Method for producing punctiform slightly-dark DM surface stainless steel band by using laser texturing machine
The DM surface work roll and multi-pass rolling process were processed by laser hairening machine, and the problem of difficult drag marks and gloss of stainless steel strips under a 40X microscope is solved, and the fine and glossy of spots is achieved. The surface improves production stability and input-output rate.
Patent Information
- Application Number
- CN202411302653.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-15
AI Technical Summary
The existing special surface processing method of stainless steel strips cannot completely eliminate drag marks under a 40X microscope, and the randomness of shot blasting treatment makes it difficult to accurately control the gloss and cannot meet customer needs.
The laser hairening machine is used to laser hairening the DM surface work roller, combined with multiple rolling, solution treatment and pulling processes to ensure the gloss and roughness of the steel strip surface is 200-300GU, and the filamentous surface is eliminated. Improve production stability and control.
It realizes a dot-shaped slightly dim DM surface stainless steel strip with no dragging, delicate surface and gloss under a 40X microscope, which improves production stability and input-output rate and meets customer needs.
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing a stainless steel strip, in particular to a method for producing a stainless steel strip with a dot-shaped slightly dim DM surface by using a laser texturing machine. Background Art
[0002] The stainless steel belt with a dot-shaped and slightly dim DM surface is a stainless steel belt that has a dot-shaped surface and is visually slightly dim under a 40X light source microscope. This is a stainless steel belt with a special surface shape.
[0003] At present, there are two types of stainless steel belts with special surface shapes produced in the industry, one is the ordinary stainless steel belt with a wire-shaped grinding pattern surface, and the other is the conventional stainless steel belt with a low gloss on the dot-shaped surface. For the ordinary stainless steel belt with a wire-shaped grinding pattern surface, the processing process generally finely grinds the working roller to control the surface roughness of the working roller to Ra0.3-0.4um, and the gloss is relatively high, basically exceeding 350GU, but the original grinding marks always exist, especially under a 40X microscope, there are obvious signs of dragging, which can never be overcome. For the conventional stainless steel belt with a low gloss on the dot-shaped surface, the dot-shaped surface is produced by sandblasting or shot blasting. The surface roughness Ra of the working roller treated by sandblasting or shot blasting is basically above 0.6um, and the gloss is less than 200GU, which cannot meet customer needs. Although the surface roughness Ra of the working roller is basically 0.3-0.45um and the gloss is 300-400GU when fine shot blasting is used, which can meet customer needs, it cannot be accurately controlled due to the large randomness of the shot blasting process. Summary of the invention
[0004] The purpose of the present invention is to solve the shortcomings of the prior art and provide a method for producing a stainless steel belt with a dot-shaped slightly dull DM surface by using a laser texturing machine. The stainless steel belt with a dot-shaped slightly dull DM surface produced by the method is not only free of filaments when visually observed, and dot-shaped without drag under a 40X microscope, but also has a fine surface and a glossiness of 200-300GU in the Y-axis direction, and also has a relatively high input-output ratio, good stability, and an easy-to-control production process.
[0005] To solve the above problems, the following technical solutions are adopted: The method of producing a stainless steel strip with a dot-shaped slightly dim DM surface by using a laser texturing machine of the present invention is characterized in that it comprises the following steps: The first step is material selection. Select Zhangpu's SUS304 cold-rolled stainless steel billet with a thickness of more than 0.5 mm for use.
[0006] The second step is one-time rolling. The raw material thickness selected according to the finished product performance requirements is rolled in 3-4 passes. The last pass is rolled using a rough shot blasting roller Ra0.6-1.0um working roller, and the semi-finished product thickness is directly rolled to 0.22+ / -0.01mm. At this time, the surface glossiness of the steel strip is low, only 100-160GU, and it appears dot-shaped under a 40X microscope with a light source.
[0007] The third step is cleaning. The rolled semi-finished product is removed from the surface of the steel strip at a speed of 80-100m / min on the degreasing cleaning unit to prepare for the solution treatment.
