Multi-layer core-shell structure catalyst as well as preparation method and application thereof

By developing a multi-layer core-shell structure catalyst with acidic spherical shell-like core and multi-layer spherical shell-like shell, the problems of multi-step reaction and multiple catalysts in the synthesis of biomass RJ-4 and JP-10 are solved, and a one-step preparation is achieved RJ-4 or JP-10 precursors reduce energy consumption and equipment requirements, and improve conversion and product yield.

CN118950103AActive Publication Date: 2024-11-15QINGDAO UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411001318.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The existing synthesis methods of biomass RJ-4 and JP-10 require multiple reactions and multiple catalysts, resulting in waste of products, high energy consumption, complex equipment requirements, large mass transfer resistance, difficult to separate and purify intermediates, and hydrogenation The deoxygenation reaction conditions are harsh.

Method used

Develop a multi-layer core-shell structural catalyst with an acid spherical core and a multi-layer spherical shell with holes in the inner core shell wall and shell layer, which is used to prepare RJ-4 or JP-10 precursors in one-step catalyzed biomass raw materials, Mass transfer resistance and intermediate separation and purification are avoided.

Benefits of technology

The RJ-4 or JP-10 precursors are achieved in one-step preparation of biomass raw materials, reducing mass transfer resistance, simplifying the process flow, improving the conversion rate and product yield, and avoiding the harsh conditions of hydrodeoxygenation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950103A_ABST
    Figure CN118950103A_ABST
Patent Text Reader

Abstract

The invention discloses a multilayer core-shell structure catalyst. The multilayer core-shell structure catalyst comprises an acidic spherical-shell-shaped inner core and a multilayer spherical-shell-shaped outer shell. The invention also discloses a preparation method of the multi-layer core-shell structure catalyst and application of the multi-layer core-shell structure catalyst in catalyzing biomass raw materials to prepare oxygen-free precursors of RJ-4 or JP-10 in one step.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to a multilayer core-shell structure catalyst, a preparation method thereof and use thereof in the synthesis of a high-density fuel precursor. Background Art

[0002] RJ-4 (bridged tetrahydromethyldicyclopentadiene dimer) is the first petroleum-based high-density liquid fuel that was artificially synthesized and used in the Talos missile. With the increasing attention paid to fossil resources, reports on the synthesis of RJ-4 by various biomass methods have gradually emerged. The literature (ChemSusChem 2011, 4, 465-469) reported that methylcyclopentene methanol was prepared from linalool as a raw material through the development of organic coordination precious metal rhodium, and then methylcyclopentene methanol was dehydrated and condensed under an acidic catalyst to prepare the RJ-4 precursor. However, the linalool here is a plant metabolite and has limited sources. The literature (Green Chem. 2020, 22, 7765-7768.) reported that 5-hydroxymethylfurfural was used as raw material, and 2,5-hexanedione was first prepared by selective hydrodeoxygenation ring opening under the action of Ni2P / mordenite catalyst, and then methylcyclopentenone was prepared by aldehyde condensation under alkaline catalyst, and then methylcyclopentenol was prepared from methylcyclopentenone by selective hydrodeoxygenation. Finally, methylcyclopentenol was dehydrated and condensed under the action of acidic catalyst to synthesize RJ-4 and a mixture of methylcyclohexadiene trimers. The literature (ChemSusChem 2011, 4, 465-469) reported that 2,5-hexanedione was used as the raw material, and 3-methyl-2-cyclopentene-1-one was generated by base-catalyzed 2,5-hexanedione aldehyde condensation reaction, and then it was selectively reduced to 3-methyl-2-cyclopentene-1-ol by [RuCl2(PPh3)3 / NH2(CH2)2NH2 / KOH], and then dehydrated and condensed under AlPO4 / MgSO4 to prepare RJ-4 precursor. It can be seen that the current synthesis of biomass RJ-4 is either limited in the source of raw materials; or although the source of raw materials is extensive, it needs to go through multiple steps to convert to the product RJ-4 precursor.

[0003] JP-10 (tetrahydrodicyclopentadiene) has higher energy density (0.94 g / mL), better thermal stability and lower freezing point than traditional aviation fuel. Traditional JP-10 is mainly prepared by dimerization, hydrogenation and isomerization of cyclopentadiene from petroleum refining, and the source of raw materials is limited. Recently, biomass JP-10 synthesis has also been developed. The literature reports that alkaline catalysts catalyze the rearrangement of furfuryl alcohol to produce 4-hydroxycyclopent-2-enone, and then 4-hydroxycyclopent-2-enone is selectively hydrogenated and deoxygenated to produce 1,3-cyclopentanediol. 1,3-cyclopentanediol is dehydrated to produce cyclopentadiene, and then undergoes a Diels-Alder reaction to produce cyclopentadiene dimers. Finally, the cyclopentadiene dimers are hydrogenated and isomerized to bridge tetrahydrodicyclopentadiene dimers. In other words, it takes four steps from furfuryl alcohol to the precursor of JP-10 (Angew.Chem.Int .Ed.2019,58,12154–12158; Shaanxi University of Science and Technology, 2023.DOI:10.27733 / d.cnki.gsxlg.2023.000292.); It is estimated that the cost of JP-10 obtained by this synthesis method is less than US$5,600 / ton. Moreover, if the price of furfuryl alcohol is expected to drop to US$400 / ton, JP-10 can reach US$2,547 / ton, which is much lower than the current market price of US$7,091 / ton of petroleum-based JP-10. It can be seen that the current synthesis of biomass JP-10 also requires multi-step reactions to achieve.

[0004] At present, there are many types of catalysts used to synthesize RJ-4 and JP-10 from biomass raw materials. The synthesis of RJ-4 precursor from cellulose-derived raw material 2,5-hexanedione is mainly achieved through multiple steps, each step using a different catalyst, the properties of these catalysts are completely different, and the reaction products of each step need to be separated and purified. For example, the literature (Green Chem. 2020, 22, 7765-7768.) uses alkaline catalysts such as Mg-Zr-O, MgO, TiO2, Al2O3, Mg-Al-O, K3PO4, NaOH, etc. to catalyze 2,5-hexanedione in water or / and toluene solvent to first synthesize methylcyclopentenone, and then methylcyclopentenone is reacted in NaBH4 / Ce 3+ / Methanol system is selectively hydrogenated to synthesize methylcyclopentenol, and then methylcyclopentenol is dehydrated and condensed under the action of molecular sieve acid catalyst to generate RJ-4 precursor. The literature (ChemSusChem 2021,14,339–343) uses KOH as a catalyst to catalyze the synthesis of methylcyclopentenone from 2,5-hexanedione, and then uses RuCl2[P(C6H5)3]3 to selectively reduce methylcyclopentenone to methylcyclopentenol, and finally dehydrates and condenses under the catalysis of AlPO4 and MgSO4 to prepare RJ-4 precursor. The synthesis of JP-10 precursor from hemicellulose-derived raw material furfuryl alcohol is also achieved through multi-step reactions. Each time, the product needs to be separated and purified before being used in the next step reaction, and the properties of the catalysts used in each step are also completely different. As reported in (Angew. Chem. Int. Ed. 2019, 58, 12154–12158), furfuryl alcohol was converted into 4-hydroxy-cyclopentene-2-one catalyzed by CaO, and then 4-hydroxy-cyclopentene-2-one was selectively reduced to cyclopentanediol using lanthanum niobium nickel, and finally 4-hydroxy-cyclopentene-2-one was dehydrated and condensed to cyclopentanediol using molecular sieve HUSY to prepare JP-10 precursor.

