Modified perovskite manganese oxide for NH3 catalytic oxidation and preparation method and application thereof

Through the preparation of modified perovskite manganese oxide, the problems of insufficient activity and high cost of perovskite catalysts are solved, and the efficient catalytic oxidation of NH3 is achieved, with good low-temperature activity and N2 selectivity are good, and suitable for waste gas treatment.

CN118949972AInactive Publication Date: 2024-11-15SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
CN202410891371.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art has problems in the catalytic oxidation of NH3, such as insufficient catalyst activity, high cost, low purification efficiency and possible secondary pollution in terms of NH3 catalytic oxidation. In particular, the specific surface area of ​​perovskite catalysts is low, which limits its application.

Method used

By preparing modified perovskite manganese oxide, MnCO3 and CaCO3 are used to react in HNO3 solution, pH value is adjusted, acid-induced surface disparity is carried out, calcium-manganese ratio and reaction conditions are optimized, and high catalytic activity and good hydrothermal stability are formed. catalyst.

Benefits of technology

It achieves high conversion rate and high N2 selectivity of NH3 under low temperature conditions, is low cost, has high stability and repeatability, and is suitable for selective catalytic ammonia oxidation and waste gas treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949972A_ABST
    Figure CN118949972A_ABST
Patent Text Reader

Abstract

The invention discloses a modified perovskite manganese oxide for NH3 catalytic oxidation and a preparation method and application thereof. The preparation method of the modified perovskite manganese oxide for NH3 catalytic oxidation is simple and controllable, low in cost and high in stability and repeatability. Experiments prove that when the calcium-manganese ratio is 1: 3 and the acid-induced surface disproportionation time is 24 hours, the perovskite manganese oxide has the best performance in the NH3-SCO catalytic reaction, the catalyst has good low-temperature activity in the NH3-SCO reaction, the conversion rate of NH3 at 180 DEG C is about 100%, and the N2 selectivity is relatively high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a catalyst for NH 3 Modified perovskite manganese oxide for catalytic oxidation and preparation method and application thereof. Background Art

[0002] NH 3 It is a colorless gas at room temperature and pressure with a strong pungent odor. 3 It not only harms human health, but also causes various atmospheric environmental problems such as haze and photochemical smog. Ammonia comes from a wide range of sources, mainly agricultural production (animal husbandry, fertilizers), industrial waste gas, biomass combustion and motor vehicle exhaust.

[0003] Currently controlling NH 3 There are many methods for emission, including absorption, adsorption, biological, plasma activation, etc. However, these methods have problems such as harsh purification conditions, low purification efficiency, and even secondary pollution, which are difficult to meet the actual purification needs. 3 -SCO) is a promising method for removing gaseous ammonia. 3 -SCO catalyst can release NH 3 It can selectively catalyze the oxidation of NH 3 Converted to harmless N 2 and H 2 O, and the core of this technology is to find 2 Selective and hydrothermally stable NH 3 -SCO catalyst.

[0004] Perovskite (ABO 3 ) composite oxides are widely used due to their low cost, high hydrothermal stability, and adjustable composition elements. In existing studies, La-Mn and La-Co perovskites are commonly used in the field of thermal catalysis, but they require the addition of expensive lanthanide metal elements and have high preparation costs. Ca-Mn composite materials have the characteristics of abundant resources, low cost, and environmental friendliness, and have more practical application value. At present, Ca-Mn composite perovskite catalysts are mainly used in the field of electrochemistry. 3 There is no systematic research on catalytic oxidation. The low specific surface area of ​​perovskite limits its NH 3 In applications of catalytic oxidation, the A-site elements in inactive sites often occupy the surface of perovskite, and modification methods are needed to improve the catalytic activity of perovskite. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and provide a method for 3 Modified perovskite manganese oxides for catalytic oxidation.

[0006] Another object of the present invention is to provide a method for preparing the modified perovskite manganese oxide.

