Method for producing casting mould, core and moulding base stock regenerated therefrom
By using a molding mixture of water glass and a granular amorphous silica and layered silicate, the problem of poor disintegration characteristics of the casting model core after casting is solved, and efficient casting mold and core regeneration and environmental protection are achieved. Casting process.
Patent Information
- Application Number
- CN202410988275.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-04-07
- Filing Date
- 2018-04-05
- Publication Date
- 2024-11-15
AI Technical Summary
Existing casting molds and cores have poor disintegration characteristics after casting, difficult to reuse, and the use of organic disintegration accelerators can lead to CO2 and other undesirable emissions, affecting the environment and the quality of recycled materials.
Using a molding mixture containing water glass and granular amorphous silica and layered silicate, the molding mold with high disintegration characteristics and renewable properties is cured by chemical reaction between components of the molding mixture and Core.
The good disintegration characteristics and high renewability of the casting mold and core are achieved, the CO2 emission is reduced, and the regenerated molding base material is close to the initial material, which is suitable for multiple recycling.
Smart Images

Figure BDA0004958118720000321 
Figure BDA0004958118720000351 
Figure BDA0004958118720000371
Abstract
Description
[0001] This invention application is a divisional application of the invention patent application with application date of April 5, 2018, application number of "201880037427.5", and invention name of "Method for manufacturing casting molds, cores and molding base materials regenerated therefrom". Technical Field
[0002] The invention relates to a method for producing a casting mold, a core and a molding base material regenerated therefrom, a mixture for combining with a solution or dispersion containing water glass to produce a casting mold and / or a core, a molding compound mixture, a molding base material mixture and a casting mold or a core. The invention also relates to the corresponding use of a certain amount of a particulate sheet silicate with a d90 value of less than 45 μm or a corresponding mixture as an additive for producing a molding compound mixture containing water glass and particulate, amorphous silicon dioxide, which during the production of the casting mold or the core solidifies by chemical reaction of the components of the molding compound mixture with one another in order to simplify the disintegration of the casting mold or the core and / or to increase the reproducibility. Background Art
[0003] Casting in lost foam is a common method for producing near-net-shape components. After casting, the mold is destroyed and the casting is removed. The casting mold is a negative mold that contains the cavity to be cast, which results in the casting to be produced. The inner contour of the future casting is formed by the core. When producing the casting mold, the cavity is shaped into the molding material with the help of a model of the casting to be produced. The inner contour is shown by the core formed in a separate core box.
[0004] For the casting mold and the core, refractory granular materials are mainly used as molding materials, for example cleaned, classified quartz sand. The refractory molding base material is preferably in a free-flowing form so that it can be filled into a suitable mold cavity and compacted there. The molding material is compacted to increase the strength. To produce the casting mold, the molding material is bonded by means of an inorganic or organic binder. The binder produces a firm bond between the particles of the molding base material, so that the casting mold obtains the required mechanical stability.
[0005] Moulds and cores must meet different requirements. In the casting process itself, the moulds and cores must first have sufficient strength and heat resistance to be able to contain the liquid metal in the cavity formed by one or more (sub) moulds. After the solidification process begins, the mechanical stability of the casting is ensured by the solidified metal layer formed along the wall of the mould. The material of the mould should now decompose under the influence of the heat emitted by the metal, so that the material loses its mechanical strength, that is, the bonding between the individual particles of the refractory material is lost. Ideally, the moulds and cores disintegrate into fine sand again, which can be removed from the casting without difficulty and has corresponding favorable disintegration characteristics. There is currently a special need to reuse the disintegration residues of the used moulds and cores, and to produce a moulding base material regenerated from the used moulds and cores. This reuse as a regenerated moulding base material (regenerated material) places special requirements on the disintegration characteristics of the moulds and cores.
[0006] For producing the casting mold, organic and inorganic binders can be used, the curing of which can be carried out by cold or hot methods. In this case, a cold method refers to a method that is carried out essentially at room temperature without heating the casting mold. In this case, curing usually takes place by a chemical reaction that is triggered, for example, by passing a gas as a catalyst through the casting mold to be cured. In hot methods, after the molding, the molding material mixture is heated to a sufficiently high temperature, for example in order to drive off solvents contained in the binder or to initiate a chemical reaction, by which the binder cures, for example, by crosslinking.
[0007] Regardless of the curing mechanism, all organic binder systems have in common that they decompose thermally when the liquid metal is introduced into the casting mold and release harmful substances such as benzene, toluene, xylene, phenol, formaldehyde and other partially unidentified cracking products. Although it is possible to minimize these emissions by various measures, they cannot be completely avoided in the case of organic binders.
[0008] In order to minimize or avoid the emission of decomposition products during the casting process, a binder can be used, which is based on an inorganic material or contains a very small portion of organic compounds. Such binder systems have long been known, for example from GB 782205A, US 6972059B1, US 5582232A, US 5474606A and US 7022178. The term "inorganic binder" hereinafter refers to a binder that is composed of more than 95% by weight, preferably more than 99% by weight, of water and inorganic materials, so that the portion of organic compounds in the inorganic binder is less than 5% by weight, preferably less than 1% by weight. The expression "inorganic bonding" refers to the production of casting molds or cores using an inorganic binder.
[0009] Alkali water glass is particularly useful as a component of an inorganic binder. Alkali water glass, also referred to below as water glass, refers to glassy, i.e. amorphous, water-soluble sodium, potassium and lithium silicates that solidify from a melt or their aqueous solutions. The term "water glass" hereinafter refers to mixtures with a molar modulus SiO2 / M2O in the range of 1.6 to 4.0, preferably in the range of 1.8 to 2.5, where M2O denotes the total amount of lithium oxide, sodium oxide and potassium oxide. The expression "water glass bonding" means that the casting mold or core is produced using a binder containing water glass.
[0010] Inorganic bonding molding material mixtures are known in the prior art. For example, in US 7770629B2, a molding material mixture is proposed, which, in addition to a refractory molding base material, also contains a water glass-based binder and particulate metal oxides, wherein precipitated silicic acid or pyrogenic silicic acid is preferably used as the particulate metal oxide.
[0011] US 4233076 discloses a molding material mixture, which consists of sand, an alkali metal silicate binder, at least one curing agent selected from: alkylene carbonate, organic monocarboxylic acid or dicarboxylic acid or its methyl ester, carbon dioxide or blast furnace slag and Al2O3-containing substances, and its average particle size distribution is between 0.2 and 5 μm.
[0012] DE 102012113073 A1 discloses a molding material mixture for producing molds and cores for metal processing, the molding material mixture comprising at least one refractory molding base material, an inorganic binder and at least one particulate metal oxide, wherein the particulate metal oxide comprises or consists of at least one α-phase aluminum oxide and / or at least one aluminum / silicon mixed oxide, but does not include an aluminum / silicon mixed oxide with a layered silicate structure.
[0013] DE 10 2012113074A1 discloses a molding material mixture for producing molds and cores for metal processing, the molding material mixture comprising at least one refractory molding base material, an inorganic binder and at least one particulate mixed metal oxide, wherein the particulate mixed metal oxide is at least one particulate mixed oxide or a particulate mixture of at least two oxides, or at least one particulate mixed oxide is present in addition to at least one other particulate oxide or in addition to at least one other particulate mixed oxide, and the particulate mixed metal oxide comprises at least one aluminum oxide and at least one zirconium oxide.
[0014] The disintegration behavior (also called de-coring performance) of molds and cores, i.e. the ability of molds and cores to disintegrate rapidly into an easily pourable form under mechanical load after metal casting, is generally worse in the case of purely inorganically bonded molds and cores, in particular in the case of waterglass-bonded molds and cores than in the case of molds and cores produced with the aid of organic binders. This unfavorable disintegration behavior is generally explained by the fact that the high temperatures during the casting of the metal melt cause sintering of the molding material composition containing alkali metal silicate glass or the formation of a melt phase. This leads to a high residual strength of the molds and cores. In this context, importance is generally attributed to the alkali metal content of the molding material mixture, wherein a high alkali metal content is generally regarded as disadvantageous.
[0015] Poor disintegration characteristics are particularly disadvantageous when using thin-walled or fine-line or complex casting molds, which are difficult to remove after the casting process. In particular, poor disintegration characteristics are an obstacle when striving to reuse inorganically bonded casting molds and cores that have been used in casting and to produce regenerated molding base materials (regenerated materials) from such casting molds and cores. Insufficient disintegration characteristics can cause: the obtained regenerated molding base materials exist in block form and are not free flowing enough to be reused alone or in combination with "fresh" initial molding base materials when producing casting molds and cores. In EP 2692460 B1, a method for producing a granular refractory composition is disclosed, which is used to produce casting molds and cores from used casting molds or cores, and the used casting molds or cores are made of refractory materials and alkaline binders, and the alkaline binders contain alkali metal particles.
[0016] In order to solve the problem of poor disintegration properties, it is known to add organic disintegration promoters to the molding mixture, which pyrolyze / react under the action of hot metal and thus simplify the disintegration of the mold or core after casting by forming pores. Document DE 1558155A discloses, for example, the use of sugar, hard coal powder or granular asphalt for water glass-bonded cores, DD 82809B1 discloses the use of starch products, coal powder and molasses as organic disintegration promoters, and DD 141118A1 discloses the use of coal powder, carbohydrates, starch, starch derivatives and sugar as disintegration promoters. However, the use of organic components in the molding mixture during casting usually leads to the occurrence of undesirable emissions of CO2 and other pyrolysis products. In addition, it is considered to be particularly disadvantageous that organic disintegration promoters usually lose their effectiveness at high casting temperatures, because they are at high temperatures, such as the high temperatures that occur when cast steel, and the complete burning out of organic disintegration promoters occurs rapidly, and when the organic disintegration promoters are exhausted, the melting and sintering process still proceeds. In this case, the disintegration characteristics are only not significantly improved usually by organic disintegration promoters. In addition, the reusability of the casting mold and core manufactured by organic disintegration promoters is often limited, because the regenerated molding base material that can be manufactured by the casting mold and core may be polluted by the residue or decomposition products of the organic disintegration promoter, which can have an adverse effect on the characteristics of the regenerated molding base material, and then it must be removed costly. In addition, in own experiments, it has been confirmed that the use of organic disintegration promoters can reduce the resistance of the casting mold and core manufactured with respect to air humidity and / or water-based refractory coatings.
[0017] Due to the disadvantages of organic disintegration promoters described in detail above, there is a need for alternative, preferably inorganic disintegration promoters for inorganically bonded casting molds and cores, which can also have a positive influence on the disintegration properties of casting molds and cores at high casting temperatures without having the disadvantages of the known organic disintegration promoters. Such inorganic disintegration promoters are described in the prior art.