[0005] In summary, the currently reported synthesis of RJ-4 or JP-10 from biomass all adopt a multi-step method, which is difficult to separate and purify products and recycle catalysts after multiple intermediate product separation and purification and the application of multiple catalysts, and even the application of homogeneous catalysts. The final hydrodeoxygenation reaction has very harsh reaction conditions due to the presence of carbonyl groups. In fact, the cost of synthesizing RJ-4 or JP-10 from biomass mainly comes from raw materials, process energy consumption and catalysts. Because the current route has many steps, each step requires separation and purification, which consumes a lot of energy. In addition, multi-step reactions also have high requirements for equipment.

[0006] The development of efficient catalysts can greatly save process energy consumption and equipment requirements. Core-shell catalysts have received extensive attention in the field of catalysts because they can combine multiple functions of catalysts to catalyze cascade reactions. The core-shell catalysts currently under development usually use SiO2, zeolite, CeO2, Al2O3, etc. as shells, and the preparation methods include sol-gel method, microemulsion method, physical coating method, precipitation method, self-assembly method, atomic layer deposition method, etc. Patents CN118002194A, CN117983289A, CN110064399A, CN117884131A, CN117328096A, CN113394417A, CN106953104A, CN109603848A, CN105797749A, as well as master's and doctoral dissertations and journals, such as: Journal of Fuel Chemistry and Technology (Chinese and English), 2024, 52(03): 353-361. DOI: 10.19906 / j.cnki.JFCT.2023072, Chinese Journal of Environmental Science, 20 24,44(01):193-201.DOI:10.19674 / j.cnki.issn1000-6923.20230908.018, Journal of Chemical Industry, 2023,74(06):2458-2467, etc. have reported the synthesis of three-layer core-shell structure catalysts, in which the core and shell layers may involve metal alloys, metal oxides, carbon layers, silicon dioxide, aluminum oxide, etc. However, as a catalyst, this multi-layer core-shell structure generally has the problem of large mass transfer resistance, and these reports have not seen core-shell catalysts with an acidic core, a metal oxide middle layer, and an alkaline outer shell structure.

[0007] In summary, the prior art has the following problems: 1. The RJ-4 or JP-10 precursor obtained by using biomass as a raw material reaction is a multi-step process, and the product after each step of the reaction needs to be separated, purified and transferred, resulting in product waste and the use of multiple solvents and equipment, which is cumbersome to operate. 2. The RJ-4 or JP-10 precursor obtained by using biomass as a raw material reaction uses a variety of different catalysts, which increases the complexity of the operation. 3. The RJ-4 or JP-10 precursor obtained by using biomass as a raw material reaction contains oxygen, resulting in harsh conditions for hydrogenation and deoxygenation to obtain the final RJ-4 or JP-10 product. 4. The mass transfer resistance of the multi-layer core-shell structure catalyst used is large.

[0008] The present invention has been proposed to solve the above-mentioned problems. Summary of the invention

[0009] The present invention discloses for the first time a multi-layered shell structure catalyst comprising an acidic spherical shell core and a multi-layered spherical shell shell and a preparation method thereof. The core of the multi-layered shell structure catalyst of the present invention is hollow, and there are holes on its shell wall and on the two shell layers, and the holes are interconnected, such as Figure 1The multi-layer shell structure catalyst of the present invention is used for catalytic reaction to prepare RJ-4 precursor or JP-10 precursor in one step, and the precursor does not contain oxygen, thus solving the problem of many steps in the synthesis of RJ-4 or JP-10 in the prior art.

[0010] The technical solution of the present invention is as follows:

[0011] The first aspect of the present invention discloses a multi-layer core-shell structure catalyst, which comprises: an acidic spherical shell core and a multi-layer spherical shell shell. The core shell layer and the multi-layer shell layer can be regular spherical shells, or irregular spherical shells, such as ellipsoidal shells, flat spherical shells or other irregular spherical shells.

[0012] Preferably, there are holes on the shell wall of the inner core, the pore size is 0.5nm-30nm, the average diameter of the hollow cavity in the shell wall of the inner core is 5.0-200nm, and the shell wall thickness of the inner core is 5-100nm; the acidic spherical shell inner core is one of acidic metal oxides, molecular sieves, a composite of acidic metal oxides and molecular sieves, or a composite of acidic metal oxides and silica.

[0013] Preferably, the acidic metal oxide is NbWOx, WO3, Al2O3, Nb2O5, SiO2-Al2O3, SiO2-Nb2O5, MOF-808-2.5SO4, HfTPA, SnTPA, ZrTPA, SO4 2- / ZrO2, MMT-K10, or HPW; the molecular sieve is one or more of Al-MCM-41, Al-SBA-15, Al-SBA-16, Ti-MCM-41, HY, Hβ, HZSM-5, MCM-41, ITQ, KIT-6 or Mordenite.

[0014] Preferably, the outer shell is a double-layered shell, both shells have holes on their walls, and the pore size is 0.5nm-100nm; the inner shell is a metal oxide composite layer, and the thickness of the inner shell wall is 5-100nm; the outer shell is a solid base layer, and the thickness of the outer shell wall is 10-200nm.

[0015] Preferably, the metal oxide composite is ZnMoO X 、ZrMoO x 、SiMoO x 、FeMoO x 、ZnCoO X 、ZrCoO x 、SiCoO x 、FeCoO x 、CeMoO x 、CeCoO X、SiMoO x 、CuCoO X 、CuMoO X 、ZnCuMoO X 、CuFeMoO x 、ZnFeCoO x One or more of the following; the solid base is CaO and / or MgO, or a complex of CaO and / or MgO and silicon dioxide.