[0007] Another object of the present invention is to provide applications of the modified perovskite manganese oxide.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] One for NH 3 The modified perovskite manganese oxide for catalytic oxidation is prepared by the following steps:

[0010] (1) MnCO 3 and CaCO 3 Add HNO 3 The solution was stirred until completely dissolved, and (NH 4 ) 2 CO 3 solution, stirring, standing, suction filtering, drying, and calcining to obtain calcium manganese oxide;

[0011] (2) Take the calcium manganese oxide prepared in step (1), add HNO 3 solution, stirred for reaction, filtered, adjusted pH, dried, and obtained NH 3 Modified perovskite manganese oxides for catalytic oxidation.

[0012] The MnCO in step (1) 3 and CaCO 3 The amount ratio of the substance is 1-2:1-3; preferably 1:3.

[0013] HNO described in step (1) 3 The concentration of the solution is 1-2 mol·L -1 .

[0014] Step (1) (NH 4 ) 2 CO 3 The concentration of the solution is 1-2 mol·L -1 .

[0015] The MnCO in step (1) 3 and CaCO 3 The total amount of substance and NH 4 HCO 3 The molar ratio of substances is 1:1~5.

[0016] The stirring time in step (1) is 30 to 60 minutes, preferably 40 minutes.

[0017] The standing time in step (1) is 5 to 20 minutes, preferably 10 minutes.

[0018] The drying condition in step (1) is drying at 80°C.

[0019] The calcination conditions in step (1) are to increase the temperature to 800-1000° C. at a heating rate of 5-10° C. / min and calcine for 5-8 hours; preferably, to increase the temperature to 850° C. at a heating rate of 6° C. / min and calcine for 7 hours.

[0020] HNO described in step (2) 3 The concentration of the solution is 1 to 5 mol·L -1 .

[0021] The stirring reaction time in step (2) is 1 to 72 hours, preferably 24 hours.

[0022] The pH adjustment in step (2) is to adjust the pH to 6-8.

[0023] The drying condition in step (2) is 80° C. for 24 hours.

[0024] The above is used for NH 3 Modified perovskite manganese oxides for catalytic oxidation of NH 3 -SCO reaction application.

[0025] The NH 3 The conditions for the -SCO reaction are 120 to 300°C, preferably 120 to 180°C.

[0026] The above is used for NH 3 Application of catalytically oxidized modified perovskite manganese oxide in the preparation of catalysts for selective catalytic oxidation of ammonia.

[0027] The above is used for NH 3 Application of modified perovskite manganese oxide for catalytic oxidation in the preparation of farm odor catalysts.

[0028] The farm odor contains NH 3 of exhaust gas.

[0029] The above is used for NH 3 Application of catalytically oxidized modified perovskite manganese oxide in the preparation of catalysts for waste gas treatment in the hairdressing industry.

[0030] Compared with the prior art, the present invention has the following advantages and effects:

[0031] The present invention prepares the NH 3 The preparation method of modified perovskite manganese oxide by catalytic oxidation is simple, controllable, low-cost, and highly stable and reproducible. Experimental verification shows that when the calcium-manganese ratio is 1:3 and the acid-induced surface disproportionation time is 24h, the perovskite manganese oxide is 3 -SCO has the best performance in the catalytic reaction. 3 -SCO reaction has good low temperature activity, NH 3 At 180℃, the conversion rate is about 100%, N 2 High selectivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Different lengths of acid induce surface disproportionation of CaMn 3 O 6 NH of perovskite manganese oxide 3 Conversion rate.

[0033] Figure 2 Different lengths of acid induce surface disproportionation of CaMn 3 O 6 N in perovskite manganese oxide 2 Selective.

[0034] Figure 3 The NH of catalysts with different calcium-manganese ratios before and after acid-induced surface disproportionation 3 Conversion rate.

[0035] Figure 4 is the N of catalysts with different calcium-manganese ratios before and after acid-induced surface disproportionation 2 Selective.