[0008] The fourth step is solution treatment. The semi-finished steel strip that has been cleaned once passes through a bright annealing furnace at a temperature of 1100-1140°C at a speed of 9-13m / min.
[0009] The fifth step is secondary rolling. It is divided into two passes of rolling, and all DM surface working rolls are used for rolling. The DM surface working rolls are divided into 2 gears, Ra0.3-0.4um, Ra0.4-0.5um. The surface after rolling is a dotted surface with a roughness of Ra0.3-0.4um and Ra0.4-0.5um. The Y-axis glossiness reaches 250-350GU. The performance of the finished product is adjusted by the thickness tolerance to ensure the performance of the finished steel strip. Among them, the processing technology of the DM surface working roll is as follows: first, the surface of the working roll is ground with fine particles to obtain a Ra0.1-0.2um fine surface, so that the surface glossiness of the working roll reaches 300-400GU, and then the laser texturing machine is used to perform laser texturing on the ground working roll to ensure the surface roughness Ra0.3-0.4um, Ra0.4-0.5um, and the glossiness 300-400GU.
[0010] The sixth step is cleaning. The finished steel strip is removed from the surface of the steel strip at a speed of 80-100m / min on the degreasing cleaning unit to prepare for straightening.
[0011] The seventh step is straightening. The cleaned finished steel strip is straightened on the straightening machine, and the surface gloss of the steel strip is guaranteed to be 200-300GU by small pressure reduction and small elongation control. This is the key step to control the surface gloss of the steel strip.
[0012] Step 8: Cut and pack. Cut and pack according to customer requirements and put into storage.
[0013] In the fourth step of solution treatment, in order to ensure the rolling hardness and surface gloss, the solution treatment is carried out under the protection of pure hydrogen or ammonia decomposition gas, and the dew point of the protective gas is strictly controlled below -70°C, in order to ensure that the surface of the steel strip does not turn blue during the solution treatment process. The heating section of the bright annealing furnace is 9 meters long.
[0014] The tensile straightening machine used in the seventh step of the straightening process is a 23-roller tensile straightening machine produced by Unger Company of Germany.
[0015] The above solution has the following advantages: The method of the present invention for producing stainless steel strips with dot-shaped and slightly dull DM surfaces by using a laser texturing machine is as follows: material selection → primary rolling → cleaning → solution treatment → secondary rolling → cleaning → straightening, and then a stainless steel strip with dot-shaped and slightly dull DM surfaces can be obtained. Since the DM surface working rollers used in the secondary rolling are laser texturing treated after grinding, the stainless steel strips with dot-shaped and slightly dull DM surfaces obtained through the entire process are free of filaments when visually observed, and the surface is dot-shaped and drag-free under a 40X microscope. The surface is fine and the glossiness is 200-300GU in the Y-axis direction, which can fully meet customer needs. Moreover, the production using laser texturing treated DM surface working rollers does not have the problem of randomness, has good stability, a relatively high input-output ratio, and the production process is easy to control. DETAILED DESCRIPTION
[0016] The present invention is further described in detail below with reference to the embodiments. Embodiment 1
[0017] The method of producing a stainless steel strip with a dot-shaped slightly dim DM surface by using a laser texturing machine in this embodiment comprises the following steps: The first step is material selection. Select Zhangpu's SUS304 cold-rolled stainless steel billet with a thickness of more than 0.5 mm for use.
[0018] The second step is one-time rolling. The raw material thickness selected according to the finished product performance requirements is rolled in three passes. The last pass is rolled using a rough shot blasting roller Ra0.6-1.0um working roller, and is directly rolled to a semi-finished product thickness of 0.22+ / -0.01mm. At this time, the surface glossiness of the steel strip is relatively low, only 100-160GU, and it appears dot-shaped under a 40X microscope with a light source.
[0019] The third step is cleaning. The rolled semi-finished products are removed from the surface of the steel strip at a speed of 80m / min on the degreasing and cleaning unit to prepare for the solution treatment.