[0016] The second aspect of the present invention discloses a method for preparing the multilayer core-shell structure catalyst, comprising the following steps:

[0017] (1) adding a certain amount of the first surfactant to water or a mixed solution of water and the first alcohol to dissolve and adding carbon spheres, adding the core precursor and continuing to mix for a period of time; adjusting the pH value to 10-11 and maintaining it, and then hydrothermally crystallizing; filtering, washing with water, and drying to obtain a solid powder S1; or,

[0018] The carbon spheres and the second surfactant are added to the second alcohol and stirred to mix evenly, and then the core precursor is added and stirred to mix evenly; then water is added and stirred to mix to obtain a sol; the obtained sol is gelled at a certain temperature for a period of time and then heated and dried for a period of time to obtain a solid powder S1;

[0019] (2) adding the solid powder S1 obtained in step (1) and the third surfactant to the third alcohol and mixing them evenly, then adding the inner shell layer precursor and mixing them evenly; adding water and continuing to stir and adjusting the pH value of the solution to form a sol; gelling the obtained sol at a certain temperature for a period of time; then drying the gelled sample for a period of time to obtain a catalyst precursor S2;

[0020] (3) dissolving a certain amount of S2 and a fourth surfactant in an aqueous solution of ammonia in ethanol, and then adding a solid base precursor and ethanol to mix; separating the solid after gelation for a period of time, washing and drying, and then calcining for a period of time to obtain the multilayer core-shell structure catalyst S3.

[0021] Preferably, the first surfactant, the second surfactant, the third surfactant and the fourth surfactant are each independently a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123), a polyethylene glycol-polypropylene glycol-polyethylene glycol triblock copolymer (F127), polyvinyl pyrrolidone (PVP), polyethylene oxide (PEO), oleylamine polyoxyethylene ether (PEG), polyoxyacrylamide (PPG), sorbitan monooleate polyoxyethylene ether (Tween 80), sorbitan monooleate (Span 80), dodecylphenol polyoxyethylene ether (OP-10), isooctylphenyl polyoxyethylene ether (TX-100), octadecyl alcohol polyoxyethylene ether (Brij 76), fatty alcohol polyoxyethylene ether (AEO-9), polyethylene glycol octylphenyl ether (TritonX-100), coconut fatty acid monoethanolamide (CMEA), C12-14 alkyl glucoside (APG), fatty alcohol polyoxyethylene 3 / 7 / 9 ether (AEO-3 / 7 / 9), nonylphenol polyoxyethylene ether (TX-4.5 / 6.5 / 10 / 15 / 20 / 40), hydroxyl synthetic alcohol polyoxyethylene ether (GENAPOL UD-080), hydroxyl synthetic alcohol polyoxyethylene ether (UD-080), triethanolamine monostearate (emulsifier 4H), dodecyltrimethylammonium chloride (DTAC), dodecyltrimethylammonium bromide (DTAB), hexadecyltrimethylammonium chloride (CTAC), hexadecyltrimethylammonium bromide (CTAB), tetrabutylammonium hydroxide (TBAOH), tetrapropylammonium hydroxide (TPAOH), dodecyldimethylbenzylammonium chloride (DDAC), dodecyldimethylbenzylammonium bromide (DDAB), behenyltrimethylammonium methyl sulfate (BTMS), alkyl pyridine, alkyl morpholine, alkyl imidazoline, alkyl aziridine, lauryl amide propyl amine oxide (AMP), cocamidopropyl betaine (DEHYTON K), dodecyl propyl betaine (BS-12), dodecyl dimethyl amine oxide (OA-12), cocamidopropyl dimethyl betaine (CAB-35), cocamidopropyl hydroxysulfonic acid betaine (CHS-35), coconut imidazoline (CAMA-30), fatty alcohol (9EO) (AEC-9), sodium lauryl sulfate (SDS), secondary alkyl sulfate (Teep01), fatty alcohol sulfate (FAS), fatty alcohol sulfate monoethanolamine salt (ASEA), fatty alcohol polyoxyethylene ether sulfate (AES), α-sulfated fatty acid disodium salt (DSFA), dodecyl phosphate (MAP-85), dodecyl phosphate potassium salt (MAP-K), dodecyl phosphate triethanolamine (MAP-A), sodium tetrapropylene benzene sulfonate (ABS), sodium alkyl benzene sulfonate (LAS), sodium dodecyl benzene sulfonate (SDBS), primary alkyl sulfonate (AS), secondary alkyl sulfonate (SAS), α-olefin sulfonate (AOS), α-sulfonated fatty acid methyl ester (MES), fatty acid sulfonalkyl ester (1gepon A), fatty acid sulfonamide (Igepon T), sodium dioctyl sulfosuccinate (AerosolOT), alkyl glycerol ether sulfonate (AGS), sodium dibutyl naphthalene sulfonate (penetrant BX), sodium p-methoxy fatty amide benzene sulfonate (cleaner LS), sodium methylene bis naphthalene sulfonate (NNO), fatty acid methyl ester sulfonate (MES), sodium fatty acid (SOAP), Lamepon A, sodium carboxymethyl cellulose (SCMC), sodium acyl sarcosine (DX107), one or more thereof, the surfactant concentration is 0.1% (w / v) to 10% (w / v). .

[0022] Preferably, the first alcohol in step (1) is one or both of ethanol and propanol, and the second alcohol is propanol; the third alcohol in step (2) is propanol; the hydrothermal crystallization temperature in step (1) is 100-140°C, and the time is 1-4 days; the gelation temperature in step (1) or (2) is 45-55°C, and the time is 1-12 days; the drying temperature is 90°C-120°C, and the time is 10-24h; the calcination temperature in step (3) is 350°C-800°C, and the time is more than 2h.

[0023] Preferably, the acidic metal oxide precursor in the inner core precursor of step (1) is one or more of tungsten chloride, zinc chloride, phosphotungstic acid, niobium chloride, zirconium oxychloride, zirconium chloride, cerium nitrate, niobium oxalate, aluminum chloride, hafnium chloride, tin chloride, tetraethyl silicate, 1,2-bis(triethoxysilyl)ethane, tetrabutyl titanate, sodium silicate, and aluminum silicate; the inner shell precursor of step (2) is a co-precipitate of at least two of zinc salt, cerium salt, copper salt, molybdenum salt, tetraethyl silicate or / and 1,2-bis(triethoxysilyl)ethane, zirconium salt, iron salt, and cobalt salt; and the solid base precursor is a co-precipitate of one or two of magnesium salt or calcium salt or a complex thereof with tetraethyl silicate or / and 1,2-bis(triethoxysilyl)ethane.