[0036] Figure 5 It is the XPS spectra of catalysts with different calcium-manganese ratios. DETAILED DESCRIPTION

[0037] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.

[0038] If the specific experimental conditions are not specified in the following embodiments, the conventional experimental conditions or the experimental conditions recommended by the reagent company are usually followed. The materials and reagents used, unless otherwise specified, are all reagents and materials obtained from commercial sources.

[0039] Example 1 Preparation of perovskite manganese oxide

[0040] (1) MnCO 3 Preparation:

[0041] At room temperature, 0.1 mol Mn(NO 3 )2 ·4H 2 O (concentration 0.4 mol L -1 ) was dissolved in 250 mL of deionized water; at the same time, 500 mL of NH 4 HCO 3 Solution (concentration 1 mol L -1 NH 4 HCO 3 The solution was slowly added with Mn(NO 3 ) 2 ·4H 2 O solution and placed on a magnetic stirrer for 30 minutes (stirring while pouring the solution). Bubbles will be generated at the beginning. Finally, the precipitate is separated from the solution by suction filtration and repeatedly rinsed with deionized water until the ammonia smell is completely removed. Finally, vacuum drying is carried out at 60°C for 10 hours.

[0042] (2) CaCO 3 Preparation

[0043] At room temperature, 0.1 mol Ca(NO 3 ) 2 ·4H 2 O (concentration 0.4 mol L -1 ) was dissolved in 250 mL of deionized water; and in another beaker, 500 mL of (NH 4 ) 2 CO 3 Solution (concentration 1 mol L -1 );(NH 4 ) 2 CO 3 The solution was slowly added with Ca(NO 3 ) 2 ·4H 2 O solution and placed on a magnetic stirrer for 30 minutes. Bubbles will be generated at the beginning. Finally, the precipitate is separated from the solution by suction filtration and repeatedly rinsed with deionized water until the ammonia smell is completely removed. Finally, vacuum drying is carried out at 60°C for 10 hours.

[0044] (3) Preparation of calcium manganese oxide

[0045] ①CaMnO 3 Preparation

[0046] 0.1 mol CaCO 3 and 0.1 mol MnCO 3 After the powder is completely mixed, gradually add 300mL of 1.5mol·L -1 HNO3 solution and stirred until completely dissolved; 2+ +Mn 2+ ) / CO 3 2- =600mL (NH 4 ) 2 CO 3 (Concentration 1 mol L -1 ) solution was added to the above solution; the mixture was then placed on a magnetic stirrer and stirred for 40 min, allowed to stand for 10 min, the precipitate was filtered three times with deionized water, and finally dried under vacuum at 80 ° C; the obtained powder was placed in a muffle furnace and the heating rate was 6 ° C min -1 , and calcined at 850 ° C for 7 hours. After the powder is calcined, it is naturally cooled to room temperature to obtain the product.

[0047] ②CaMn 3 O 6 Preparation

[0048] 0.1 mol CaCO 3 and 0.3 mol MnCO 3 After the powder is completely mixed, gradually add 300mL of 1.5mol·L -1 HNO 3 solution and stirred until completely dissolved; 2+ +Mn 2+ ) / CO 3 2- = 1200mL (NH 4 ) 2 CO 3 (Concentration 1 mol L -1 ) solution was added to the above solution; the mixture was then placed on a magnetic stirrer and stirred for 40 min, allowed to stand for 10 min, the precipitate was filtered three times with deionized water, and finally dried under vacuum at 80 ° C; the obtained powder was placed in a muffle furnace and the heating rate was 6 ° C min -1 , and calcined at 850 ° C for 7 hours. After the powder is calcined, it is naturally cooled to room temperature to obtain the product.