[0018] Document DE 1558155 discloses that an improvement in the de-coring properties of castings, especially those cast at high temperatures, can be achieved when a portion of the inert filler is replaced by calcium carbonate, wherein other alkaline earth metal carbonates can also be used instead of calcium carbonate. In this case, however, the effect of accelerating disintegration is caused by the decomposition of the carbonates, wherein CO2 is released. This situation is often considered to be disadvantageous. In addition, the disclosure of DE 1558155 relates to the use in cores produced by means of water glass, which is bonded by adding a powdered hardener, which contains bentonite in addition to silicon or a silicon alloy.
[0019] DD 246488 A1 discloses a molding material with favorable disintegration properties, which is used for producing molds and cores in casting production processes, in particular for forming cast products made of steel castings, characterized in that it contains one or more refractory basic components and a binder, preferably in a ratio of 1:1, wherein the binder consists of a sodium silicate solution (modulus 2.2 ... 2.6; density 1.46 ... 1.55 g / cm 3 ) and sodium silicate solution chemically modified with alkali metal phosphate (modulus 2.6...3.5; density 1.38...1.41 g / cm 3 DD 246488 relates to a molding material which is cured by gas treatment with CO 2 .
[0020] DE 102013111626 A1 discloses a molding material mixture for producing a mold or a core, the molding material mixture comprising at least one refractory molding base material, water glass as a binder, granular amorphous silicon dioxide and one or more powdered oxidized boron compounds. In this case, the oxidized boron compound is used as a disintegration promoter.
[0021] DE 1190610 and DE 1198495 disclose the use of bentonites for producing molds and cores which readily disintegrate after casting according to the waterglass-carbonic acid process.
[0022] US 3203057 discloses a molding compound mixture consisting of a fine refractory material, a liquid binder consisting essentially of an alkali metal silicate solution, and a disintegration promoter consisting essentially of Al2O3. The alkali metal silicate solution must have a basicity in the range of 18-30%.
[0023] DE 10 2005 041 863 A1 discloses molding material mixtures which contain borosilicate glass.
[0024] R. Ramakrishnan's doctoral thesis (Technical University of Munich, passed January 2016) deals with 3D printing with the aid of inorganic molding material systems.
[0025] DE 15 58 155 A teaches a method for producing a core.
[0026] EP 2308614 A1 describes an aerogel sand which is given green strength by the addition of layered silicates and xerogels.
[0027] X. Zhang et al. reported in Mater. Horiz. 2014, 1, 232-236: Conventional aerogels, including organic resorcinol-formaldehyde aerogels, are mostly difficult to regenerate, and thus often become a problem in waste disposal. Summary of the invention
[0028] A main object of the present invention is to provide a method for producing a casting mold and a core, wherein the casting mold and the core are especially water glass bonded casting molds and cores, wherein the produced casting mold and the core are to meet the following requirements:
[0029] - Easy manufacturability using commonly used equipment and manufacturing procedures;
[0030] - high strength immediately after production and a strength that remains largely unchanged even after a long storage period;
[0031] - high resistance to air humidity and water-containing refractory coatings, so that contact with air humidity or coating of casting molds and cores with water-containing refractory coatings causes only a small loss of strength;
[0032] - Very good surface quality of the castings produced with the casting mold or core, especially in the case of brass casting, cast iron or cast steel;
[0033] - no or only low emissions of CO 2 and / or other undesirable pyrolysis products during metal casting, in particular during brass casting, iron casting or steel casting;
[0034] - Very good disintegration properties after use in metal casting, in particular in brass casting, cast iron or cast steel, ie low residual strength, so that after use in metal casting, the casting mold and core can be separated from the casting easily and without residue even under low mechanical stress.
[0035] Furthermore, it is an object of the present invention to design the method in such a way that it is possible with particularly low effort to obtain a recycled molding base material from the produced castings and cores, the properties of which are particularly similar to those of the original molding base material, i.e. a molding base material of the same kind and from the same origin which has not yet been used in the production of the castings and cores.
[0036] The regenerated molding base material (first generation) thus produced should therefore be suitable for producing casting molds and cores, in particular for producing casting molds and cores according to the method to be described. The regenerated molding base material produced is therefore suitable for producing casting molds and cores which meet the requirements defined above and which, after use in brass casting, cast iron or cast steel, also exhibit good disintegration properties again and can be easily converted into a regenerated molding base material (second generation).
[0037] The object here is to design the method in such a way that the recyclability of the basic molding material to be used in the method is particularly high, ie during the method, which is carried out cyclically, the individually considered basic molding material particles become components of the largest possible number of casting molds or cores.
[0038] In order to be able to meet the above requirements particularly well, one object is to design the proposed method in such a way that the produced regenerated molding base corresponds as precisely as possible with respect to its chemical composition to the original molding base, i.e. a molding base of the same kind and origin that has not yet been used in the production of the casting molds and cores. This means, in particular, that the content of alkali metal ions and the content of other additives, in particular the content of disintegration promoters that may be present in the casting molds and cores, in the regenerated molding base should be as low as possible so that the concentration of these components does not increase during the method to be described.
[0039] Furthermore, a further object is to design the method to be described in such a way that it can be carried out particularly effectively in practice using a molding base batch cycle.
[0040] A supplementary object of the present invention is to achieve that the steps of the method to be described are carried out at least partially using a 3D printer or a 3D printing method.
[0041] Furthermore, it was an object of the present invention to specify (i) mixtures for combination with solutions or dispersions containing water glass, (ii) multi-component binder systems, and (iii) molding material mixtures with which casting molds and cores which meet the requirements defined above can be produced.
[0042] Furthermore, the object of the present invention is to propose a molding base material mixture, with the help of which casting molds and cores that meet the requirements defined above can be manufactured, and the molding base material mixture contains recycled molding base material, which can be manufactured with the help of the method to be described (see above).
[0043] Furthermore, it is an object of the present invention to specify a casting mold or a core which meets the requirements defined above.
[0044] Further (sub)objects of the invention emerge from the dependent patent claims and the description.
[0045] The abovementioned objects are achieved by a method, a mixture, a multi-component binder system, a molding compound mixture, a molding base compound mixture, a use, a casting mold and a core, as defined in the appended claims. Preferred embodiments according to the invention are given in the dependent claims.
[0046] In particular, the above-mentioned objects are achieved by a method for producing a casting mold, a core and a basic molding compound regenerated therefrom, the method comprising the following steps for producing a casting mold or a core:
[0047] - Providing or producing a molding compound mixture, the molding compound mixture comprising:
[0048] - a molding base material, preferably a granular molding base material,
[0049] - a solution or dispersion comprising water glass,
[0050] - 0.1 to 3% by weight of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide,
[0051] and to simplify the disintegration of the mold or core and / or to improve reproducibility,
[0052] - one or more particulate phyllosilicates in a total amount of 0.05 to 1.5% by weight, preferably 0.1 to 0.4% by weight, particularly preferably 0.1 to 0.3% by weight, wherein d 90 The value is less than 45μm,
[0053] The percentages are based on the total amount of the molding compound mixture.
[0054] - forming of the molding compound mixture,
[0055] The molding compound mixture is solidified by chemical reaction of its components with one another, so that a casting mold or a core is produced.
[0056] The basic molding material is preferably a refractory basic molding material. In this context, "refractory" is understood to mean, in accordance with the general understanding of the person skilled in the art, materials, and minerals that can at least temporarily withstand the temperature loads during casting or during the solidification of the iron melt, usually cast iron. Suitable basic molding materials are, for example, quartz sand, zircon sand or chrome ore sand, olivine, vermiculite, bauxite, soft clay, and synthetic basic molding materials.
[0057] The molding base material preferably accounts for more than 80% by weight, preferably more than 90% by weight, and particularly preferably more than 95% by weight of the total amount of the molding material mixture. The refractory molding base material preferably has a free-flowing state. Therefore, the molding base material to be used according to the present invention is preferably and usually (see above) present in granular or particulate form.
[0058] The average diameter of the molding base material particles is usually between 100 μm and 600 μm, preferably between 120 μm and 550 μm and particularly preferably between 150 μm and 500 μm. The particle size can be determined, for example, by sieving in accordance with DIN ISO 3310. Preferably, within the scope of the present invention, the particle size or the average diameter of the molding base material particles is determined by sieving in accordance with point 4.3 of the VDG data sheet (i.e. the data sheet of the “German Association of Foundry Experts”) from October 1999, page 27, which stipulates the use of test sieves in accordance with DIN ISO 3310.
[0059] Solutions or dispersions containing water glass can be prepared by dissolving glassy lithium silicate, sodium silicate and potassium silicate in water. It is possible to use water glass which contains one, two or more of the alkali metal ions mentioned and / or contains one or more polyvalent cations, such as aluminum.
[0060] The solution or dispersion containing water glass preferably has a solids content in the range of 25% to 65% by weight, preferably 30% to 55% by weight, particularly preferably 30% to 50% by weight, based on the total amount of the solution or dispersion. In calculating the solids content, the entire liquid phase contained in the molding material mixture, for example water or alcohol, is included in the solution or dispersion.
[0061] Depending on the use of the molds and cores to be produced and the desired strength level, the molding material mixture comprises 0.5% to 5% by weight, preferably 0.75% to 4% by weight, particularly preferably 1% to 3.5% by weight, of a solution or dispersion containing water glass, based on the total amount of the molding material mixture.
[0062] According to the invention, the molding compound mixture contains granular, amorphous silicon dioxide ("SiO2"); preferably pyrogenic, granular, amorphous silicon dioxide of conventional purity, i.e. with conventional impurities and secondary components. The term "granular" here means solid powder (including dust) or also granular material, which is pourable and thus also sieveable.
[0063] Granular, amorphous silicon dioxide, preferably pyrogenic, granular, amorphous silicon dioxide 90 The value is preferably less than 100 μm, preferably less than 45 μm, particularly preferably less than 25 μm. This means that 90% of the particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide contained in the molding compound mixture is preferably less than 100 μm, preferably less than 45 μm, particularly preferably less than 25 μm. 90 The values were determined by photographing with a scanning electron microscope (JSM-6510 from Jeol).
[0064] As granular, amorphous silicon dioxide, synthetically produced or naturally occurring types can be used. The latter is known, for example, from DE 102007045649, but is not preferred because it usually contains a not insignificant crystalline content and is therefore classified as a carcinogen. Synthetically produced amorphous silicon dioxide is produced by a deliberate chemical reaction. Examples of this are the flame hydrolysis of silicon tetrachloride and the reduction of quartz sand in an electric arc furnace, for example with the aid of coke, when producing ferrosilicon and silicon. Amorphous SiO2 ("silicon dioxide") produced according to these two methods is also referred to as pyrolytic SiO2.