[0024] The third aspect of the present invention discloses the use of the multilayer core-shell structure catalyst for catalyzing biomass raw materials to prepare oxygen-free precursors of RJ-4 or JP-10 in one step. The biomass raw materials are selected from 2,5-hexanedione and / or furfuryl alcohol; the RJ-4 precursor containing only CC single bonds and C=C double bonds and no oxygen is synthesized from 2,5-hexanedione; and the JP-10 precursor containing only CC single bonds and C=C double bonds and no oxygen is synthesized from furfuryl alcohol.

[0025] Beneficial effects of the present invention:

[0026] 1. The present invention synthesizes for the first time a multilayer core-shell structure catalyst having an acidic spherical shell core, a metal oxide spherical shell middle layer, and an alkaline metal oxide spherical shell outer shell; wherein the shell wall of the core and the two layers of the outer shell have holes, which are interconnected, such as Figure 1 As shown, the permeability of the pores is increased, which reduces the mass transfer resistance and improves the mass transfer effect for catalytic reactions.

[0027] 2. The multilayer core-shell structure catalyst of the present invention can be considered as a three-layer spherical shell structure with a hollow cavity, which is composed of an acidic core layer, a metal oxide middle layer and an alkaline metal oxide outer layer from the inside to the outside; the inner core layer and the two outer shell layers can be regular spherical shells, or non-spherical shells, such as ellipsoidal shells, flat spherical shells or other irregular spherical shells; for catalytic reactions, the three-layer structure plays the role of ring formation, selective hydrogenation and dehydration condensation from the outside to the inside. The core-shell structure catalyst of the present invention realizes a combination of multiple catalysts, and one catalyst can realize the one-step synthesis of RJ-4 precursor or JP-10 precursor, which solves the problem that multiple different catalysts are needed to synthesize RJ-4 precursor or JP-10 precursor from biomass, and avoids the separation, purification and transfer of intermediates.

[0028] 3. The multilayer core-shell structure catalyst of the present invention includes but is not limited to the following: NbWOx@ZnMoO X @MgO、Al-MCM-41@ZrMoO x @CaO、WO3@SiMoO x @MgO-CaO、Al-SBA-15@FeMoO x @SiO2-MgO、Al-SBA-16@ZnCoO X @SiO2-CaO、Ti-MCM-41@ZrCoO x @SiO2-MgO-CaO、HY@SiCoO x @SiO2-MgO-CaO, Hβ@FeCoO x @SiO2-CaO、HZSM-5@CeMoO x @SiO2-MgO、Al2O3@CeCoO X @MgO-CaO、Nb2O5@SiMoO x @CaO、SiO2-Al2O3@CuCoO X @MgO, CsTPA@CuMoO X @MgO、HfTPA / MCM-41@ZnCuMoO X @CaO、SiO2-Nb2O5@ZrMoO x @MgO-CaO、MOF-808-2.5SO4@SiMoO x @SiO2-MgO, HfTPA@CuFeMoO x @SiO2-CaO, SnTPA@ZnCoO X @SiO2-MgO-CaO, ZrTPA@ZrCoO x @SiO2-MgO-CaO, SO4 2- / ZrO2@SiCoOx @SiO2-CaO, ITQ@ZnFeCoO x @SiO2-MgO, KIT-6@CeMoO x @MgO-CaO、Mordenite@CeCoO X @CaO、MMT-K10@SiMoO x @MgO、HPW / MCM-41@CuMoO X @MgO. In the multilayer core-shell structure catalyst of the present invention, the first @ before the core-shell structure indicates the composition of the core, the " / " indicates the composite of the two, the b between the two @ indicates the composition of the inner shell, and the c after the second @ indicates the composition of the outer shell. If the core-shell layer is a bimetal or a metal and silicon, the molar ratio is 1:20 to 20:1; if it is a trimetal or silicon and two metals, the molar ratio is 1:20:1 to 20:1:20.

[0029] 4. The preparation method of the multilayer core-shell structure catalyst of the present invention uses carbon balls and prepares a hollow spherical shell core through a subsequent high-temperature calcination step; at the same time, the surfactant acting as a template is removed through the calcination step to form interconnected holes on the shell wall of the core and the shell walls of the two shells; the use of the multilayer core-shell structure catalyst of the present invention solves the problems of high mass transfer pressure of the solid core, weak permeability between the core and shell layers, and high mass transfer resistance in the prior art.

[0030] 5. The multilayer core-shell structure catalyst of the present invention is used for one-step catalysis of synthesizing RJ-4 precursor from biomass 2,5-hexanedione or synthesizing JP-10 precursor from biomass furfuryl alcohol. The product RJ-4 precursor or JP-10 precursor does not contain oxygen but only has CC single bonds and unsaturated C=C double bonds. The precursor is then hydrogenated and saturated to obtain RJ-4 or JP-10, which is easy to achieve under mild conditions and avoids the harsh conditions of prior art hydrogenation and deoxygenation. The separation, purification and transfer of intermediates are avoided in the process of obtaining RJ-4 or JP-10 precursor in one step, simplifying the synthesis process of RJ-4 or JP-10. Therefore, the core-shell structure catalyst of the present invention is used for the catalytic reaction of synthesizing RJ-4 precursor from biomass 2,5-hexanedione or synthesizing JP-10 precursor from biomass furfuryl alcohol, which is innovative in terms of catalyst, reaction process method and technical means.

[0031] 6. The multilayer core-shell structure catalyst of the present invention is used for one-step catalysis of biomass 2,5-hexanedione to synthesize RJ-4 precursor, with a raw material conversion rate of 100% and a fuel precursor yield of not less than 75%; it is used for one-step catalysis of biomass furfuryl alcohol to synthesize JP-10 precursor, with a raw material conversion rate of 100% and a fuel precursor yield of not less than 70%. The raw material is completely converted and the product yield is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of the multi-layer core-shell structure catalyst of the present invention.

[0033] Figure 2 The schematic diagram of the multilayer core-shell structure catalyst of the present invention is used to catalyze the one-step preparation of RJ-4 or JP-10 containing only C=C double bond precursors from biomass raw materials; (a) RJ-4 precursor is synthesized from 2,5-hexanedione; (b) JP-10 precursor is synthesized from furfuryl alcohol. DETAILED DESCRIPTION

[0034] The technical scheme of the present invention is described in detail below with reference to specific examples. The raw materials used in the examples are all commercial products unless otherwise specified; the processes used are all conventional processes in the art unless otherwise specified.