[0049] ③Ca 2 Mn 3 O 8 Preparation

[0050] 0.2 mol CaCO 3 and 0.3 mol MnCO 3 After the powder is completely mixed, gradually add 300mL of 1.5mol·L -1 HNO3 solution and stirred until completely dissolved; 2+ +Mn 2+ ) / CO 3 2- = 1500mL (NH 4 ) 2 CO 3 (Concentration 1 mol L -1 ) solution was added to the above solution; the mixture was then placed on a magnetic stirrer and stirred for 40 min, allowed to stand for 10 min, the precipitate was filtered three times with deionized water, and finally dried under vacuum at 80 ° C; the obtained powder was placed in a muffle furnace and the heating rate was 6 ° C min -1 , and calcined at 850 ° C for 7 hours. After the powder is calcined, it is naturally cooled to room temperature to obtain the product.

[0051] Example 2 Preparation of modified perovskite manganese oxide

[0052] (1) Take 3 g of the perovskite manganese oxide CaMn prepared in Example 1 3 O 6 The sample was placed in a beaker and 3 mol L -1 150mL of dilute nitric acid solution was placed on a magnetic stirrer at room temperature and stirred. Five groups of samples were set with different reaction times, namely 1h, 6h, 12h, 24h, and 72h. After the reaction, the precipitate was filtered until the pH value of the filtrate was neutral. The sample obtained after filtration was placed in an oven and dried at 80℃ for 24h to obtain the final product, modified CaMn 3 O 6 -1h~72h.

[0053] (2) Referring to the above steps, prepare modified CaMnO 3 -24h and Ca 2 Mn 3 O 8 -24h.

[0054] Example 3 Catalyst Activity Evaluation

[0055] The prepared catalysts were subjected to a selective catalytic oxidation experiment of ammonia, and the catalysts prepared in Examples 1 and 2 were subjected to an activity evaluation device for NH 3 -SCO activity test, the specific steps are as follows:

[0056] (1) Use 40-mesh and 60-mesh porous sieves to screen 0.1 g of the catalyst sample in turn to ensure the consistency of the particle size. Subsequently, the screened catalyst sample is thoroughly mixed with 0.4 g of quartz sand of the same mesh size (the purpose is to evenly disperse the catalyst in the quartz sand and eliminate the influence of internal diffusion). The fully mixed sample is loaded into a quartz tube. In order to fix the catalyst sample, it is wrapped with quartz wool and cordierite. Finally, the quartz tube containing the sample is placed in a heating furnace for subsequent treatment;

[0057] (2) Pretreatment was performed under dry air conditions with a total gas flow rate of 100 mL / min, the temperature was programmed to 300 °C and maintained for 1 h, and the heating rate was 5 °C / min;

[0058] (3) The reaction gas composition is 500ppm NH 3 , 10vol.%O 2 , N 2 Balance, the total gas flow rate is 200mL / min. The reaction temperature range is 120℃-300℃. First, increase the temperature to 120℃ at a rate of 5℃ / min and hold for 1h, then increase the temperature by 30℃ for 30min each time until 300℃.

[0059] NH 3 Conversion rate, N 2 Selectivity, NO generation rate, NO 2 Generation rate and N 2 The formula for calculating the O generation rate is as follows:

[0060]

[0061] Among them, [NH 3 ] in Indicates NH 3 The inlet concentration, [NH 3 ] out Indicates NH 3 The outlet concentration, [NO] out 、[NO 2 ] out , [N 2 O] out Respectively represent NO and NO 2 、N 2 The outlet concentration of O.

[0062] Figure 1 Different lengths of acid-induced surface disproportionation of CaMn 3 O 6 NH of perovskite manganese oxide 3 Conversion rate, it can be seen that with the increase of acid-induced surface disproportionation time, the catalytic activity increases significantly.3 O 6 Except for the above samples, the other samples all reached 100% conversion at a lower temperature of about 180℃. 3 O 6 -72h catalyst even reached NH 3 Conversion rate 100%. Figure 2 Different lengths of acid-induced surface disproportionation of CaMn 3 O 6 N in perovskite manganese oxide 2 Selectivity, it can be seen that CaMn 3 O 6 -72h N 2 The selectivity is relatively poor overall, CaMn 3 O 6 -24h N 2 The overall selectivity performance is the best, at 180℃ N 2 Selectivity can reach 80% without acid-induced surface disproportionation of CaMn 3 O 6 N 2 The selectivity is general, therefore, appropriate acid-induced surface disproportionation can greatly improve the CaMn 3 O 6 Catalyst N 2 Selective.