[0065] The molding compound mixture preferably contains synthetically produced, particulate, amorphous SiO 2 , particularly preferably pyrogenic, particulate, amorphous SiO 2 .
[0066] In the process according to the invention (or in the molding compound mixture of the process according to the invention), the pyrogenic, granular, amorphous silicon dioxide to be used with particular preference includes, within the scope of the invention, the following types of granular, amorphous silicon dioxide (often also referred to as "pyrogenic silicic acid"), which are designated by CAS RN 69012-64-2 and CAS RN 112945-52-5. Such types of pyrogenic, granular, amorphous silicon dioxide to be used with particular preference in the process according to the invention can be prepared in a manner known per se, in particular by flame hydrolysis of silicon tetrachloride, by reduction of quartz sand with carbon (e.g. coke) in an electric arc furnace (preferably in the production of ferrosilicon and silicon), or from ZrSiO4 or in the preparation of ZrO2 from ZrSiO4.
[0067] More particularly preferably, the pyrogenic, granular, amorphous silicon dioxide preferably to be used according to the invention comprises a granular, amorphous silicon dioxide which is designated by CAS RN 69012-64-2 and which is preferably produced by reducing quartz sand with carbon (e.g. coke) in an electric arc furnace (preferably in the production of ferrosilicon and silicon) or which is precipitated as a by-product in the production of ferrosilicon and silicon and / or which is produced from ZrSiO4 or precipitated as a by-product in the production of ZrO2 from ZrSiO4. In the professional field, this specific pyrogenic, granular, amorphous silicon dioxide is also referred to as "microsilica".
[0068] "CAS RN" stands for CAS Registry Number and CAS Registration Number, in English: CAS Registry Number (CAS Registry Number), CAS = Chemical Abstracts Service (Chemical Abstracts Service). This is the international naming standard for chemical substances. For each chemical substance registered in the CAS database (also biosequences, alloys, polymers), there is a one-to-one CAS number.
[0069] In a preferred variant of the method according to the invention, the molding compound mixture contains exclusively pyrogenic, particulate, amorphous silicon dioxide as particulate, amorphous silicon dioxide.
[0070] Layered silicates are silicates and are salts of orthosilicates (Si(OH4)). These salts are compounds constructed by SiO4 tetrahedra. Layered silicates are silicates whose silicate anions consist of (double) layers of corner-connected SiO4 tetrahedra. The layers or double layers are not connected to each other via further Si-O bonds to form a framework. Preferred layered silicates are kaolinite, metakaolin, montmorillonite, halloysite, hectorite, montmorillonite, muscovite, pyrophyllite and synthetic layered silicates, wherein synthetic layered silicates are not naturally occurring layered silicates, but rather layered silicates artificially produced by targeted chemical reactions.
[0071] According to the present invention, the total amount of phyllosilicate is d 90 The value is less than 45 μm. This means that 90% of the layered silicate particles contained in the molding compound mixture are smaller than 45 μm. 90 The values were determined by photographing with a scanning electron microscope (JSM-6510 from Jeol).
[0072] In the process according to the invention, the molding compound mixture contains one or more sheet silicates in order to simplify the disintegration of the casting mold or core and / or to increase the reproducibility.
[0073] In the process according to the invention, the molding compound mixture preferably contains one or more sheet silicates in order to simplify the disintegration of the casting mold or core and to increase the reproducibility.
[0074] Simplified disintegration means that molds and cores made from the molding compound mixture have low residual strength after use in metal casting, i.e. after contact with hot molten metal, for example molten iron, and can be separated from the casting quickly and without residue even under low mechanical loads. The increased reproducibility of the mold or core means that from the mixture obtained from the used mold or core by stripping it from the casting, a regenerated material can be obtained, which can be used again as a molding base material in the molding compound mixture for producing the mold or core, wherein the chemical composition and properties of the regenerated material are particularly similar to the chemical composition and properties of the molding base material which has been used to produce the original mold or original core.
[0075] Compared with the molds and cores made of the molding material mixture that does not contain granular, amorphous silicon dioxide, preferably pyrolytic, granular, amorphous silicon dioxide, nor granular phyllosilicate, the disintegration of the mold or core is simplified or its reproducibility is improved by the simultaneous presence of granular, amorphous silicon dioxide, preferably pyrolytic, granular, amorphous silicon dioxide, and one or more granular, phyllosilicates in the molding material mixture for production. When preparing the molding material mixture, for example, it occurs that a refractory molding base material is usually placed in a mixer in advance. Subsequently, a solution or dispersion containing water glass, granular amorphous silicon dioxide, preferably pyrolytic, granular amorphous silicon dioxide, granular phyllosilicate and other components as needed is mixed into the refractory molding base material under stirring. The mixing duration is preferably selected so that the intimate mixing of the components of the molding material mixture is achieved.
[0076] The shaping of the molding material mixture includes any intentional and targeted shaping of the molding material mixture, i.e. any intentional and targeted conversion of the molding material mixture into a three-dimensional configuration. Preferably, the shaping of the molding material mixture is carried out by introducing the molding material mixture into a (hollow) mold. Alternatively, the shaping of the molding material mixture can also be carried out by means of other methods known to those skilled in the art. For example, the shaping of the molding material mixture can be carried out within the scope of a 3D printing method by means of a 3D printer.
[0077] The curing of the molding material mixture includes any of the following processes, by which the strength of the molded molding material mixture is increased compared to the uncured molded molding material mixture. The curing of the molding material mixture does not need to be a prerequisite for complete curing. Therefore, the curing of the molding material mixture also includes incomplete curing of the molding material mixture. This corresponds to the understanding of the term "curing" by the person skilled in the art, because for reasons of reaction kinetics, it is not expected that all reactive components in the prepared or provided molding material mixture react during the curing process. In this regard, the person skilled in the art is familiar with the phenomenon of post-curing of the molding material mixture, for example.
[0078] According to the invention, the curing of the molding mixture takes place by chemical reaction of the components of the molding mixture with one another, so that a casting mold or a core is produced. The reason for curing the molding mixture containing a solution or dispersion containing water glass is mainly the condensation of the water glass, that is, the silicate units of the water glass are linked to one another.
[0079] Within the scope of the present invention, the curing of the molding compound mixture takes place by a chemical reaction of the components of the molding compound mixture with one another, if, in order to accelerate or initiate curing, no further substances need to be supplied to the formed molding compound mixture from the outside or even with the aid of suitable equipment, which further substances participate in the curing reaction or which initially initiate the curing reaction.
[0080] Examples of curing of the molding compound mixture by chemical reaction of the components of the molding compound mixture with one another are methods known per se to the person skilled in the art, in which curing is accelerated or caused by heating the shaped molding compound mixture, and methods in which curing of the molding compound mixture is accelerated or caused by saponification of an ester which is part of the molding base mixture.
[0081] An example of a non-inventive curing of a molding compound mixture is a method in which the curing of the molding compound mixture is promoted or caused by targeted gas treatment of the molded molding compound mixture with a gas or a gas mixture containing more than 1 mol % CO2 in a suitable facility and / or using suitable equipment (e.g., lines, pumps, etc.). In this method for curing molding compound mixtures, known as the CO2 method, the curing of the molding compound mixture occurs not only by chemical reactions of the components of the molding compound mixture with one another, but also, in particular, by reactions of the components of the molding compound mixture with a reactant supplied from the outside, namely CO2. In contrast to the casting molds and cores produced by means of the method according to the invention, the casting molds and cores produced by curing according to the CO2 method in an otherwise identical method design do not show the surprising advantages observed. In particular, the corresponding casting molds and cores show poor disintegration properties and significantly reduced reproducibility compared to the casting molds and cores according to the invention.
[0082] It is to be understood that the method according to the invention is preferably carried out under ambient conditions, i.e. in the presence of room air. Although the room air contains carbon dioxide, this does not correspond in the sense of the invention to curing by means of a CO2 method, which presupposes targeted gas treatment of the molding compound mixture by means of a gas rich in CO2, in particular in suitable facilities and / or when using suitable equipment (e.g. pipelines, pumps, etc.). On the contrary, when using the CO2 method, chemical bonding of the water glass components also occurs to a small extent, without the transported CO2 molecules participating in the chemical bonding. However, this is not to be understood as curing the molding compound mixture by chemical reactions of the components of the molding compound mixture with one another.
[0083] Correspondingly preferred is a method according to the invention (preferably as described above as preferred) in which the curing of the molding compound mixture takes place to an extent of more than 95%, preferably more than 99%, based on the amount of condensation reactions, by chemical reaction of the components of the molding compound mixture with one another, and / or
[0084] The curing of the molding compound mixture does not take place by means of a CO2 process.
[0085] Preferred is the method according to the invention set out above (preferably as described above as preferred), said method comprising the following steps for making a casting mould or core:
[0086] - Providing or producing a molding compound mixture, the molding compound mixture comprising:
[0087] - a molding base material, preferably a granular molding base material,
[0088] wherein the average diameter of the molding base material particles is preferably in the range of 100 μm to 600 μm, preferably in the range of 120 μm to 550 μm and particularly preferably in the range of 150 μm to 500 μm, wherein the particle size or average diameter of the molding base material particles is determined by sieving according to page 27, point 4.3 of the VDG data sheet of October 1999,
[0089] a solution or dispersion containing water glass, wherein the water glass in the molding material mixture preferably has a SiO2 / M2O molar modulus in the range from 1.6 to 4.0, particularly preferably in the range from 1.8 to 2.5, where M2O denotes the sum of lithium oxide, sodium oxide and potassium oxide,
[0090] - 0.1 to 3% by weight of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide,
[0091] and, in order to simplify the disintegration of the mold or core and / or to improve reproducibility,
[0092] - one or more particulate layered silicates in a total amount of 0.05 to 1.5% by weight, preferably 0.1 to 0.4% by weight, more preferably 0.1 to 0.3% by weight, wherein d 90 The value is less than 45μm,
[0093] The percentages are based on the total amount of the molding compound mixture.
[0094] - forming of the molding compound mixture,
[0095] The molding compound mixture is solidified by chemical reaction of its components with one another, so that a casting mold or a core is produced.
