Saddle-shaped sheet metal part forming device and method

By using a mold, drawing rib and hydraulic press in the saddle sheet metal forming device for multiple hydraulic forming of rubber bladders, combined with rubber blocks and lubricant treatment, the problem of wrinkles and cracks during saddle forming process is solved. Improve the surface quality of parts and product qualification rate, achieving cost reduction and efficiency improvement.

CN118950809APending Publication Date: 2024-11-15CHANGHE AIRCRAFT INDUSTRIES CORPORATION

Patent Information

Application Number
CN202411269454.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The saddle-shaped sheet metal parts of the aircraft are thin and complex in appearance. The existing hammer-assisted manual forming process is prone to wrinkles and cracks.

Method used

A saddle-shaped sheet metal forming device is designed, including molds, drawing ribs, breathable holes, exhaust slots and hydraulic presses, which are hydraulically formed by multiple rubber bladders and use rubber blocks and transparent films or lubrication during the forming process. The agent improves the fluidity of the material and performs a flat wrinkle treatment to solve the problem of local wrinkles.

Benefits of technology

It effectively solves the problems of wrinkles and cracks during saddle forming, improves the surface quality of parts and product qualification rate, and achieves cost reduction and efficiency improvement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950809A_ABST
    Figure CN118950809A_ABST
Patent Text Reader

Abstract

The invention provides a saddle-shaped sheet metal part forming device which comprises a die body, a first mold body, a second mold body, a third mold body, a fourth mold body, a fifth mold body and a sixth mold body, and the first mold body is attached to the outer mold surface of a saddle-shaped sheet metal part; the draw bead is arranged on the die body, and the draw bead is used for slowing down the speed of a plate entering the first molded surface; the air holes are formed in the bottom filling surface; the exhaust groove is formed in the back surface of the die body, and the exhaust groove is communicated with the air hole; the reference hole is formed in the surface of the die body; meanwhile, the invention further provides a saddle-shaped sheet metal part forming method. The problem that wrinkles and cracks are generated in the original forming process is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of sheet metal technology, and in particular, relates to a saddle-shaped sheet metal forming device and method. Background Art

[0002] Aircraft saddle-shaped sheet metal parts are thin (δ0.8), complex in shape, and difficult to form. The existing forming technology uses drop hammer assisted manual forming. During the drop hammer forming process, too much material is collected and wrinkles are easily formed. Too little material is collected and the parts are prone to become too thin and cracks are generated.

[0003] In view of the problems existing in the prior art, the present invention provides a saddle-shaped sheet metal forming device and method. Summary of the invention

[0004] Purpose of the invention: The present invention solves the problem of wrinkles and cracks generated in the saddle-shaped parts during the drop hammer forming process, and proposes a saddle-shaped sheet metal forming device and method.

[0005] In a first aspect, the present application provides a saddle-shaped sheet metal forming device, the device comprising:

[0006] A mold body having a first molding surface and a bottom filling surface, wherein the first molding surface fits the outer molding surface of the saddle-shaped sheet metal part;

[0007] A draw rib is arranged on the die body, and the draw rib is used to slow down the speed at which the sheet metal enters the first molding surface;

[0008] A vent hole is provided on the bottom filling surface;

[0009] The exhaust groove is arranged on the back side of the mold body, and the exhaust groove is communicated with the air vent.

[0010] The reference hole is arranged on the surface of the mold body.

[0011] Preferably, the size of the drawbead is determined according to the length and extension height of the saddle-shaped sheet metal.

[0012] Preferably, the cross-sectional shape of the drawbead is semicircular.

[0013] Preferably, the device further comprises:

[0014] A hydraulic press comprises a rubber and a table; wherein the table is used to place the mold body, and the rubber is used to squeeze the sheet material to obtain a saddle-shaped sheet metal part.

[0015] In a second aspect, the present application further provides a saddle-shaped sheet metal forming method, the method being applied to the above-mentioned device, the method comprising:

[0016] Place multiple layers of rubber blocks between the mold and the sheet. Try to completely fill the mold cavity with rubber blocks. The height is slightly lower than the upper surface of the mold. Perform the first hydraulic forming with a pressure of 5-10 MPa. If there are local wrinkles after forming, smooth the wrinkles. During the forming process, place a transparent film or apply lubricant between the sheet and the mold to improve the fluidity of the material.