[0063] In summary, the different lengths of acid-induced surface disproportionation of CaMn 3 O 6 Among perovskite catalysts, CaMn 3 O 6 -24h catalyst NH 3 Oxidation activity and N 2 The best selectivity is achieved with an optimum reaction temperature of 180°C. If the temperature exceeds 180°C, the N 2 The selectivity dropped significantly, which shows that CaMn 3 O 6 Perovskite in NH 3 -SCO reaction temperature can not be too high, which also shows that CaMn 3 O 6 Perovskite catalysts in NH 3 -SCO reaction has good low temperature activity.

[0064] Figure 3 NH of catalysts with different calcium-manganese ratios before and after acid-induced surface disproportionation 3 Conversion rate, we can see that CaMnO 3 and CaMn 3 O 6 After 24 h of acid-induced surface disproportionation, NH3 The conversion rate was significantly improved, and NH 3 The conversion rate is close to 100%. Figure 4 is the N of catalysts with different calcium-manganese ratios before and after acid-induced surface disproportionation 2 Selectivity, the figure shows that the product CaMn after 24h of acid-induced surface disproportionation 3 O 6 -24h N 2 The overall selectivity performance is the best, especially at 180℃, its N 2 The selectivity can reach over 75%.

[0065] In summary, when the calcium-manganese ratio is 1:3 and the acid-induced surface disproportionation time is 24 h, the perovskite manganese oxide in NH 3 -SCO catalytic reaction has the best performance, and too long or too short acid disproportionation treatment cannot achieve good N 2 Selectivity, if N 2 Poor selectivity, even though NH 3 Even a high conversion rate cannot make the exhaust gas harmless, but will lead to NH 3 In order to prepare a better catalyst for the selective catalytic oxidation of ammonia, it is important to choose the appropriate disproportionation time and calcium-manganese ratio.

[0066] Example 4 XPS test analysis

[0067] The elemental composition and valence distribution of the catalyst surface were analyzed using an XLESCALAB 250Xi electron spectrometer (Thermo Fisher Scientific, USA). The samples were dried, ground and crushed for testing, using a Mg target (hv = 1253.6 eV) as the excitation light source, and the binding energy of the elements was calibrated using the C1s peak at 284.8 eV.

[0068] Figure 5 The XPS spectra of Mn 2p orbital electrons and O1s orbital electrons of catalysts with different calcium-manganese ratios after 24h acid-induced surface disproportionation. The peaks of Mn 2p orbital are respectively attributed to Mn 4+ (at 642.5eV), Mn 3+ (located at 641.2 eV) and a satellite peak at 644.1 eV, while the high binding energy peak on the O1s orbital (located near 531.1 eV) corresponds to the surface adsorbed oxygen species (O ads ), the low binding energy (near 529.4 eV) corresponds to the lattice oxygen species (O latt ) and hydroxyl oxygen (located near 533.0 eV). The Mn of the catalyst can be obtained by calculating the fitted peak area. 3+ / Mn4+ The larger the ratio, the lower the average valence of Mn ions on the catalyst surface. In order to maintain charge balance, the catalyst will form more oxygen vacancies, which are important active sites for catalytic oxidation reactions. In addition, low-valence Mn is also NH 3 The binding site of Mn 3+ / Mn 4+ The larger the ratio, the more conducive it is to promoting NH 3 The combination on the catalyst. ads / O latt The ratio of can be used to analyze the surface adsorption of oxygen species on the catalyst. The larger the ratio, the more oxygen species are adsorbed on the catalyst surface. 2 The more active substances that catalyze the oxidation reaction are formed on the active sites of the catalyst, the better the activity of the catalyst. 3 O 6 -24h catalyst Mn 3+ / Mn 4+ and O ads / O latt The ratios of are the largest, indicating that it is easier to combine with NH 3 , there are more oxygen vacancies and more active oxygen species, so its NH 3 The better the catalytic oxidation performance, the better the catalytic oxidation performance. In summary, by adjusting the acid-induced surface disproportionation time and the calcium-manganese ratio, the best NH 3 -SCO catalyst.