[0020] The fourth step is solution treatment. The semi-finished steel strip that has been cleaned once is passed through a bright annealing furnace at a temperature of 1100-1140℃ at a speed of 9m / min. In order to ensure the rolling hardness and surface glossiness, the solution treatment is carried out under the protection of pure hydrogen or ammonia decomposition gas. The dew point of the protective gas is strictly controlled below -70℃ to ensure that the surface of the steel strip does not turn blue during the solution treatment process. The heating section length of the bright annealing furnace is 9 meters.
[0021] The fifth step is secondary rolling. It is divided into two passes of rolling, and all DM surface working rolls are used for rolling. The DM surface working rolls are divided into 2 gears, Ra0.3-0.4um, Ra0.4-0.5um. The surface after rolling is a dotted surface with a roughness of Ra0.3-0.4um and Ra0.4-0.5um. The Y-axis glossiness reaches 250-350GU. The performance of the finished product is adjusted by the thickness tolerance to ensure the performance of the finished steel strip. Among them, the processing technology of the DM surface working roll is as follows: first, the surface of the working roll is ground with fine particles to obtain a Ra0.1-0.2um fine surface, so that the surface glossiness of the working roll reaches 300-400GU, and then the laser texturing machine is used to perform laser texturing on the ground working roll to ensure the surface roughness Ra0.3-0.4um, Ra0.4-0.5um, and the glossiness 300-400GU.
[0022] The sixth step is cleaning. The finished steel strip is removed from the surface of the steel strip at a speed of 80m / min on the degreasing and cleaning unit to prepare for straightening.
[0023] The seventh step is straightening. The cleaned finished steel strip is straightened on a straightening machine, and a small pressure reduction and small elongation control are used to ensure that the surface gloss of the steel strip is 200-300GU. This is a key step in controlling the surface gloss of the steel strip. The straightening machine is a 23-roll straightening machine produced by Unger, Germany.
[0024] Step 8: Cut and pack. Cut and pack according to customer requirements and put into storage. Embodiment 2
[0025] The method of producing a stainless steel strip with a dot-shaped slightly dim DM surface by using a laser texturing machine in this embodiment comprises the following steps: The first step is material selection. Select Zhangpu's SUS304 cold-rolled stainless steel billet with a thickness of more than 0.5 mm for use.
[0026] The second step is one-time rolling. The raw material thickness selected according to the finished product performance requirements is rolled in 4 passes. The last pass is rolled using a rough shot blasting roller Ra0.6-1.0um working roller, and is directly rolled to a semi-finished product thickness of 0.22+ / -0.01mm. At this time, the surface glossiness of the steel strip is relatively low, only 100-160GU, and it appears dot-shaped under a 40X microscope with a light source.
[0027] The third step is cleaning. The rolled semi-finished products are removed from the surface of the steel strip at a speed of 90m / min on the degreasing and cleaning unit to prepare for the solution treatment.
[0028] The fourth step is solution treatment. The semi-finished steel strip that has been cleaned once is passed through a bright annealing furnace at a temperature of 1100-1140℃ at a speed of 11m / min. In order to ensure the rolling hardness and surface glossiness, the solution treatment is carried out under the protection of pure hydrogen or ammonia decomposition gas. The dew point of the protective gas is strictly controlled below -70℃ to ensure that the surface of the steel strip does not turn blue during the solution treatment process. The heating section length of the bright annealing furnace is 9 meters.
[0029] The fifth step is secondary rolling. It is divided into two passes of rolling, and all DM surface working rolls are used for rolling. The DM surface working rolls are divided into 2 gears, Ra0.3-0.4um, Ra0.4-0.5um. The surface after rolling is a dotted surface with a roughness of Ra0.3-0.4um and Ra0.4-0.5um. The Y-axis glossiness reaches 250-350GU. The performance of the finished product is adjusted by the thickness tolerance to ensure the performance of the finished steel strip. Among them, the processing technology of the DM surface working roll is as follows: first, the surface of the working roll is ground with fine particles to obtain a Ra0.1-0.2um fine surface, so that the surface glossiness of the working roll reaches 300-400GU, and then the laser texturing machine is used to perform laser texturing on the ground working roll to ensure the surface roughness Ra0.3-0.4um, Ra0.4-0.5um, and the glossiness 300-400GU.