[0017] Pull out one or two layers of rubber blocks and carry out the second rubber bag hydraulic press forming pressure of 5-10MPa. The number of rubber layers pulled out at one time depends on the part material and the total extension height. If wrinkles are locally formed after forming, wrinkle flattening should be carried out immediately. The number of extensions should be greater than the total extension height of the part / rubber single layer thickness.

[0018] Until the part completely fits the first surface.

[0019] Preferably, the method further comprises:

[0020] After the platform is cleaned, the mold is placed steadily on the forming table and formed using a 77000T rubber bag hydraulic press. A naturally transitioning rubber pad slope is placed in the unformed area near the mold, and rubber pads are filled between the side wall and the mold to the same height as the mold. Rubber is also filled in the mold cavity. After the mold is placed, oil and impurities on the surface of the mold are cleaned again.

[0021] Preferably, the method further comprises:

[0022] After the mold is placed, place the raw material or unfolded material flatly on the mold, visually check whether the cutting line of the mold is consistent with the unfolded material to avoid incorrect placement of the unfolded material. After the raw material is placed, clean the surface of the raw material again to remove surface oil and impurities, clean impurities on the auxiliary rubber, and cover the auxiliary rubber flatly.

[0023] Preferably, the method further comprises:

[0024] After the parts are formed, check the degree of adhesion of the parts to the tire. If there is a partial non-adhesion to the tire, the non-adhesion position needs to be manually calibrated until the adhesion requirement is met.

[0025] Beneficial technical effects of this application:

[0026] The present invention provides a saddle-shaped part forming method and device, which solves the problem of wrinkles and cracks in the original forming process. The rubber bag hydraulic press is used for multiple forming, which can greatly improve the surface quality of the parts, increase the qualified rate of the products, and achieve the purpose of reducing costs and increasing efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is an isometric view of a saddle forming device provided in an embodiment of the present application;

[0028] Figure 2 is an axonometric view of a saddle provided in an embodiment of the present application;

[0029] Figure 3 is a schematic diagram of a saddle rubber bag forming process provided in an embodiment of the present application;

[0030] Figure 4 is a top view of a saddle forming device provided in an embodiment of the present application;

[0031] Figure 5 is a cross-sectional view of a saddle forming device provided in an embodiment of the present application;

[0032] Among them, 1-mold body; 2-first molding surface; 3-drawing ribs; 4-rubber; 5-hydraulic press table; 6-sheet material; 7-rubber block. DETAILED DESCRIPTION

[0033] See also Figure 1-Figure 5 The present application provides a saddle forming method, comprising the following steps:

[0034] Step 1: Picking Materials

[0035] Collect the corresponding materials according to the material specifications given in the parts manufacturing instructions. When collecting materials, you must carefully check the material brand, specification, and standard, which must be consistent with those written in the instructions. The collected materials must be stored separately according to the material brand, specification, and standard, and be properly labeled.

[0036] Step 2: Cutting

[0037] Saddle-shaped sheet metal parts are cut using CNC milling

[0038] 2.1. Check the equipment: Turn on the power of the equipment and check whether the fault light of the equipment is on.

[0039] 2.2. After opening the production instruction, expand the digital model according to the corresponding instructions and import the corresponding expanded digital model into the CNC software.

[0040] 2.3. Copy and expand the digital model according to the number of parts in the production order and arrange them to maximize the use of the space of a sheet of sheet metal.

[0041] 2.4. The CNC milling worker places the sheet metal on the workbench of the CNC milling machine according to the CNC program data.

[0042] 2.5. After the sheet is placed, use a fixing clamp to fix the sheet to prevent it from slipping during the milling process (if the vacuum suction can hold the sheet, there is no need to use a fixing clamp to fix the sheet).

[0043] 2.6. The operator operates the milling machine to perform tool alignment operations, find the milling cutter origin, and after aligning the milling cutter, perform part milling according to the set CNC program.

[0044] 2.7. Let the milling head run through the cutter first to make sure there is no problem with the CNC program before milling the parts. The milling machine will mill the inner hole and then the outer shape of the part.