[0096] Preferred is a method according to the invention (preferably as mentioned above as preferred), wherein the molding compound mixture comprises one or more of the following components:
[0097] 0.3% to 3% by weight, preferably 0.57% to 0.77% by weight, of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide,
[0098] - one or more particulate layered silicates in a total amount of 0.1% to 0.4% by weight, preferably 0.1% to 0.3% by weight, wherein d 90 The value is less than 45μm,
[0099] - graphite and / or molybdenum(IV) sulfide in a total amount of up to 1% by weight, preferably up to 0.2% by weight, preferably in a total amount in the range from 0.01% to 0.2% by weight, preferably in a range from 0.03% to 0.08% by weight, wherein preferably only graphite is used,
[0100] - esters in a total amount of up to 0.4% by weight, preferably in a total amount in the range of 0.01% to 0.4% by weight, wherein preferably at least one ester is selected from: intramolecular or intermolecular reaction products of alcohols and acids, wherein
[0101] The alcohol is selected from C1-C8 monohydric alcohol, C1-C8 dihydric alcohol, preferably C2-C8 dihydric alcohol, and C1-C8 trihydric alcohol, preferably C3-C8 trihydric alcohol, preferably selected from ethylene glycol, 1,2-propylene glycol and glycerol,
[0102] as well as
[0103] The acid is selected from organic C2-C8 monocarboxylic acids, organic C2-C8 dicarboxylic acids, organic C2-C8 tricarboxylic acids, preferably organic C4-C8 tricarboxylic acids and inorganic acids, preferably selected from formic acid, acetic acid, propionic acid, lactic acid, oxalic acid, succinic acid, malonic acid, phosphoric acid, sulfuric acid, boric acid and carbonic acid,
[0104] Preferably, at least one ester is propylene carbonate or γ-butyrolactone,
[0105] - up to 4% by weight of particulate, mixed metal oxides, preferably comprising at least one aluminum oxide and at least one zirconium oxide,
[0106] - one or more surface-active substances selected from the group consisting of anionic surfactants, nonionic surfactants, cationic surfactants and amphoteric surfactants, the total amount of which is 0.001% to 1% by weight,
[0107] one or more oxidized boron compounds in a total amount of 0.002% to 1% by weight, wherein one or at least one oxidized boron compound is preferably selected from the group consisting of borates, boric acid, boric anhydride, borosilicates, boron phosphates and borophosphosilicates, particularly preferably from the group consisting of alkali metal borates and alkaline earth metal borates, wherein the oxidized boron compound preferably does not contain any organic groups,
[0108] - one or more phosphorus compounds in a total amount of 0.05% to 1% by weight, wherein one or at least one phosphorus compound is preferably selected from: organic phosphates and inorganic phosphates, preferably from: inorganic alkali metal phosphates,
[0109] - one or more carbohydrates in a total amount of 0.01 wt.% to 10 wt.%, wherein one or at least one carbohydrate is preferably selected from: oligosaccharides and polysaccharides, preferably selected from: cellulose, starch and dextrin,
[0110] - 0.02 to 5% by weight of barium sulfate,
[0111] - one or more silanes in a total amount of 0.1 to 2% by weight,
[0112] One or at least one silane is preferably selected from the group consisting of aminosilanes, epoxysilanes, mercaptosilanes, hydroxysilanes and ureidosilanes,
[0113] - one or more lithium compounds in a total amount of 0.01% to 0.2% by weight, wherein one or at least one lithium compound is preferably selected from: amorphous lithium silicate, lithium oxide and lithium hydroxide,
[0114] - particulate aluminum oxide, preferably aluminum oxide in the alpha phase, and / or particulate aluminum / silicon mixed oxide without a phyllosilicate structure, in a total amount of 0.05% to 4% by weight,
[0115] The percentages stated therein are each based on the total amount of the molding compound mixture.
[0116] The correspondingly preferred method according to the invention has proven to be particularly advantageous in its own experiments, since it allows the production of casting molds and cores which have particularly good disintegration properties and can be regenerated particularly easily, so that the regenerated molding base material obtained can be used again as molding base material particularly easily, in particular again in the method according to the invention.
[0117] Graphite and / or molybdenum(IV) sulfide serve as lubricants and thus improve the processability of the molding compound mixture, which in particular simplify the step of shaping the molding compound mixture in the method according to the invention. Surprisingly, the presence of these substances in the molding compound mixture has no negative effect on the disintegration properties of the molds and cores produced. It has been shown that graphite is preferred to molybdenum(IV) sulfide, since in this case the reproducibility of the produced casting molds and cores is higher.
[0118] Another component preferably contained in the molding material mixture is an ester. The ester is the reaction product of an alcohol and an acid in an esterification reaction, wherein the esterification reaction can take place not only intermolecularly but also intramolecularly, i.e., in a single molecule having an acid function and an OH group, a ring closure is caused. An example of an ester which is an intramolecular reaction product of an alcohol and an acid is gamma-butyrolactone. Esters are preferred as components of the molding material mixture because they can cause or accelerate the curing of the molding material mixture; corresponding curing methods are also known to those skilled in the art as "ester methods".
[0119] Advantageously, it has been demonstrated in own experiments that the molding compound mixture to be provided or produced in the method according to the invention can also contain one or more components in a given amount selected from the group consisting of particulate, mixed metal oxides, surface-active substances, oxidized boron compounds, phosphorus compounds, carbohydrates, barium sulfate, silanes, lithium compounds and particulate aluminum oxide (preferably as mentioned above as preferred) without impairing the advantages of the method according to the invention, in particular the improved disintegration properties and increased reproducibility of the casting molds and cores that can be produced by means of the method according to the invention. This is therefore particularly advantageous, since the processing properties of the molding compound mixture and / or the properties of the produced casting molds and cores (for example the strength of the casting molds and cores or the surface quality of the castings that can be produced) can be adapted to the respective requirements by means of the components detailed above, without losing the advantages of the method according to the invention.
[0120] Barium sulfate can be added to the molding material mixture in order to further improve the surface quality of the casting, especially when casting aluminum. Barium sulfate is preferably added in an amount of 0.05% to 3.0% by weight, particularly preferably 0.1% to 2.0% by weight, based on the total amount of the molding material mixture.
[0121] Preferably, silanes are added to the molding compound mixture in order to increase the wettability of the molding base or the flowability of the molding compound mixture.
[0122] Particulate aluminum oxide, preferably in the alpha phase, and / or particulate aluminum / silicon mixed oxides without a phyllosilicate structure and / or particulate mixed metal oxides can be added to the molding compound mixture in order to further improve the surface quality of the casting, in particular in cast steel and cast iron, so that after the mold has been removed from the casting, only a small amount of post-processing of the surface of the casting is necessary or even no post-processing at all. Preferably, the concentration is between 0.1% and 2.0% by weight, particularly preferably between 0.1% and 1.5% by weight, and particularly preferably between 0.2% and 1.2% by weight, based on the total amount of the molding compound mixture.
[0123] Phosphorus compounds can be added to the molding compound mixture in order to enable the production of particularly thin-walled casting molds and cores which nevertheless have high strength and high resistance when used in metal casting. Aluminum phosphate can also be used as a curing agent for waterglass adhesives.
[0124] Surface-active substances, in particular surfactants, can be added to the molding compound mixture in order to improve the flowability of the molding compound mixture. Suitable representatives of these compounds are described, for example, in WO 2009 / 056320 (= US 2010 / 0326620 A1).
[0125] Oxidized boron compounds can be added to the molding compound mixture in order to be able to produce particularly moisture-resistant casting molds and cores.
[0126] Carbohydrates can be added to the molding compound mixture in order to be able to produce particularly strong casting molds and cores having a high storage stability.
[0127] Lithium compounds can be added to the molding compound mixture in order to be able to produce particularly storage-stable casting molds and cores which are highly resistant to moisture.
[0128] In own experiments, the above-defined preferred contents of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide, and the total amount of particulate phyllosilicate have proven to be ranges in which the surprising effects of improved cracking behavior and increased reproducibility of casting molds and cores produced by the method according to the invention are particularly evident. This effect is particularly pronounced when the molding compound mixture contains both components in the amounts given as preferred, preferably in the amounts given as particularly preferred.
[0129] This means that it is very preferred (preferably as mentioned above) for the method according to the invention in which the molding compound mixture comprises:
[0130] - 0.3% to 3% by weight, preferably 0.57% to 0.77% by weight, of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide, and
[0131] - one or more particulate layered silicates in a total amount of 0.1% to 0.4% by weight, preferably 0.1% to 0.3% by weight, wherein d 90 The value is less than 45μm.
[0132] Taking into account the advantages mentioned above, a method according to the invention is particularly preferred (preferably as mentioned above as preferred), which method comprises providing or producing a molding compound mixture, the molding compound mixture comprising:
[0133] - Moulding base material,
[0134] - a solution or dispersion comprising water glass,
[0135] - one or more particulate layered silicates, in a total amount of 0.1% to 0.4% by weight, preferably 0.1% to 0.3% by weight, wherein d 90 The value is less than 45μm,
[0136] - 0.3% to 3% by weight, preferably 0.57% to 0.77% by weight, of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide, and
[0137] - 0.01 to 1% by weight of graphite,
[0138] The percentages stated therein are each based on the total amount of the molding compound mixture.
[0139] Particularly preferred is also a method according to the invention (preferably as indicated above as preferred), which comprises providing or producing a molding compound mixture, which comprises:
[0140] - Moulding base material,
[0141] - a solution or dispersion comprising water glass,
[0142] - one or more particulate layered silicates in a total amount of 0.1% to 0.4% by weight, preferably 0.1% to 0.3% by weight, wherein d 90 The value is less than 45μm,
[0143] 0.3% to 3% by weight, preferably 0.57% to 0.77% by weight, of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide,
[0144] - 0.01 to 1% by weight of graphite, and
[0145] - one or more components selected from the group consisting of particulate, mixed metal oxides, surface-active substances, oxidized boron compounds, phosphorus compounds, carbohydrates, barium sulfate, silanes, lithium compounds and particulate aluminum oxide (preferably as mentioned above as preferred),
[0146] The percentages stated therein are each based on the total amount of the molding compound mixture.
[0147] Furthermore, preference is given to a method according to the invention (preferably as indicated above) in which the water glass in the molding material mixture has a molar modulus SiO2 / M2O in a range from 1.6 to 4.0, preferably in a range from 1.8 to 2.5, wherein M2O denotes the total amount of lithium oxide, sodium oxide and potassium oxide.
[0148] The method according to the invention, which is preferably used, is advantageous because it allows particularly strong casting molds and cores to be produced which have excellent disintegration properties and can be easily regenerated.
[0149] In the case of molar moduli of water glass above those stated above, the initial strength of the casting molds or cores produced from the molding compound mixture is in some cases insufficient for use in metal casting, in particular in cast steel, cast iron or brass casting.