[0035] The schematic diagram of the multilayer core-shell structure catalyst of the present invention is as follows Figure 1 The layered core-shell structure catalyst of the present invention can be used to obtain the RJ-4 precursor from the biomass 2,5-hexanedione or the JP-10 precursor from the furfuryl alcohol in one step. Figure 2 shown.

[0036] The present invention Figure 1 The multilayer core-shell structure catalyst shown comprises: an acidic spherical shell core and a multilayer spherical shell shell. The core shell layer and the multilayer shell layer can be regular spherical shells, or irregular spherical shells, such as ellipsoidal shells, flat spherical shells or other irregular spherical shells.

[0037] The inner core has holes on its shell wall, the pore diameter is 0.5nm-30nm, the average diameter of the hollow cavity in the inner core shell wall is 5.0-200nm, and the thickness of the inner core shell wall is 5-100nm; the acidic spherical shell inner core is one of acidic metal oxide, molecular sieve, a composite of acidic metal oxide and molecular sieve, or a composite of acidic metal oxide and silicon dioxide.

[0038] Among them, acidic metal oxides are NbWOx, WO3, Al2O3, Nb2O5, SiO2-Al2O3, SiO2-Nb2O5, MOF-808-2.5SO4, HfTPA, SnTPA, ZrTPA, SO4 2- / ZrO2, MMT-K10, or HPW; the molecular sieve is one or more of Al-MCM-41, Al-SBA-15, Al-SBA-16, Ti-MCM-41, HY, Hβ, HZSM-5, MCM-41, ITQ, KIT-6 or Mordenite.

[0039] The outer shell is double-layered, both shells have holes on their walls, and the pore diameter is 0.5nm-100nm; the inner shell is a metal oxide composite layer, and the thickness of the inner shell wall is 5-100nm; the outer shell is a solid base layer, and the thickness of the outer shell wall is 10-200nm.

[0040] Among them, the metal oxide composite is ZnMoO X 、ZrMoO x 、SiMoO x 、FeMoO x 、ZnCoO X 、ZrCoO x 、SiCoO x 、FeCoO x 、CeMoO x 、CeCoO X 、SiMoO x 、CuCoO X 、CuMoO X 、ZnCuMoO X 、CuFeMoO x 、ZnFeCoO x One or more of the following; the solid base is CaO and / or MgO, or a complex of CaO and / or MgO and silicon dioxide.

[0041] The multilayer core-shell structure catalyst of the present invention includes but is not limited to the following: NbWOx@ZnMoO X @MgO、Al-MCM-41@ZrMoO x @CaO、WO3@SiMoO x @MgO-CaO、Al-SBA-15@FeMoO x @SiO2-MgO、Al-SBA-16@ZnCoO X @SiO2-CaO、Ti-MCM-41@ZrCoO x @SiO2-MgO-CaO、HY@SiCoO x @SiO2-MgO-CaO, Hβ@FeCoO x @SiO2-CaO、HZSM-5@CeMoO x @SiO2-MgO、Al2O3@CeCoO X @MgO-CaO、Nb2O5@SiMoO x @CaO、SiO2-Al2O3@CuCoO X @MgO, CsTPA@CuMoO X @MgO、HfTPA / MCM-41@ZnCuMoO X@CaO、SiO2-Nb2O5@ZrMoO x @MgO-CaO、MOF-808-2.5SO4@SiMoO x @SiO2-MgO, HfTPA@CuFeMoO x @SiO2-CaO, SnTPA@ZnCoO X @SiO2-MgO-CaO, ZrTPA@ZrCoO x @SiO2-MgO-CaO, SO4 2- / ZrO2@SiCoO x @SiO2-CaO, ITQ@ZnFeCoO x @SiO2-MgO, KIT-6@CeMoO x @MgO-CaO、Mordenite@CeCoO X @CaO、MMT-K10@SiMoO x @MgO、HPW / MCM-41@CuMoO X @MgO. If the core-shell layer is a bimetal or a metal and silicon, the molar ratio is 1:20 to 20:1; if it is a trimetal or silicon and two metals, the molar ratio is 1:20:1 to 20:1:20.

[0042] The preparation method of the multilayer core-shell structure catalyst of the present invention comprises the following steps:

[0043] (1) adding a certain amount of the first surfactant to water or a mixed solution of water and the first alcohol to dissolve and adding carbon spheres, adding the core precursor in sequence while stirring and continuing stirring for 2-6 hours; adjusting the pH value to 10-11, maintaining for 2 hours, and then placing it in a polytetrafluoroethylene-lined stainless steel reactor, hydrothermally crystallizing at 100-140° C. for 1-4 days, filtering the product after the crystallization, washing with water, and drying at 90-120° C. for 10-24 hours to obtain the acidic core precursor S1; or,

[0044] Add the carbon spheres and the second surfactant to the second alcohol and stir and mix evenly, then add the core precursor and continue to stir and mix evenly; then add water and continue to stir and mix to obtain a sol; gel the obtained sol at 45-55°C for 1-12 days and then heat it to 90-120°C and dry it for 10-24 hours to obtain an acidic core precursor S1; using an aqueous solvent requires hydrothermal crystallization;

[0045] (2) adding the solid powder S1 obtained in step (1) and the third surfactant to the third alcohol and mixing them evenly, then adding the inner shell precursor and mixing them evenly; adding water and continuing to stir and adjusting the pH value of the solution to form a sol; gelling the obtained sol in a culture dish at 45-55° C. for 1-12 days; then drying the aged gel sample at 90-120° C. for 10-24 hours to obtain a catalyst precursor S2 having an acidic center and an outer shell structure with a metal oxide complex precursor;

[0046] (3) A certain amount of S2 and a fourth surfactant are dissolved in an aqueous solution of ammonia in ethanol, and then a solid base precursor and / or a silica precursor and ethanol are added and stirred, and gelled in a culture dish at 45-55° C. for 1-12 days. The reaction product is collected by centrifugation, washed with water three times, dried at 90-120° C. for 10-24 hours, and then calcined in a muffle furnace at 350-800° C. for more than 2 hours to obtain the multilayer core-shell structure catalyst S3.