[0045] 2.8. After the parts are milled, they are inspected using gelatin boards.

[0046] Step 3: Forming

[0047] 3.1. Blank preparation: Clean the blank with a clean cotton cloth to ensure that there is no oil or debris on the surface of the blank to avoid marks during the forming process. Check whether the burrs on the edge of the blank are removed cleanly.

[0048] 3.2. Check and clean the tooling: Check the sharp corners of the mold. In principle, the sharp corners of the edges in the non-working area shall not be less than R10. In principle, holes other than those required by the process are not allowed to exist on the mold. If necessary, semi-circular ball pins should be used for plugging during the forming process. Check that the mold height (including the thickness of the wool and auxiliary rubber) must be lower than the depth of the workbench. Use a scouring pad to remove oil and impurities on the mold surface.

[0049] 3.3. Check the work surface: Clean the work surface in the mold placement area. Make sure the work surface is clean and free of eraser residue or other excess materials.

[0050] 3.4. Placement and cleaning of tooling: After the platform is cleaned, place the mold steadily on the forming table and use 77000T rubber bag hydraulic press equipment to form it. Place a natural transition rubber pad slope in the unformed area near the mold, fill the rubber pad between the side wall and the mold to the same height as the mold, and fill the mold cavity with rubber. After the mold is placed, clean the oil and impurities on the mold surface again.

[0051] 3.5. Place and clean the blank: After the mold is placed, place the raw material or unfolded material flatly on the mold, visually check whether the cutting line of the mold is consistent with the unfolded material to avoid incorrect placement of the unfolded material. After the raw material is placed, clean the surface of the raw material again to remove surface oil and impurities, clean impurities on the auxiliary rubber, and cover the auxiliary rubber flatly.

[0052] 3.6 Hydroforming

[0053] 3.6.1 Place multiple layers of rubber blocks between the mold and the sheet. Try to fill the mold cavity completely with rubber blocks. The height is slightly lower than the upper surface of the mold. Perform the first hydraulic forming with a pressure of 5 to 10 MPa. If there are local wrinkles after forming, smooth the wrinkles. During the forming process, a transparent film or lubricant can be placed between the sheet and the mold to improve the fluidity of the material.

[0054] 3.6.2. Pull out one or two layers of rubber blocks and carry out the second rubber bag hydraulic press forming pressure of 5-10MPa. The number of rubber layers pulled out at one time depends on the part material and the total extension height. If wrinkles are locally formed after forming, wrinkle flattening should be carried out immediately. The number of extensions should be greater than the total extension height of the part / the thickness of the rubber single layer.

[0055] 3.6.3. Repeat step 3.6.2 until the part fits the tooling completely.

[0056] 3.7 Correction:

[0057] After the parts are formed, check the degree of adhesion of the parts to the tire. If there is a partial non-adhesion to the tire, the non-adhesion position needs to be manually calibrated until the adhesion requirement is met.

[0058] 3.8 Inspection: The formed sheet metal parts should comply with the product design drawings and relevant technical conditions. The adhesion and surface quality of the formed sheet metal parts should meet the quality requirements.

[0059] In other embodiments of the present application, a saddle-shaped piece forming device provided by the present application is composed of a mold body 1, see Figure 1 .

[0060] The mold body has a first mold surface, and the first mold surface 2 fits the outer mold surface of the saddle piece and is designed as a concave mold structure.

[0061] Furthermore, the mold body surface adds draw ribs on both sides of the saddle sheet metal in the width direction to increase the flow resistance of the saddle sheet metal during stretching. The cross-sectional shape is semicircular, and the size of the draw ribs (R / a / b) is determined according to the length and extension height of the saddle sheet metal.

[0062] Furthermore, the distance between the part cutting line in the mold and the mold boundary is ≥120mm (such as Figure 4 shown).

[0063] Furthermore, the bottom of the mold body surface needs to have a corresponding number of vent holes according to the size of the part, generally with a diameter of D = 2×t, t being the thickness of the part, and there is a venting groove at the bottom of the mold.

[0064] Further, the depth L of the groove when the rubber bag is stretched into the groove area cannot exceed 1.5 times the width of the opening. If necessary, such a groove or cavity must be filled with enough rubber bands to ensure that the rubber bag is not destroyed even under maximum pressure.