[0150] In the case of lower molar moduli, in some cases, the application of heat to the mold or core produced from the molding material mixture during the casting process only leads to a relatively high residual strength, so that the disintegration behavior is slightly less favorable than in the case of the mold and core produced by the preferred method according to the invention. At higher M2O concentrations, i.e., at lower molar moduli, the mold and core produced from the molding material mixture also show a slightly less favorable reproducibility, in particular a slightly less favorable multiple reproducibility. The latter means that the reproducibility of the mold or core produced from the molding material mixture that already contains the regenerated molding base material is reduced in this case. This poorer behavior compared to the preferred method according to the invention may be related to the enrichment of alkali metal oxides in the regenerated molding base material.
[0151] Preferred is the process of the invention (preferred as described above as preferred), wherein the molding base comprises quartz sand, preferably at least 50% by weight, particularly preferably at least 80% by weight, based on the total amount of the molding base.
[0152] The corresponding preferred method according to the invention has proven to be particularly advantageous in practice, since when using quartz sand as a basic casting mold material, particularly good disintegration and thus good reproducibility of casting molds and cores that can be produced from the molding compound mixture are shown, making the molding compound technically preferred. The reason for this may be that quartz sand composed of silicon dioxide has a particularly high chemical compatibility with water glass, which is also silicon-based and used as a binder, and granular, amorphous silicon dioxide, preferably pyrogenic, granular, amorphous silicon dioxide. Due to the combination of these components, which contain in particular silicon and oxygen, almost no impurities can accumulate, i.e., for example, no oxides of other elements can accumulate in the regenerated molding compound.
[0153] Regenerated molding base materials which, in addition to the quartz sand used, also contain small amounts of solidified water glass and particulate, amorphous silicon dioxide, preferably residues of pyrogenic, particulate, amorphous silicon dioxide, are not chemically contaminated by these components or are only insignificantly contaminated, since these components have the same or at least very similar chemical compositions. In contrast, molding base materials other than quartz sand are contaminated with particularly small amounts of silicon dioxide during each regeneration process, so that the properties and chemical composition of the molding base material change compared to non-regenerated molding base materials.
[0154] Preferred is a method according to the invention (preferably as mentioned above as preferred) in which the curing of the molding compound mixture
[0155] - the formation of the shaped molding compound is accelerated or caused by heating the shaped molding compound, preferably by heating in a heated molding tool, preferably in a heated molding tool at a temperature in the range of 100° C. to 300° C., and / or by gas treatment with hot air, wherein preferably the heating and / or gas treatment is set at 120° C. at least in some regions of the shaped molding compound.
[0156] to 180°C in the range of temperature,
[0157] - promoted or caused by saponification of an ester, wherein preferably at least one ester is selected from: intramolecular or intermolecular reaction products of an alcohol and an acid, wherein
[0158] The alcohol is selected from the group consisting of C1-C8 monohydric alcohol, C1-C8 dihydric alcohol, preferably C2-C8 dihydric alcohol, and C1-C8 trihydric alcohol, preferably C3-C8 trihydric alcohol, preferably selected from the group consisting of ethylene glycol, 1,2-propylene glycol and glycerol,
[0159] as well as
[0160] The acid is selected from organic C2-C8 monocarboxylic acids, organic C2-C8 dicarboxylic acids, organic C2-C8 tricarboxylic acids, preferably organic C4-C8 tricarboxylic acids and inorganic acids, preferably selected from formic acid, acetic acid, propionic acid, lactic acid, oxalic acid, succinic acid, malonic acid, phosphoric acid, sulfuric acid, boric acid and carbonic acid,
[0161] Preferably, at least one ester is propylene carbonate or γ-butyrolactone,
[0162] or
[0163] - promoted or caused by gassing the shaped molding compound mixture with a gas or a gas mixture which contains less than 1 mol % of CO2.
[0164] The correspondingly preferred method according to the invention can be carried out particularly easily, reliably and using established methods and furthermore allows the production of casting molds and cores having particularly favorable disintegration properties and particularly favorable reproducibility.
[0165] The curing of the molding compound mixture can be accelerated or caused by heating the shaped molding compound mixture, because water is removed from the molding compound mixture by the increased temperature and, if necessary, by a hot air stream. Since water is one of the products of the cross reaction of water glass, according to Le Chatelier's principle, the chemical equilibrium of the cross reaction is shifted to the side of the condensed water glass, that is, the side of the solidified water glass, so that the curing of the molding compound mixture is accelerated or caused.
[0166] The curing of the molding compound mixture can also be accelerated or initiated by saponification of the ester. The saponification reaction also removes byproducts of the condensation reaction of the water glass from the chemical equilibrium, which is thus shifted according to the Le Chatelier principle towards condensed water glass, ie, solidified water glass.
[0167] Furthermore, water present in the molding compound mixture or water produced during the condensation of water glass can also be removed by gassing the shaped molding compound mixture with a gas or a gas mixture, thereby accelerating or initiating curing as described above. However, it should be noted in this case that the gas or gas mixture used contains less than 1 mol % CO2, i.e., the curing is not carried out according to the CO2 method, but in the manner according to the invention.
[0168] The advantage of the preferred method according to the invention is that it can be used to promote or cause the solidification of the molding material mixture in a particularly effective manner without reducing the disintegration properties and in particular the reproducibility of the castings and cores produced by means of the method. The advantages of the method according to the invention are particularly evident in comparison with methods for solidifying the molding material mixture using the CO2 method. Such castings and cores produced by solidifying the molding material mixture by means of the CO2 method show significantly poorer reproducibility, which is presumably due to the formation of alkali metal carbonates during the solidification process, which subsequently makes the recovery of the advantageously regenerated molding base material, i.e. the regenerated molding base material that can be used again in the production of the castings and cores, impossible or significantly more difficult.
[0169] In other words, preference is also given to a method according to the invention (preferably as indicated above) in which the curing of the molding compound mixture
[0170] - is not promoted or caused by gassing of the shaped molding compound mixture by means of a gas treatment device with the aid of a gas or a gas mixture which contains more than 1 mol % of CO2,
[0171] and / or
[0172] - Not promoted or induced by CO2 methods.
[0173] Preferred is a method according to the invention (preferably as referred to above as preferred), in which the produced casting mold or the produced core is temporarily heated to a temperature of >900° C. at least in some areas, so that the subsequent disintegration is simplified, preferably heating to a temperature of <1600° C., particularly preferably heating to a temperature in the range between 900° C. and 1600° C.
[0174] The corresponding method according to the invention is preferred because the improved disintegration properties of the molds and cores that can be produced by means of the method according to the invention are particularly evident when the molds and cores are temporarily heated at least in some regions during the casting process to a temperature of >900° C., wherein the temperature is preferably less than 1600° C. This means that the produced casting mold or core is preferably temporarily heated at least in some regions to a temperature in the range between 900° C. and 1600° C.
[0175] Even if the technical effect of the invention also manifests itself outside the temperature range specified, the temperature range specified is still preferred, because if the molds and cores are not temporarily heated to temperatures >900° during the manufacturing process at least in some areas, then the disintegration properties of the molds and cores are sometimes considered to be less problematic in practice after all, because sintering occurs to a lesser extent at lower temperatures or a melt phase is formed in the mold or core, which is generally considered to be the (common) cause for unfavorable disintegration properties. At temperatures above 1600° C., which are of only minor significance in casting practice, it can sometimes also be observed that the disintegration of the molds and cores is less problematic, so that an absolute improvement in the disintegration properties occurs less frequently. Therefore, within the temperature range specified, the advantages of the method according to the invention are particularly evident.
[0176] The reason for this is that the advantages of the method according to the invention with regard to the improved disintegration at temperatures >900° C. are particularly pronounced, presumably due to thermally induced processes in the molding compound mixture which take place at corresponding temperatures.
[0177] The casting mold or core produced by the method according to the invention is usually temporarily heated to the temperatures specified above (>900° C.; <1600° C.) by contact with the metal melt during casting. Therefore, preference is given to the method according to the invention (preferably as described above as preferred) in which the produced casting mold or the produced core is temporarily heated at least in some regions to a temperature of >900° C. by contact with the metal melt during the casting process, so that subsequent disintegration is simplified, wherein heating to a temperature of <1600° C. is preferred, particularly preferably to a temperature in the range between 900° C. and 1600° C.
[0178] The prerequisite for heating the casting mold or the core with a molten metal is that the temperature of the molten metal is sufficiently high. Typical molten metals processed at correspondingly high temperatures are molten metals consisting of iron, iron alloys, steel, steel alloys, brass or brass alloys.
[0179] Correspondingly preferred is a method according to the invention (preferably as indicated above as preferred) in which a metal melt is used which consists of iron, an iron alloy, steel, a steel alloy, brass or a brass alloy.
[0180] The correspondingly preferred method according to the invention is therefore particularly advantageous because the use of given metal melts has hitherto often resulted in particularly poor disintegration properties of the casting molds or cores used, in particular when using molding material mixtures containing water glass, so that in these cases the method according to the invention results in a particularly large absolute improvement in the disintegration properties and in some cases it makes sense overall to use water glass-bonded casting molds and cores in this casting process.
[0181] Preference is given to a method according to the invention (preferably as referred to above as preferred) in which the solidified, shaped molding compound mixture is completely or partially provided with a coating of a refractory coating composition, wherein the total amount of solid particles contained in the refractory coating composition is d 90 The value is preferably less than 200 μm, wherein the refractory coating composition is preferably a water-based refractory coating or an alcohol-based refractory coating, particularly preferably a water-based refractory coating.
[0182] The corresponding method according to the invention is preferred, since the use of casting molds and cores in cast iron generally requires that the casting molds or cores are completely or at least partially provided with a coating of a refractory coating composition. Advantageously, corresponding coated casting molds and cores can be produced by means of the method according to the invention without thereby significantly affecting the effects and advantages associated with the invention.
[0183] Refractory coatings are suspensions of fine-grained, refractory to highly refractory inorganic materials in a carrier liquid such as water or alcohol. In the first case, the person skilled in the art speaks of water-based refractory coatings, while in the second case he speaks of alcohol-based refractory coatings. The refractory coating is applied to the mold or the core by a suitable application method, such as spraying, dipping, flow coating or brushing, and dried there, so that a coating with the refractory coating composition is produced.
[0184] Advantageously, the still uncoated casting molds and cores produced by the method according to the invention are particularly resistant to water and air moisture, so that water-based refractory coatings can also be used for coating the casting molds and cores without losing the advantageous basic strength and good disintegration properties of the casting molds and cores. The use of water-based refractory coatings is particularly advantageous because they are more environmentally compatible than alcohol-based refractory coatings and result in a smaller load on the working space during discharge.