[0047] The first surfactant, the second surfactant, the third surfactant and the fourth surfactant are each independently a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123), a polyethylene glycol-polypropylene glycol-polyethylene glycol triblock copolymer (F127), polyvinyl pyrrolidone (PVP), polyethylene oxide (PEO), oleylamine polyoxyethylene ether (PEG), polyoxyacrylamide (PPG), sorbitan monooleate polyoxyethylene ether (Tween 80), sorbitan monooleate (Span 80), dodecylphenol polyoxyethylene ether (OP-10), isooctylphenyl polyoxyethylene ether (TX-100), octadecyl alcohol polyoxyethylene ether (Brij 76), fatty alcohol polyoxyethylene ether (AEO-9), polyethylene glycol octylphenyl ether (TritonX-100), coconut fatty acid monoethanolamide (CMEA), C12-14 alkyl glucoside (APG), fatty alcohol polyoxyethylene 3 / 7 / 9 ether (AEO-3 / 7 / 9), nonylphenol polyoxyethylene ether (TX-4.5 / 6.5 / 10 / 15 / 20 / 40), hydroxyl synthetic alcohol polyoxyethylene ether (GENAPOL UD-080), hydroxyl synthetic alcohol polyoxyethylene ether (UD-080), triethanolamine monostearate (emulsifier 4H), dodecyltrimethylammonium chloride (DTAC), dodecyltrimethylammonium bromide (DTAB), hexadecyltrimethylammonium chloride (CTAC), hexadecyltrimethylammonium bromide (CTAB), tetrabutylammonium hydroxide (TBAOH), tetrapropylammonium hydroxide (TPAOH), dodecyldimethylbenzylammonium chloride (DDAC), dodecyldimethylbenzylammonium bromide (DDAB), behenyltrimethylammonium methyl sulfate (BTMS), alkyl pyridine, alkyl morpholine, alkyl imidazoline, alkyl aziridine, lauryl amide propyl amine oxide (AMP), cocamidopropyl betaine (DEHYTON K), dodecyl propyl betaine (BS-12), dodecyl dimethyl amine oxide (OA-12), cocamidopropyl dimethyl betaine (CAB-35), cocamidopropyl hydroxysulfonic acid betaine (CHS-35), coconut imidazoline (CAMA-30), fatty alcohol (9EO) (AEC-9), sodium lauryl sulfate (SDS), secondary alkyl sulfate (Teep01), fatty alcohol sulfate (FAS), fatty alcohol sulfate monoethanolamine salt (ASEA), fatty alcohol polyoxyethylene ether sulfate (AES), α-sulfated fatty acid disodium salt (DSFA), dodecyl phosphate (MAP-85), dodecyl phosphate potassium salt (MAP-K), dodecyl phosphate triethanolamine (MAP-A), sodium tetrapropylene benzene sulfonate (ABS), sodium alkyl benzene sulfonate (LAS), sodium dodecyl benzene sulfonate (SDBS), primary alkyl sulfonate (AS), secondary alkyl sulfonate (SAS), α-olefin sulfonate (AOS), α-sulfonated fatty acid methyl ester (MES), fatty acid sulfonalkyl ester (1gepon A), fatty acid sulfonamide (Igepon T), sodium dioctyl sulfosuccinate (AerosolOT), alkyl glycerol ether sulfonate (AGS), sodium dibutyl naphthalene sulfonate (penetrant BX), sodium p-methoxy fatty amide benzene sulfonate (cleaner LS), sodium methylene bis naphthalene sulfonate (NNO), fatty acid methyl ester sulfonate (MES), sodium fatty acid (SOAP), Lamepon A, sodium carboxymethyl cellulose (SCMC), sodium acyl sarcosine (DX107), one or more thereof, the surfactant concentration is 0.1% (w / v) to 10% (w / v). .

[0048] The first alcohol in step (1) is one or both of ethanol and propanol, and the second alcohol is propanol; the third alcohol in step (2) is propanol; the hydrothermal crystallization temperature in step (1) is 100-140°C and the time is 1-4 days; the gelation temperature in step (1) or (2) is 45-55°C and the time is 1-12 days; the drying temperature is 90°C-120°C and the time is 10-24 hours; the calcination temperature in step (3) is 350°C-800°C and the time is more than 2 hours.

[0049] The acidic metal oxide precursor in the inner core precursor of step (1) is one or more of tungsten chloride, zinc chloride, phosphotungstic acid, niobium chloride, zirconium oxychloride, zirconium chloride, cerium nitrate, niobium oxalate, aluminum chloride, hafnium chloride, tin chloride, tetraethyl silicate, 1,2-bis(triethoxysilyl)ethane, tetrabutyl titanate, sodium silicate, and aluminum silicate; the inner shell precursor in step (2) is a co-precipitate of at least two of zinc salt, cerium salt, copper salt, molybdenum salt, tetraethyl silicate, or / and 1,2-bis(triethoxysilyl)ethane, zirconium salt, iron salt, and cobalt salt; and the solid base precursor is a co-precipitate of one or two of magnesium salt or calcium salt, or a complex thereof with tetraethyl silicate or / and 1,2-bis(triethoxysilyl)ethane.

[0050] The multilayer core-shell structure catalyst of the present invention is used to catalyze the biomass raw materials to prepare RJ-4 or JP-10 oxygen-free precursor in one step, such as Figure 2 The biomass raw material is selected from 2,5-hexanedione and / or furfuryl alcohol; the oxygen-free RJ-4 precursor is synthesized from 2,5-hexanedione; and the oxygen-free JP-10 precursor is synthesized from furfuryl alcohol.

[0051] Catalyst Preparation Example 1: Preparation of a multilayer core-shell structure catalyst, the steps are as follows:

[0052] (1) 1 g of carbon spheres and 1 g of surfactant P123 were added to 10 g of anhydrous 1-propanol and mixed at 2000 rpm, and then 3 mmol of metal niobium chloride and 3 mmol of tungsten chloride were added and continued to be stirred and mixed; then 30 mmol of water was added and continued to be stirred and mixed to obtain a sol; the obtained sol was gelled in a culture dish at 50° C. for 2 days, and then dried in a dryer at 100° C. for 12 h to obtain a solid powder S1;

[0053] (2) The solid powder S1 and 1 g of P-123 were added to 10 g of anhydrous 1-propanol, stirred vigorously, and 4 mmol of (NH4)6Mo7O 24 4H2O and 2mmol zinc oxalate were stirred evenly; 30mmol water was added to the solution to adjust the pH value to 10-11 and further stirred to obtain a sol; the obtained sol was gelled in a petri dish at 50°C for 2 days; then the aged gel sample was dried in a dryer at 100°C for 12h to obtain catalyst S2;

[0054] (3) S2 and 2.0 g CTAB were dissolved in a mixed solution of 350 mL water, 35 mL ethanol, and 20 mL concentrated ammonia (25 wt%), and heated to 50°C; then, 3.0 g magnesium chloride and 7.5 mL ethanol were added to the mixed solution under stirring at 1100 rpm; gelation was carried out in a petri dish at 50°C for 2 days, and the white reaction product was collected by centrifugation, washed with water 3 times, dried in a drying oven at 100°C for 12 h, and then calcined in a muffle furnace at 500°C for 5 h to obtain the multilayer core-shell structure catalyst S3 shown, namely NbWOx@ZnMoO x @MgO.