[0065] Furthermore, the mold body material is Q235A steel.

[0066] Furthermore, three reference holes are opened around the mold body, and the reference holes are Φ8H8 in size and 15mm in depth.

[0067] The present invention provides a saddle-shaped part forming method and device, which solves the problem of wrinkles and cracks in the original forming process. The rubber bag hydraulic press is used for multiple forming, which can greatly improve the surface quality of the parts, increase the qualified rate of the products, and achieve the purpose of reducing costs and increasing efficiency.

Claims

1. A saddle-shaped sheet metal forming device, characterized in that: The device comprises: A mold body having a first molding surface and a bottom filling surface, wherein the first molding surface fits the outer molding surface of the saddle-shaped sheet metal part; A draw rib is arranged on the die body, and the draw rib is used to slow down the speed at which the sheet metal enters the first molding surface; A vent hole is provided on the bottom filling surface; An exhaust groove is arranged on the back of the mold body, and the exhaust groove is connected with the air vent; The reference hole is arranged on the surface of the mold body.

2. The device according to claim 1, characterized in that The size of the drawbead is determined according to the length and extension height of the saddle-shaped sheet metal part.

3. The device according to claim 2, characterized in that The cross-sectional shape of the drawbead is semicircular.

4. The device according to claim 3, characterized in that The device also includes: A hydraulic press comprises a rubber and a table; wherein the table is used to place the mold body, and the rubber is used to squeeze the sheet material to obtain a saddle-shaped sheet metal part.

5. A method for forming a saddle-shaped sheet metal part, characterized in that: The method is applied to the device according to any one of claims 1 to 4, and the method comprises: Place multiple layers of rubber blocks between the mold and the sheet. Try to completely fill the mold cavity with rubber blocks. The height is slightly lower than the upper surface of the mold. Perform the first hydraulic forming with a pressure of 5-10 MPa. If there are local wrinkles after forming, smooth the wrinkles. During the forming process, place a transparent film or apply lubricant between the sheet and the mold to improve the fluidity of the material. Pull out one or two layers of rubber blocks and carry out the second rubber bag hydraulic press forming pressure of 5-10MPa. The number of rubber layers pulled out at one time depends on the part material and the total extension height. If wrinkles are locally formed after forming, wrinkle flattening should be carried out immediately. The number of extensions should be greater than the total extension height of the part / rubber single layer thickness. Until the part completely fits the first surface.

6. The method according to claim 5, characterized in that The method further comprises: After the platform is cleaned, the mold is placed steadily on the forming table and formed using a 77000T rubber bag hydraulic press. A naturally transitioning rubber pad slope is placed in the unformed area near the mold, and rubber pads are filled between the side wall and the mold to the same height as the mold. Rubber is also filled in the mold cavity. After the mold is placed, oil and impurities on the surface of the mold are cleaned again.

7. The method according to claim 5, characterized in that The method further comprises: After the mold is placed, place the raw material or unfolded material flatly on the mold, visually check whether the cutting line of the mold is consistent with the unfolded material to avoid incorrect placement of the unfolded material. After the raw material is placed, clean the surface of the raw material again to remove surface oil and impurities, clean impurities on the auxiliary rubber, and cover the auxiliary rubber flatly.

8. The method according to claim 5, characterized in that The method further comprises: After the parts are formed, check the degree of adhesion of the parts to the tire. If there is a partial non-adhesion to the tire, the non-adhesion position needs to be manually calibrated until the adhesion requirement is met.

Citation Information

Patent Citations

  • Sheet shallow cavity part rubber forming method and mold

    CN106475466A

  • Aircraft metal plate drawing forming process method

    CN107755509A

  • Rubber padding assisted creep age forming tool for aluminum-lithium alloy thin-wall structure

    CN112570538A

  • Auxiliary method suitable for extension forming of aluminum alloy sheet part

    CN113680885A

  • Rubber bag hydraulic die for forming flanged holes and double bent edges

    CN210702021U

Cited By

  • Step-by-step hydraulic forming method for rubber bag of deep-cavity sheet metal part

    CN120460581A

  • A deep cavity sheet metal part rubber bag step-by-step hydraulic forming method