[0185] With regard to the reproducibility of molds and cores, the necessity for a mold and core coating for a particular application is generally considered disadvantageous, since the refractory coating differs from the cured molding base mixture in its material composition, but can only be separated from it again with difficulty after the disintegration of the mold or core, so that the regenerated molding base can be contaminated with components of the refractory coating composition. This effect is all the more pronounced the more frequently the molding base is regenerated.
[0186] It has been confirmed that when the total amount of solid particles contained in the refractory coating composition is d 90 At values of less than 200 μm, the reproducibility of the coated casting molds and cores produced in the method according to the invention is improved. It has been shown that, in particular, molding base materials with a particle size of >200 μm, as is usually present in "coated" casting molds and cores produced in accordance with the method according to the invention, can be separated from the components of the refractory coating composition particularly easily during regeneration, wherein the same separation method can advantageously be used as is also used to separate the other components of the molding material mixture used for production, in particular the particulate phyllosilicate used, from the molding base material to be regenerated. Preferably, the separation of the components of the refractory coating composition is carried out by physical separation, particularly preferably by physical dust separation.
[0187] Preferred is the method according to the invention (preferred as described above as preferred), in order to prepare a regenerated molding base material from the finished casting mold or the finished core after heating, the method has the following additional steps:
[0188] - mechanical action on the produced casting mould or the produced core, so that the casting mould or the core collapses,
[0189] - Preparation of a regenerated moulding base from the disintegrated casting mould or the disintegrated core, preferably including separation and removal of dust, wherein the separation preferably includes physical separation.
[0190] The corresponding preferred method according to the invention is advantageous because it allows the production of a recycled basic molding compound from a produced casting mold or a produced core in a particularly simple manner and in a method that can be easily automated.
[0191] A regenerated molding base material of particularly advantageous quality, i.e. particularly suitable for reuse in the method for producing molds and cores, is only obtained when the preparation of the regenerated molding base material includes the separation and removal of dust. The term "dust" here refers to all particles with a diameter of <200 μm. This means that in particular the fraction of the particulate sheet silicate used in the molding material mixture according to the invention is separated, but if necessary also other components contained in the dust, such as solid particles of a refractory coating composition, with a particle size of <200 μm are separated.
[0192] The separation and removal of dust preferably comprises a physical separation of the dust. This can be done, for example, by washing away the dust. However, it is particularly preferred that the physical separation is carried out by air separation, i.e. the dust is separated from other components in the gas stream. A corresponding method is preferred, since air separation can be integrated particularly easily into a molding base material recycling system and results in a particularly thorough separation of the dust. It is also advantageous that the regenerated molding base material obtained is not contaminated by the method and, for example, does not require a drying step.
[0193] Preference is given to a method according to the invention (preferably as indicated above as preferred) in which the molding compound mixture provided or prepared contains a proportion of recycled molding base compound, which was prepared according to the method indicated above as preferred.
[0194] The method according to the invention, which is preferred in this regard, is therefore particularly advantageous, since surprisingly good strength and excellent disintegration properties are also exhibited for such produced castings and cores, wherein the molding compound mixture provided or prepared according to the method according to the invention already contains a certain proportion of a molding base material that is recycled in the manner according to the invention. In other methods known from the prior art, the use of recycled molding base materials is considered disadvantageous in certain cases, and if the ecological and economic advantages of using recycled molding base materials are to be utilized, then losses in strength and disintegration properties of the castings and cores must be accepted.
[0195] In particular, the preferred method according to the invention has the following advantages: by using a recycled molding base material, the reproducibility of the produced casting molds and cores is not or only slightly impaired compared to the methods known from the prior art, so that the method according to the invention can be configured particularly easily in such a way that it includes a molding base material cycle, i.e. a molding base material recycling system. This means that the quality deterioration of the molding base material that increases with each reuse is advantageously particularly small. In particular, the method according to the invention can advantageously obtain a recycled molding base material whose chemical composition is particularly similar to the chemical composition of the corresponding unused molding base material.
[0196] Preferred is the method according to the invention (preferred as referred to above as preferred),
[0197] wherein the molding of the molding material mixture and / or the curing of the molding material mixture is carried out by means of a 3D printer,
[0198] and / or
[0199] The molding of the molding compound mixture takes place in a 3D printing method, and the curing of the molding compound mixture takes place during and / or after the 3D printing process.
[0200] The corresponding preferred method according to the invention is advantageous since the production of casting molds and cores by means of a 3D printer and / or in a 3D printing method allows the production of casting molds and cores which have complex geometries and which have a particularly uniform structural structure and a particularly uniform distribution of the components in the formed molding material mixture.
[0201] The casting molds and cores produced by means of the corresponding preferred method according to the invention advantageously exhibit no or only slight inhomogeneities or concentration gradients in the shaped and / or solidified molding compound mixture, which could lead to undesired agglomerations or to locally reduced disintegration properties.
[0202] The disintegration behavior of the respective casting molds and cores is therefore particularly uniform, constant and reproducible, regardless of the complexity of their geometry, thereby advantageously achieving a high degree of process reliability during the production of the casting molds and cores.
[0203] Furthermore, the reproducibility of the corresponding casting molds and cores is particularly high, since, due to their homogeneous composition, even under slight mechanical loads they are able to produce particularly fine-grained disintegration products which have a very low proportion of agglomerated molding base material particles which otherwise form, for example, due to locally particularly high concentrations of binder or locally particularly low molar moduli of water glass.
[0204] The invention also relates to a mixture for use in combination with a solution or dispersion containing water glass for producing a casting mold and / or a core, the mixture comprising:
[0205] - 10 to 98% by weight of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide,
[0206] - 0 to 15% by weight of graphite,
[0207] one or more particulate, mixed metal oxides, each comprising at least one aluminum oxide and / or at least one zirconium oxide in a total amount of 0% to 80% by weight,
[0208] and to simplify the disintegration of the mold or core and / or to improve reproducibility,
[0209] - one or more particulate layered silicates, in a total amount of 2% to 80% by weight, wherein d 90 The value is less than 45μm,
[0210] The percentages stated herein are based on the total amount of the mixture.
[0211] The corresponding mixture is advantageous because the molding material mixture to be prepared or provided according to the method according to the invention can be prepared particularly simply by combining the mixture according to the invention with a solution or dispersion containing water glass and a molding base material. Surprisingly, the corresponding mixture according to the invention is also particularly storage-stable.
[0212] Preference is given to mixtures according to the invention comprising:
[0213] 25 to 95% by weight, preferably 40 to 95% by weight, of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide,
[0214] - 1.5 to 12.5% by weight, preferably 1.5 to 6% by weight, of graphite,
[0215] one or more particulate, mixed metal oxides, each comprising at least one aluminum oxide and / or at least one zirconium oxide in a total amount of 0% to 65.5% by weight, preferably 0% to 45% by weight,
[0216] - one or more particulate layered silicates in a total amount of 5 to 50% by weight, preferably 15 to 50% by weight, wherein d 90 The value is less than 45μm,
[0217] The percentages stated herein are based on the total amount of the mixture.
[0218] This preferred mixture according to the invention is advantageous because the flowability of the mixture and its processability are particularly high. A corresponding mixture according to the invention can be transported particularly easily via pipelines, especially in continuously operating plants.
[0219] Preferably, the mixture according to the invention (preferably as mentioned above as preferred) additionally comprises one or more compounds selected from the group consisting of: surface-active substances, oxidized boron compounds, phosphorus compounds, carbohydrates, silanes, lithium compounds, particulate aluminum oxide, particulate aluminum / silicon mixed oxides without phyllosilicate structure and barium sulfate,
[0220] The surface active substance is preferably selected from: anionic surfactants, nonionic surfactants, cationic surfactants, amphoteric surfactants and mixtures thereof,
[0221] The oxidized boron compound is preferably selected from the group consisting of borates, boric acid, boric anhydride, borosilicates, borophosphates, borophosphosilicates and mixtures thereof,
[0222] The phosphorus compound is preferably selected from: organic phosphates, inorganic phosphates and mixtures thereof,
[0223] The carbohydrate is preferably selected from the group consisting of oligosaccharides, polysaccharides and mixtures thereof, preferably selected from the group consisting of cellulose, starch, dextrin and mixtures thereof,
[0224] The silane is preferably selected from the group consisting of aminosilane, epoxysilane, mercaptosilane, hydroxysilane, ureasilane and mixtures thereof.
[0225] The lithium compound is preferably selected from the group consisting of amorphous lithium silicate, lithium oxide, lithium hydroxide and mixtures thereof.
[0226] The corresponding preferred mixtures according to the invention are advantageous because the preferred molding material compounds according to the invention for the method according to the invention can be prepared particularly easily with the aid of these mixtures, and the presence of the compounds listed does not have a negative effect on the durability and processability of the mixture. In this regard, the above statements about the preferred components of the molding material mixtures to be used according to the invention and about their corresponding advantages can be applied accordingly, mutatis mutandis.
[0227] It is particularly advantageous in this context that when using corresponding mixtures, the individual components do not need to be stored and handled separately, but can be added to the molding compound mixture to be produced according to the invention in the form of a single component, ie as a preferred mixture according to the invention.
[0228] Preferred are mixtures according to the invention (preferably as mentioned above as preferred), wherein the mixture is a solid mixture or a dispersion consisting of two or more phases.
[0229] Particularly preferred here are mixtures according to the invention (preferably as indicated above as preferred), wherein the mixture is a dispersion composed of two or more phases.
[0230] In the respective mixture according to the invention, at least one phase is a liquid phase. This can advantageously influence the processing properties of the respective preferred mixture according to the invention, since the mixture can be particularly easily conducted through a pipeline by means of a pump system, which is advantageous in particular for large-scale and possibly continuously operated plants. Furthermore, the respective mixture is particularly advantageous with regard to occupational safety and health, since the respective mixture does not generate dust and thus does not cause a fine and ultrafine dust load in the working space during processing, so that the risk of respiratory diseases can be advantageously minimized.
[0231] Furthermore, the corresponding preferred mixtures according to the invention can be mixed particularly easily, quickly and completely with the other components of the molding compound mixture to be used in the method according to the invention, so that a particularly homogeneous molding compound mixture without concentration gradients is obtained. It is particularly advantageous if, when using the corresponding mixtures, the water-soluble components of the molding compound mixture can already be incorporated in dissolved form, thereby avoiding local concentration gradients in the molding compound mixture due to slow and / or incomplete dissolution.
