the cover plate to be in contact with the outer surface of the cover plate. A portion of the side wall of the outer can between the opening and the electrode group is bent, and the cover plate is sandwiched by the bent portion via the base end wall of the gasket and the side peripheral wall.

3. The alkaline battery according to claim 2, wherein: The cover plate further comprises a through hole, The sealing body further includes a valve body, and the valve body is arranged on the outer surface of the cover plate in a manner of sealing the through hole.

4. The alkaline battery according to claim 3, wherein The gasket has a compression rate of 30% or more at the base end wall in a direction along a thickness direction of the cover plate.

5. The alkaline battery according to any one of claims 1 to 4, wherein The polyamide resin is polyamide 66.

6. The alkaline battery according to any one of claims 1 to 4, wherein At least a portion of the polyamide resin is recycled resin from gasket waste.

7. A method for manufacturing a gasket for an alkaline battery, the method comprising: A step of recycling gasket waste containing a polyamide resin having a weight average molecular weight of 40,000 or more to form a gasket.

8. The method for producing a gasket for an alkaline battery according to claim 7, wherein: acquiring in advance information indicating the relationship between the weight average molecular weight of the polyamide resin contained in the gasket waste and the number of times of reuse, In the gasket molding step, the gasket scrap having a weight average molecular weight of the polyamide resin of 40,000 or more is used based on the information.