[0069] Table 1 Mn of catalysts with different calcium-manganese ratios 3+ / Mn 4+ With O ads / O latt Ratio results

[0070]

[0071] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A modified perovskite manganese oxide for catalytic oxidation of NH3, characterized in that Prepared by the following steps: (1) adding MnCO3 and CaCO3 to HNO3 solution and stirring until completely dissolved, adding (NH4)2CO3 solution, stirring, standing, filtering, drying, and calcining to obtain calcium manganese oxide; (2) Take the calcium manganese oxide prepared in step (1), add HNO3 solution, stir to react, filter, adjust the pH, and dry to obtain a modified perovskite manganese oxide for NH3 catalytic oxidation.

2. The modified perovskite manganese oxide for catalytic oxidation of NH3 according to claim 1, characterized in that: The molar ratio of MnCO3 to CaCO3 in step (1) is 1-2:1-3; The ratio of the total amount of MnCO3 and CaCO3 to the amount of NH4HCO3 in step (1) is 1:1 to 5.

3. The modified perovskite manganese oxide for catalytic oxidation of NH3 according to claim 2, characterized in that: The molar ratio of MnCO3 and CaCO3 in step (1) is 1:

3.

4. The modified perovskite manganese oxide for catalytic oxidation of NH3 according to claim 1, characterized in that: The stirring reaction time in step (2) is 1 to 72 hours.

5. The modified perovskite manganese oxide for catalytic oxidation of NH3 according to claim 4, characterized in that: The stirring reaction time in step (2) is 24 hours.

6. The modified perovskite manganese oxide for catalytic oxidation of NH3 according to claim 1, characterized in that: The concentration of the HNO3 solution in step (1) is 1 to 2 mol·L -1 ; The concentration of the (NH4)2CO3 solution in step (1) is 1 to 2 mol·L -1 ; The stirring time in step (1) is 30 to 60 minutes; The standing time in step (1) is 5 to 20 minutes; The drying condition in step (1) is drying at 80°C.

7. The modified perovskite manganese oxide for catalytic oxidation of NH3 according to claim 1, characterized in that: The calcination conditions in step (1) are to increase the temperature to 800-1000° C. at a heating rate of 5-10° C. / min and calcine for 5-8 hours.

8. The modified perovskite manganese oxide for catalytic oxidation of NH3 according to claim 1, characterized in that: The concentration of the HNO3 solution in step (2) is 1 to 5 mol·L -1 ; The pH adjustment in step (2) is to adjust the pH to 6-8; The drying condition in step (2) is 80° C. for 24 hours.

9. Use of the modified perovskite manganese oxide for catalytic oxidation of NH3 according to any one of claims 1 to 8 in catalyzing NH3-SCO reaction.

10. Use of the modified perovskite manganese oxide for catalytic oxidation of NH3 according to any one of claims 1 to 8 in the preparation of a catalyst for odor in a farm or a catalyst for waste gas treatment in the hairdressing industry.

Citation Information

Patent Citations

  • Porous microsphere perovskite type calcium manganese oxide compound and preparation method and application thereof

    CN102867965A

  • Preparation method of calcium manganese oxide compound and application thereof as ozone oxidation catalyst

    CN108128809A

  • Ammonia oxidation catalyst for high-acidity single-coating perovskite-based diesel engine and preparation method and use method of ammonia oxidation catalyst

    CN111841572A

Cited By

  • Perovskite catalyst for producing nitrogen oxide through low-temperature ammonia gas oxidation and preparation method and application thereof

    CN121060542A