[0055] Catalyst preparation example 2: Preparation of multi-layer core-shell structure catalyst.

[0056] (1) Dissolve 1.8g CTAB in 70mL water, heat and stir to dissolve it into a transparent solution, and let it stand for 10 minutes. Add 1g carbon spheres, 0.2g aluminum nitrate, and 5.7g sodium silicate in sequence while stirring continuously to mix them evenly, and continue stirring for 2 hours; adjust the pH of the solution to about 10.50 with 2mol / L sulfuric acid solution, continue stirring for 0.5h to form a uniform gel phase, and adjust the pH to about 10.50 again; then transfer it into a stainless steel reactor with a polytetrafluoroethylene liner and hydrothermally crystallize it at 120°C for 72h; the product after hydrothermal crystallization is filtered, washed with water, and dried at 100°C for 12h to obtain solid powder S1;

[0057] Step (2) and step (3) are the same as in Example 1. Al-MCM-41@ZnMoO x @MgO.

[0058] Other catalysts WO3@SiMoO x @MgO-CaO、Al-SBA-15@FeMoO x @SiO2-MgO、Al-SBA-16@ZnCoO X @SiO2-CaO、Ti-MCM-41@ZrCoO x @SiO2-MgO-CaO、HY@SiCoO x @SiO2-MgO-CaO, Hβ@FeCoO x @SiO2-CaO、HZSM-5@CeMoO x @SiO2-MgO、Al2O3@CeCoO X @MgO-CaO、Nb2O5@SiMoO x @CaO、SiO2-Al2O3@CuCoO X @MgO, CsTPA@CuMoOX @MgO、HfTPA / MCM-41@ZnCuMoO X @CaO、SiO2-Nb2O5@ZrMoO x @MgO-CaO、MOF-808-2.5SO4@SiMoO x @SiO2-MgO, HfTPA@CuFeMoO x @SiO2-CaO, SnTPA@ZnCoO X @SiO2-MgO-CaO, ZrTPA@ZrCoO x @SiO2-MgO-CaO, SO4 2- / ZrO2@SiCoO x @SiO2-CaO, ITQ@ZnFeCoO x @SiO2-MgO, KIT-6@CeMoO x @MgO-CaO、Mordenite@CeCoO X @CaO、MMT-K10@SiMoO x @MgO、HPW / MCM-41@CuMoO X The preparation method of @MgO etc. is the same or similar to that of Example 1 or Example 2.

[0059] Preparation of JP-10 Precursor Example 1-25: Multilayer core-shell structure catalyst is used to catalytically prepare JP-10 precursor.

[0060] A fixed bed reactor was used. Before the reaction started, 2.5 g of catalyst S3 was loaded. The multilayer core-shell structure catalyst was activated with hydrogen at 400°C for 2 h. Then, furfuryl alcohol and hydrogen were introduced into the reactor as reactants and carrier gases using an HPLC pump. The conditions and results are shown in Table 1.

[0061] Table 1 Preparation of JP-10 fuel precursor from furfuryl alcohol

[0062]

[0063] As can be seen from Table 1, biomass furfuryl alcohol can generate JP-10 precursor under the catalytic action of the multi-layer core-shell structure catalyst of the present invention, within the temperature range of 180°C to 450°C, the hydrogen pressure of 0.1 to 0.5 MPa, WHSV=0.10 to 0.45 g / g / h, and the H2 / furfuryl alcohol molar ratio controlled at 30 to 50; the raw material conversion rate is 100%, and the yield of the fuel precursor is not less than 70%.

[0064] Preparation of RJ-4 Precursor Example 26-50: Multilayer core-shell structure catalyst is used to prepare RJ-4 precursor.

[0065] The same preparation method as Example 1-25 for JP-10 precursor was used, except that the reactant was replaced with 2,5-hexanedione. The conditions and results are shown in Table 2.

[0066] Table 2 Preparation of fuel RJ-4 precursor from 2,5-hexanedione

[0067]

[0068] As can be seen from Table 2, under the catalytic action of the multi-layer core-shell structure catalyst of the present invention, in the temperature range of 180°C to 450°C, the hydrogen pressure is 0.1 to 0.5 MPa, WHSV=0.10 to 0.45 g / g / h, the H2 / 2,5-hexanedione molar ratio is controlled at 30 to 50, the raw material conversion rate of the RJ-4 precursor is 100%, and the yield of the fuel precursor is not less than 75%.

[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A multilayer core-shell structure catalyst, characterized in that: It includes: Acidic spherical shell core and multi-layer spherical shell shell.

2. The multilayer core-shell structure catalyst according to claim 1, characterized in that: The shell wall of the inner core has holes with a pore diameter of 0.5nm-30nm, the average diameter of the hollow cavity in the shell wall of the inner core is 5.0-200nm, and the thickness of the shell wall of the inner core is 5-100nm; the acidic spherical shell inner core is one of acidic metal oxides, molecular sieves, a composite of acidic metal oxides and molecular sieves, or a composite of acidic metal oxides and silicon dioxide.

3. The multilayer core-shell structure catalyst according to claim 2, characterized in that: Acidic metal oxides are NbWOx, WO3, Al2O3, Nb2O5, SiO2-Al2O3, SiO2-Nb2O5, MOF-808-2.5SO4, HfTPA, SnTPA, ZrTPA, SO4 2- / ZrO2, MMT-K10, or HPW; the molecular sieve is one or more of Al-MCM-41, Al-SBA-15, Al-SBA-16, Ti-MCM-41, HY, Hβ, HZSM-5, MCM-41, ITQ, KIT-6, or Mordenite.

4. The multilayer core-shell structure catalyst according to claim 1, characterized in that: The outer shell is double-layered, both shell walls have holes with a pore size of 0.5nm-100nm; the inner shell is a metal oxide composite layer with a thickness of 5-100nm; the outer shell is a solid base layer with a thickness of 10-200nm.

5. The multilayer core-shell structure catalyst according to claim 4, characterized in that: The metal oxide composite is ZnMoO X 、ZrMoO x 、SiMoO x 、FeMoO x 、ZnCoO X 、ZrCoO x 、SiCoO x 、FeCoO x 、CeMoO x 、CeCoO X 、SiMoO x 、CuCoO X 、CuMoO X 、ZnCuMoO X 、CuFeMoO x 、ZnFeCoO x One or more of the following; the solid base is CaO and / or MgO, or a complex of CaO and / or MgO and silicon dioxide.