[0030] The sixth step is cleaning. The finished steel strip is removed from the surface of the steel strip at a speed of 90m / min on the degreasing cleaning unit to prepare for straightening.
[0031] The seventh step is straightening. The cleaned finished steel strip is straightened on a straightening machine, and a small pressure reduction and small elongation control are used to ensure that the surface gloss of the steel strip is 200-300GU. This is a key step in controlling the surface gloss of the steel strip. The straightening machine is a 23-roll straightening machine produced by Unger, Germany.
[0032] Step 8: Cut and pack. Cut and pack according to customer requirements and put into storage. Embodiment 3
[0033] The method of producing a stainless steel strip with a dot-shaped slightly dim DM surface by using a laser texturing machine in this embodiment comprises the following steps: The first step is material selection. Select Zhangpu's SUS304 cold-rolled stainless steel billet with a thickness of more than 0.5 mm for use.
[0034] The second step is one-time rolling. The raw material thickness selected according to the finished product performance requirements is rolled in 4 passes. The last pass is rolled using a rough shot blasting roller Ra0.6-1.0um working roller, and is directly rolled to a semi-finished product thickness of 0.22+ / -0.01mm. At this time, the surface glossiness of the steel strip is relatively low, only 100-160GU, and it appears dot-shaped under a 40X microscope with a light source.
[0035] The third step is cleaning. The rolled semi-finished product is removed from the surface of the steel strip at a speed of 100m / min on the degreasing cleaning unit to prepare for the solution treatment.
[0036] The fourth step is solution treatment. The semi-finished steel strip that has been cleaned once is passed through a bright annealing furnace at a temperature of 1100-1140°C at a speed of 13m / min. In order to ensure the rolling hardness and surface glossiness, the solution treatment is carried out under the protection of pure hydrogen or ammonia decomposition gas. The dew point of the protective gas is strictly controlled below -70°C to ensure that the surface of the steel strip does not turn blue during the solution treatment process. The heating section length of the bright annealing furnace is 9 meters.
[0037] The fifth step is secondary rolling. It is divided into two passes of rolling, and all DM surface working rolls are used for rolling. The DM surface working rolls are divided into 2 gears, Ra0.3-0.4um, Ra0.4-0.5um. The surface after rolling is a dotted surface with a roughness of Ra0.3-0.4um and Ra0.4-0.5um. The Y-axis glossiness reaches 250-350GU. The performance of the finished product is adjusted by the thickness tolerance to ensure the performance of the finished steel strip. Among them, the processing technology of the DM surface working roll is as follows: first, the surface of the working roll is ground with fine particles to obtain a Ra0.1-0.2um fine surface, so that the surface glossiness of the working roll reaches 300-400GU, and then the laser texturing machine is used to perform laser texturing on the ground working roll to ensure the surface roughness Ra0.3-0.4um, Ra0.4-0.5um, and the glossiness 300-400GU.
[0038] The sixth step is cleaning. The finished steel strip is removed from the surface of the steel strip at a speed of 100m / min on the degreasing cleaning unit to prepare for straightening.
[0039] The seventh step is straightening. The cleaned finished steel strip is straightened on a straightening machine, and a small pressure reduction and small elongation control are used to ensure that the surface gloss of the steel strip is 200-300GU. This is a key step in controlling the surface gloss of the steel strip. The straightening machine is a 23-roll straightening machine produced by Unger, Germany.
[0040] Step 8: Cut and pack. Cut and pack according to customer requirements and put into storage.
[0041] Since the method of producing a dot-shaped slightly dull DM surface stainless steel strip using a laser texturing machine of the present invention, the DM surface working roller used in the secondary rolling is laser texturing treated by a laser texturing machine after grinding, the dot-shaped slightly dull DM surface stainless steel strip obtained through the entire process has no filaments when visually observed, and the surface is dot-shaped without drag under a 40X microscope, and the surface is fine and the glossiness is 200-300GU in the Y-axis direction, which can fully meet customer needs. Moreover, the production using the DM surface working roller treated with laser texturing does not have the problem of randomness, has good stability, relatively high input-output ratio, and the production process is easy to control.