[0232] The invention further relates to a multi-component adhesive system comprising components which are spatially separate or mixed with one another,
[0233] (A) The mixtures according to the invention are as defined above, preferably as indicated above as preferred,
[0234] (B) a solution or dispersion comprising:
[0235] The water glass preferably has a molar modulus SiO2 / M2O in the range from 1.6 to 4.0, preferably in the range from 1.8 to 2.5, wherein M2O represents the total amount of lithium oxide, sodium oxide and potassium oxide.
[0236] The corresponding multi-component adhesive system according to the invention is advantageous because the molding material mixture to be prepared in the method according to the invention, in particular also the preferred molding material mixture, can be prepared particularly easily with the aid of the multi-component adhesive system. In this regard, the above-mentioned embodiments regarding the preferred components of the molding material mixture to be used according to the invention and their corresponding advantages can be applied accordingly after necessary modifications. When used by the end consumer, that is, in the foundry applying the method according to the invention, the corresponding multi-component adhesive system is particularly advantageous because it can be handled and processed particularly easily and reliably to form the molding material mixture to be used in the method according to the invention, and is particularly not prone to errors, for example in dosing. Preferably, the multi-component adhesive system according to the invention contains components as components that are mixed with each other for this reason, thereby further minimizing the sensitivity to errors at the end user.
[0237] Preferred are multi-component adhesive systems according to the invention (preferably as indicated above as preferred) which comprise in component (B) and / or in further component (C) one or more compounds selected from the group consisting of: surface-active substances, oxidized boron compounds, phosphorus compounds, carbohydrates, silanes and lithium compounds,
[0238] The surface active substance is preferably selected from: anionic surfactants, nonionic surfactants, cationic surfactants, amphoteric surfactants and mixtures thereof,
[0239] The oxidized boron compound is preferably selected from the group consisting of borates, boric acid, boric anhydride, borosilicates, borophosphates, borophosphosilicates and mixtures thereof, and particularly preferably selected from the group consisting of alkali metal and alkaline earth metal borates, wherein the oxidized boron compound preferably contains no organic group.
[0240] The phosphorus compound is preferably selected from: organic phosphates, inorganic phosphates and mixtures thereof,
[0241] Preferably selected from inorganic alkali metal phosphates,
[0242] The carbohydrate is preferably selected from the group consisting of oligosaccharides, polysaccharides and mixtures thereof, preferably selected from the group consisting of cellulose, starch and dextrin,
[0243] The silane is preferably selected from the group consisting of aminosilane, epoxysilane, mercaptosilane, hydroxysilane, ureasilane and mixtures thereof,
[0244] The lithium compound is preferably selected from the group consisting of amorphous lithium silicate, lithium oxide, lithium hydroxide and mixtures thereof.
[0245] The corresponding preferred multi-component adhesive system according to the invention is advantageous because it allows the preferred molding compound mixture or the molding compound mixture for the preferred method according to the invention to be obtained in a particularly uncomplicated and reliable manner. In this regard, the above statements about the preferred components of the molding compound mixture to be used according to the invention and their corresponding advantages can be applied accordingly, mutatis mutandis.
[0246] The present invention also relates to a molding compound mixture, which comprises:
[0247] - at least components (A) and (B) as defined above
[0248] as well as
[0249] - Refractory moulding bases as component (D).
[0250] The corresponding molding compound mixtures according to the invention are preferred since they can be used directly and without further processing steps in the method according to the invention and can be processed to give casting molds and cores having excellent disintegration properties and very good reproducibility.
[0251] Preferred is a molding compound mixture according to the invention (preferably as mentioned above as preferred) which comprises:
[0252] Recycled molding base material as refractory molding base material or as a component of a refractory molding base material, wherein the recycled molding base material can preferably be produced by the process according to the invention.
[0253] The correspondingly preferred molding compound mixtures according to the invention are advantageous for reasons of durability, conservation of resources and avoidance of waste, and also from an economic point of view.
[0254] The particularly preferred design scheme for preparing recycled molding base material by the method according to the invention is particularly advantageous, because with the help of the corresponding recycled molding base material, the advantages of the method according to the invention can be achieved even when the molding base material is recycled multiple times from the produced casting molds and cores, that is, even when a molding base material recycling system is used.
[0255] Preferred are molding compound mixtures according to the invention (preferably as described above as preferred), in which
[0256] the water glass has a molar modulus SiO2 / M2O in the range from 1.6 to 4.0, preferably in the range from 1.8 to 2.5, wherein M2O denotes the sum of lithium oxide, sodium oxide and potassium oxide, and / or
[0257] The basic molding compound used comprises quartz sand, preferably at least 50% by weight, particularly preferably at least 80% by weight, based on the total amount of the basic molding compound.
[0258] The corresponding molding compound mixture according to the invention is preferred because it can be used directly and without further processing steps in the preferred method according to the invention. In this regard, the above statements about the preferred components of the molding compound mixture to be used according to the invention and their corresponding advantages can be applied accordingly, mutatis mutandis.
[0259] The invention further relates to a molding base mixture comprising:
[0260] (X) 0 to 99% by weight, preferably 0 to 90% by weight, of a novel molding base material,
[0261] and
[0262] (Y) 1 to 100 wt. %, preferably 10 to 100 wt. %, of recycled molding base material,
[0263] The percentages are based on the total amount of the molding base material mixture.
[0264] and
[0265] The recycled molding base material (Y)
[0266] - can be prepared by the process according to the invention.
[0267] The corresponding molding base material mixture according to the invention is advantageous because it can be used as a molding base material in the molding material mixture according to the invention and in the method according to the invention and contains at least 1% by weight, preferably at least 50% by weight, and particularly preferably at least 70% by weight of recycled molding base material, which is advantageous from the above-mentioned ecological and economic perspectives.
[0268] With the aid of a corresponding molding base material mixture according to the invention, it is possible to produce casting molds and cores in the method according to the invention which have very good disintegration properties and again high reproducibility. In this case, the fact that the casting molds and cores are produced from a molding base material which according to the invention at least partially already consists of a recycled molding base material advantageously has no or only a slight influence on the strength, disintegration properties and reproducibility of the produced casting molds and cores.
[0269] The invention also relates to a casting mould or a core,
[0270] - can be produced by a process according to the invention as defined above,
[0271] and / or
[0272] - comprising a mixture according to the invention as defined above,
[0273] and / or
[0274] - comprising a cured multi-component adhesive system according to the invention as defined above,
[0275] and / or
[0276] - comprising a molding compound mixture according to the invention as defined above,
[0277] and / or
[0278] - comprising a moulding base mixture according to the invention as defined above.
[0279] As explained above for the method according to the invention, the corresponding casting molds or cores according to the invention have good strength and particularly advantageous disintegration properties as well as high reproducibility. In this regard, the above descriptions of the preferred components of the molding material mixture to be used according to the invention and their corresponding advantages can be applied accordingly after necessary modifications.
[0280] The present invention also relates to a certain amount of d 90 The use of a particulate sheet silicate having a value of less than 45 μm or of a mixture according to the invention as defined above as an additive for the preparation of or in a molding mixture comprising water glass and particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide, which is cured by chemical reaction of the components of the molding mixture with one another,
[0281] When making a mold or core,
[0282] For simplifying the disintegration of casting molds or cores and / or increasing reproducibility. In this regard, the above descriptions of the preferred mixtures according to the invention and their corresponding advantages also apply accordingly after necessary modifications. Through the use according to the invention, as explained above for the method according to the invention, casting molds and cores can be obtained, which have good strength and particularly advantageous disintegration characteristics and high reproducibility.
[0283] Preferred is the use according to the invention (preferred as mentioned above) in which
[0284] the water glass has a molar modulus SiO2 / M2O in the range from 1.6 to 4.0, particularly preferably in the range from 1.8 to 2.5, wherein M2O denotes the sum of lithium oxide, sodium oxide and potassium oxide,
[0285] and / or
[0286] - the basic molding material used in the production of the casting mold or core contains quartz sand, preferably at least 50% by weight, particularly preferably at least 80% by weight, based on the total amount of the basic molding material,
[0287] and / or
[0288] - When making a casting mold or a core, the curing of the molding compound mixture
[0289] - promoted or caused by heating the shaped molding compound mixture, preferably by heating in a heated molding tool and / or by air treatment with hot air, wherein preferably a temperature in the range of 120° C. to 180° C. is set by heating at least in some regions of the shaped molding compound mixture,
[0290] - promoted or caused by saponification of an ester, wherein the ester is preferably selected from the group consisting of ethylene glycol diacetate, diacetin, triacetin, propylene carbonate and gamma-butyrolactone,
[0291] or
[0292] - promoted or caused by gassing the shaped molding compound mixture with a gas containing less than 1 mol % CO2.
[0293] The corresponding preferred use according to the invention is advantageous because in the corresponding use, as explained above for the method according to the invention, a surprising improvement in the disintegration properties of the produced casting molds and cores and an improvement in the reproducibility are particularly evident. With regard to the advantages of the use according to the invention, which are here referred to as preferred embodiments, the above descriptions of the preferred method and its corresponding advantages apply accordingly, mutatis mutandis.
[0294] Examples:
[0295] The present invention is described in detail below with reference to examples.
[0296] Examples V1-V5 and E1-E5:
[0297] 1. Composition and sample preparation:
[0298] First, a total of five cores according to the invention, produced by means of the method according to the invention from the molding material mixtures according to the invention (E1 to E5), and five non-inventive comparative examples (V1 to V5) were investigated. The composition of the respective molding material mixtures used to produce the respective cores is summarized in Table 1.
[0299] Table 1: Composition of the molding compound mixtures used. All values are given in parts by weight.
[0300]
[0301] a) Quartz sands (coarse foundry silicasand 1K 0.20 / 0.315 / 0.40) from Grudzen Las were used as the basic molding materials.
[0302] b) Alkaline water glass having a molar modulus SiO2:M2O (M2O=total amount of Na2O and Li2O) of 1.95 and a solids content of 35% by weight was used in each case as binder.
[0303] c) In each case a mixture of 95.625 parts by weight of pyrogenic, particulate, amorphous silicon dioxide (CAS RN 69012-64-2) and 4.375 parts by weight of graphite was used as additive.
[0304] d) Used as silicate in the examples according to Table 1:
[0305] Silicate-1:d 90 Pyrogenic, granular layered silicate with a particle size of <45 μm (from Werba-Chem GmbH under the trade name MK-I);
[0306] Silicate-2:d 90 Natural particulate layered silicate (halloysite) with a particle size of <45 μm (from Osthoff Omega Group, trade name Halloysite JM1 mineral pigment);
[0307] Silicate-3:d 90 Synthetic granular layered silicate with a particle size of <45 μm (from BYK Additives & Instruments GmbH, trade name RDS);
[0308] Silicate-4:d 90 Thermally activated granular layered silicate (metakaolin) with a particle size of <45 μm
[0309] (from BASF SE under the trade name );
[0310] Silicate-5:d 90 Natural, particulate layered silicate (montmorillonite) with a particle size of <45 μm (from Alfa Aesar / Thermo Fischer (Kandel) GmbH under the trade name Montmorillonite K10).