6. The method for preparing the multilayer core-shell structure catalyst according to any one of claims 1 to 5, characterized in that: The steps include: (1) adding a certain amount of the first surfactant to water or a mixed solution of water and the first alcohol to dissolve and adding carbon spheres, adding the core precursor and continuing to mix for a period of time; adjusting the pH value to 10-11 and maintaining it, and then hydrothermally crystallizing; filtering, washing with water, and drying to obtain a solid powder S1; or, The carbon spheres and the second surfactant are added to the second alcohol and stirred to mix evenly, and then the core precursor is added and stirred to mix evenly; then water is added and stirred to mix to obtain a sol; the obtained sol is gelled at a certain temperature for a period of time and then heated and dried for a period of time to obtain a solid powder S1; (2) adding the solid powder S1 obtained in step (1) and the third surfactant to the third alcohol and mixing them evenly, and then adding the inner shell layer precursor and mixing them evenly; adding water and continuing to stir and adjusting the pH value of the solution to form a sol; and gelling the obtained sol at a certain temperature for a period of time; The gelled sample is then dried for a period of time to obtain catalyst precursor S2; (3) dissolving a certain amount of S2 and a fourth surfactant in an aqueous solution of ammonia in ethanol, and then adding a solid base precursor and ethanol to mix; separating the solid after gelation for a period of time, washing and drying, and then calcining for a period of time to obtain the multilayer core-shell structure catalyst S3.

7. The preparation method according to claim 6, characterized in that: The first surfactant, the second surfactant, the third surfactant and the fourth surfactant are each independently a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, a polyethylene glycol-polypropylene glycol-polyethylene glycol triblock copolymer, polyvinyl pyrrolidone, polyethylene oxide, oleylamine polyoxyethylene ether, polyoxyacrylamide, sorbitan monooleate polyoxyethylene ether, sorbitan monooleate, dodecylphenol polyoxyethylene ether, isooctylphenyl polyoxyethylene ether, octadecyl alcohol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, polyethylene glycol octylphenyl ether, coconut Oil fatty acid monoethanolamide, C12-14 alkyl glucoside, fatty alcohol polyoxyethylene 3 / 7 / 9 ether, nonylphenol polyoxyethylene ether, hydroxyl synthetic alcohol polyoxyethylene ether, hydroxyl synthetic alcohol polyoxyethylene ether, triethanolamine monostearate, dodecyltrimethylammonium chloride, dodecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, tetrabutylammonium hydroxide, tetrapropylammonium hydroxide, dodecyldimethylbenzylammonium chloride, dodecyldimethylbenzylammonium bromide, docosyltrimethylammonium methyl sulfate, alkyl pyridine, alkyl morpholine, alkyl Imidazolin, alkyl aziridine, lauryl amide propyl amine oxide, cocamidopropyl betaine, dodecyl propyl betaine, dodecyl dimethyl amine oxide, cocamidopropyl dimethyl betaine, cocamidopropyl hydroxysulfonic acid betaine, coconut imidazoline, fatty alcohol (9EO), sodium lauryl sulfate, secondary alkyl sulfate, fatty alcohol sulfate, fatty alcohol sulfate ester monoethanolamine salt, fatty alcohol polyoxyethylene ether sulfate ester salt, α-sulfated fatty acid disodium salt, dodecyl phosphate, dodecyl phosphate potassium salt, dodecyl phosphite ester triethanolamine, tetrapropylene benzene One or more of sodium sulfonate, sodium alkylbenzene sulfonate, sodium dodecylbenzene sulfonate, primary alkyl sulfonate, secondary alkyl sulfonate, α-olefin sulfonate, α-sulfo fatty acid methyl ester, fatty acid sulfoalkyl ester, fatty acid sulfoalkylamide, sodium diisooctyl succinate sulfonate, alkyl glyceryl ether sulfonate, sodium dibutylnaphthalene sulfonate, sodium p-methoxy fatty amide benzene sulfonate, sodium methylene bisnaphthalene sulfonate, fatty acid methyl ester sulfonate, sodium fatty acid, remibond A, sodium carboxymethyl cellulose, and sodium acyl sarcosinate, and the surfactant concentration is 0.1% (w / v) to 10% (w / v).

8. The preparation method according to claim 6, characterized in that: The first alcohol in step (1) is one or both of ethanol and propanol, and the second alcohol is propanol; the third alcohol in step (2) is propanol; the hydrothermal crystallization temperature in step (1) is 100-140° C., and the time is 1-4 days; the gelation temperature in step (1) or (2) is 45-55° C., and the time is 1-12 days; the drying temperature is 90° C.-120° C., and the time is 10-24 hours; the calcination temperature in step (3) is 350° C.-800° C., and the time is more than 2 hours.

9. The preparation method according to claim 6, characterized in that: In step (1), the acidic metal oxide precursor in the inner core precursor is one or more of tungsten chloride, zinc chloride, phosphotungstic acid, niobium chloride, zirconium oxychloride, zirconium chloride, cerium nitrate, niobium oxalate, aluminum chloride, hafnium chloride, tin chloride, tetraethyl silicate, 1,2-bis(triethoxysilyl)ethane, tetrabutyl titanate, sodium silicate, and aluminum silicate; in step (2), the inner shell precursor is a co-precipitate of at least two of zinc salt, cerium salt, copper salt, molybdenum salt, tetraethyl silicate, or / and 1,2-bis(triethoxysilyl)ethane, zirconium salt, iron salt, and cobalt salt; and the solid base precursor is a co-precipitate of one or two of magnesium salt or calcium salt, or a complex thereof with tetraethyl silicate or / and 1,2-bis(triethoxysilyl)ethane.

10. Use of the multilayer core-shell structure catalyst according to any one of claims 1 to 5 for catalyzing the one-step preparation of RJ-4 or JP-10 oxygen-free precursor from biomass raw materials.

Citation Information

Patent Citations

  • Synthesis method of core-shell type double-active-site catalyst and method for preparing cyclohexanone by catalyzing phenol with core-shell type double-active-site catalyst

    CN111514888A

  • Application of hierarchical pore molecular sieve in preparation process of cyclopentadiene and JP-10 aviation fuel

    CN113045392A

  • Sulfur-dioxide-poisoning-resistant catalyst for treating nitrogen oxide-containing waste gas, waste gas treating agent and application of sulfur-dioxide-poisoning-resistant catalyst and waste gas treating agent

    CN114042449A

  • Hollow metal oxide coated TiO2 core-shell structure catalyst as well as preparation method and application thereof

    CN116328757A

  • Metal core nanocapsules

    US20100055170A1