Claims
1. A method for producing a stainless steel strip with a dot-shaped slightly dim DM surface using a laser texturing machine, characterized in that The following steps are involved: The first step is material selection Select Zhangpu's SUS304 cold-rolled stainless steel billet with a thickness of more than 0.5 mm for use; The second step is one-time rolling The raw material thickness selected according to the finished product performance requirements is rolled in 3-4 passes. The last pass is rolled using a rough shot blasting roller Ra0.6-1.0um working roller, and is directly rolled to a semi-finished product thickness of 0.22+ / -0.01mm. At this time, the surface glossiness of the steel strip is low, only 100-160GU, and it appears dot-shaped under a 40X microscope with a light source; Step 3: Cleaning The rolled semi-finished products are removed from the surface of the steel strip at a speed of 80-100m / min on the degreasing and cleaning unit to prepare for the solution treatment; Step 4: Solution treatment The semi-finished steel strip after one cleaning is passed through a bright annealing furnace at a temperature of 1100-1140°C at a speed of 9-13m / min; Step 5: Secondary rolling The rolling process is divided into two passes, and all of them are rolled with DM surface working rolls produced by laser texturing machines. The DM surface working rolls are divided into two gears, Ra0.3-0.4um and Ra0.4-0.5um. The surface after rolling is a dotted surface with a roughness of Ra0.3-0.4um and Ra0.4-0.5um. The Y-axis glossiness reaches 250-350GU. The performance of the finished product is adjusted by the thickness tolerance to ensure the performance of the finished steel strip; Among them, the processing technology of DM surface working roll is as follows: First, the working roller surface is ground with fine particles to obtain a Ra0.1-0.2um fine surface, so that the surface glossiness of the working roller reaches 300-400GU. Then, the ground working roller is laser-textured by a laser texturing machine to ensure the surface roughness of Ra0.3-0.4um, Ra0.4-0.5um, and the glossiness of 300-400GU. Step 6. Cleaning The finished steel strip is removed from the surface of the steel strip at a speed of 80-100m / min on the degreasing and cleaning unit to prepare for straightening. Step 7: Straighten The cleaned finished steel strip is corrected on the tensioning and leveling machine, and the surface gloss of the steel strip is guaranteed to be 200-300GU by small pressure reduction and small elongation control. This is the key step to control the surface gloss of the steel strip. Step 8: Cutting and packaging Cut, pack and store according to customer requirements.
2. The method for producing a stainless steel strip with a dot-shaped slightly dim DM surface by using a laser texturing machine as claimed in claim 1, characterized in that In the fourth step of solution treatment, in order to ensure the rolling hardness and surface gloss, solution treatment is carried out under the protection of pure hydrogen or ammonia decomposition gas. The dew point of the protective gas is strictly controlled below -70°C. The purpose is to ensure that the surface of the steel strip does not turn blue during the solution treatment process.
3. The method for producing a stainless steel strip with a dot-shaped slightly dim DM surface by using a laser texturing machine as claimed in claim 1, characterized in that In the fourth step of solution treatment, the heating section length of the bright annealing furnace is 9 meters.
4. The method for producing a stainless steel strip with a dot-shaped slightly dim DM surface by using a laser texturing machine as claimed in claim 1, characterized in that The tensile straightening machine used in the seventh step of the straightening process is a 23-roller tensile straightening machine produced by Unger Company of Germany.
Citation Information
Patent Citations
Method for producing textured surface accurate stainless steel band
CN101244427A
Cold-rolling production method for simulated laser roughened face stainless steel band
CN106623418A
Production method of stainless steel band with dotted slightly-dark DM surface
CN110788140A
Production method of point-like matte dull DH surface stainless steel band
CN115672992A
Method for producing point-shaped bright BR surface stainless steel band by using laser texturing machine
CN118389810A
Cited By
Processing method of stainless steel strip steel with textured surface
CN119140602A