[0311] Silicate-X:d90 Natural island silicate (andalusite) with a value of <45 μm (from Eggerding B.V. Industrial Minerals, trade name andalusite 200 mesh); (Note: not granular layered silicate)
[0312] Silicate-Y:d 90 Natural layered silicate (montmorillonite) with a particle size of >45 μm (from Damolin LLC, trade name Sorbix US Premium (0.3-0.7 mm)). (Note:
[0313] d 90 value is not less than 45μm)
[0314] As disclosed in VDG Data Sheet M11 of March 1974, the test specimens were produced by injection molding from the molding compound mixtures given in Table 1 using a heatable forming tool for producing bending rods. On the one hand, bending rods with the dimensions of 22.4 mm×22.4 mm×165 mm were produced, which provided the basis for subsequent investigations into the bending strength, and on the other hand, cylindrical test specimens with a height of 50 mm and a diameter of 50 mm were produced, which were used to determine the disintegration properties.
[0315] To this end, the components listed in Table 1 were mixed in a laboratory blade mixer (Multiserw). For this purpose, quartz sand was first charged and powdered additives and, if necessary, silicates were mixed in. Then the binder was added. The mixture was then stirred for a total of two minutes. The molding material mixture was introduced into a molding tool with the aid of compressed air (4 bar), the core box temperature of which was 180° C. The injection time was 3 s, followed by a hardening time of 30 s (delay time of 3 s). In order to accelerate the curing of the mixture, hot air (gas treatment pressure of 2 bar, gas treatment temperature and gas treatment hose temperature of 150° C.) was guided through the molding tool during the 30 s hardening time.
[0316] 2. Determine the bending strength:
[0317] To determine the flexural strength, the produced test bars were placed in a Georg Fischer strength tester equipped with a three-point bending device (Multiserw) and the force that causes the test bars to break was measured. The flexural strength (so-called cold strength) was measured 1 hour after removal from the forming tool. The measured values obtained are given in Table 2 under the entry "Flexural strength" as the median of 3 measurements.
[0318] 3. Study the disintegration characteristics:
[0319] To investigate the disintegration behavior, cylindrical specimens with a height of 50 mm and a diameter of 50 mm were subjected to thermal loading at a temperature of 900° C. for 10 minutes in a muffle furnace (Nabertherm). After the sample was removed from the muffle furnace and cooled to room temperature, it was placed on a vibrating sieve with a mesh width of 1.40 mm (the sieve was placed on an oscillating vibrator LPzE-3e from Multiserw) and then vibrated for 60 seconds with the greatest possible amplitude (100% of the maximum possible setting of the device). The amount of residue on the sieve and the amount of crushed material (disintegrated portion) in the collecting tray were determined respectively with the aid of a scale. The quotient of the weight of the disintegrated portion and the total amount of the two portions is referred to as the sieve throughput and is given in Table 2 under the entry “sieve throughput” as the average value of each of 4 measurements. Improved disintegration behavior is particularly evident at high values of the sieve throughput.
[0320] 4. Determine the quality of the recycled molding base material:
[0321] The quality of the regenerated molding base and its suitability for use in the production of waterglass-bonded casting molds and cores having good disintegration properties is particularly good when the concentration of water-soluble salts and oxides, in particular water-soluble alkali metal salts and alkali metal oxides, in the regenerated molding base is particularly low. This property can be checked by means of conductivity measurements.
[0322] 4.1 For each measurement, first, to prepare the initial solution, 100 mL of ultrapure water was introduced into a beaker and 0.05 mL of 1 M KCl solution was added. The conductivity of the initial solution obtained was determined using a pH / conductivity meter SevenMulti from Mettler Toledo; the conductivity corresponds to the blank value.
[0323] 4.2 To produce the regenerated molding base material, the corresponding bent bars with the dimensions of 22.4 mm×22.4 mm×165 mm were respectively subjected to thermal loading at a temperature of 900° C. in a muffle furnace (Nabertherm) for 5 minutes. After the sample was removed from the muffle furnace and after cooling to room temperature, the sample was placed in a free-flowing state by manual mechanical action. 50 g of the respectively produced regenerated molding base material were introduced into a beaker with the initial solution (see 4.1 above) without further treatment, and the beaker was then covered with a bell glass. The suspension obtained was heated to 100° C. on a hot plate, left at this temperature for 5 minutes, and then cooled to room temperature. The solid content of the suspension was separated by filtration, and the conductivity of the filtrate obtained was determined as described above in 4.1. In Table 2, under the entry "Conductivity", the following values are given, which are obtained as the average value of each of 4 measurements for the difference between the determined conductivity and the blank value determined previously.
[0324] 4.3 The quality of the regenerated molding base can also be assessed by determining the acid requirement (see VDG data sheet October 1999, page 26). The acid requirement was determined for the selected samples according to the provisions of VDG data sheet October 1999, page 26, wherein the regenerated molding base used was prepared as described in 4.2. In Table 2, under the heading "Acid requirement", the following values are given, which are calculated as average values of 4 measurements in each case.
[0325] 4.4 Measurement values and conclusions:
[0326] Table 2: Measurement values
[0327]
[0328] 4.4.1 It can be seen from the table that with the method according to the invention it is possible to obtain casting moulds and cores having good bending strength.
[0329] 4.4.2 Table 2 clearly shows that for all examples produced by means of the method according to the invention, excellent sieve throughputs (as a measure of the disintegration properties) of 95% to 100% were measured, which are all significantly higher than the sieve throughputs of 8% to 76% determined for the comparative examples.
[0330] In particular, it is shown here that the use of only particulate sheet silicate (Example V3, without (pyrogenic) particulate, amorphous silicon dioxide) and the use of only (pyrogenic), particulate, amorphous silicon dioxide (Example V2, without particulate sheet silicate) do not lead to a significant increase in the sieve throughput as in the compositions according to the invention (Examples E1 to E5). In the examples according to the invention, there is a synergistic effect, which is particularly clear in that the sieve throughput of the combination of Examples V2 and V3 is also only 77%, which is significantly lower than the minimum value determined for Examples E1 to E5.
[0331] Furthermore, a comparison of Examples E1 to E5 with Example V4 clearly shows that advantageous technical effects are achieved only with granular sheet silicates and that the use of island silicates such as andalusite (Silicate X) leads to significantly worse sieve throughputs.
[0332] In addition, a specific comparison between Example E4 and Example V5 shows that only the 90 While a granular phyllosilicate of a value of 1.3 Å yields a technical effect, a coarse-grained embodiment of a chemically identical phyllosilicate (silicate Y in example V5) results in a significantly worse sieve throughput.
[0333] Furthermore, it is clearly visible that for all granular silicates examined (Examples E1 to E5), the technical effect of an improved sieve throughput is demonstrated, without regard being paid to chemical differences between the granular silicates used.
[0334] 4.4.3 The quality of the resulting recycled molding base material can also be assessed with the aid of the conductivity value, with a low conductivity being advantageous.
[0335] Table 2 clearly shows that for all examples produced by means of the method according to the invention, low conductivities of 790 to 1420 μS / cm were measured, which are all significantly lower than the high conductivities of 1870 to 3340 μS / cm determined for the comparative examples.
[0336] It is shown here that the use of only particulate sheet silicate (Example V3, without (pyrogenic) particulate, amorphous silicon dioxide) and the use of only (pyrogenic) particulate, amorphous silicon dioxide (Example V2, without particulate sheet silicate) both lead to such a significant reduction in the electrical conductivity as the combination according to the invention (Examples E1 to E5). In particular, the use of only (pyrogenic) particulate, amorphous silicon dioxide (Example V2) even leads to an increase in the electrical conductivity compared to Example V1 (without amorphous silicon dioxide; without silicate), whereby the synergistic effect of the combination according to the invention (Examples E1-E5) becomes particularly evident.
[0337] Furthermore, a comparison of Examples E1 to E5 with Examples V4 and V5 clearly shows that this advantageous technical effect also only occurs for particulate phyllosilicates, in particular with the d 90 Values of 0.1% are obtained for granular sheet silicates, whereas the use of island silicates (V4; silicate-X) leads to disadvantageously high conductivity values, just as the coarser-grained embodiment using sheet silicates (V5, silicate-Y).
[0338] Furthermore, it is clearly visible that the technical effect of improved sieving throughput is achieved for all of the granular sheet silicates examined (E1 to E5), without regard being paid to the chemical differences between the compounds used.
[0339] 4.4.4 Consideration of the measured values for acid demand summarized in Table 2 shows that acid demand can be directly related to conductivity discussed above in 4.4.3, and that the smaller the acid demand, the smaller the conductivity.
[0340] 4.4.5 In addition to the measured values summarized in Table 2, it has been demonstrated in own studies that the physical separation (sieving) of the dust fraction of the recycled molding compound with a particle size of less than 125 μm leads to a further reduction in the electrical conductivity of 10% up to more than 20% in the case of the molding compound mixtures according to the invention (Examples E2 and E3). In the case of the mixtures not according to the invention (Example V2), the electrical conductivity was reduced by only about 5% after separation.
[0341] 5. Other studies:
[0342] Furthermore, cores produced with the molding compound mixtures according to the invention or comparative molding compound mixtures were investigated. The components of the molding compound mixtures are first associated with abbreviations in Table 3. According to Table 4, the investigated cores were grouped according to their components and qualitatively evaluated with regard to their strength, their disintegration behavior and their reproducibility.
[0343] Table 3: Composition of the molding compound mixture used in the method.
[0344]
[0345] Table 4: Qualitative evaluation of the cores produced from the molding compound mixtures used with respect to their strength, their disintegration behavior and their reproducibility. The symbols here represent: (-) = very poor, (-) = poor, (+) = good and (++) = very good.
[0346]
[0347] The qualitative evaluation in Table 4 shows that only the molding compound mixture or core according to the invention (reference number: F) exhibits very good disintegration behavior and very good reproducibility, and for these at the same time good strength is observed.
[0348] According to an embodiment of the present disclosure, the following additional notes are also disclosed:
[0349] 1. A method for producing a casting mold, a core and a molding base material regenerated therefrom, the method comprising the following steps for producing a casting mold or a core:
[0350] - Providing or producing a molding compound mixture, the molding compound mixture comprising:
[0351] - Moulding base material,
[0352] - a solution or dispersion comprising water glass,
[0353] - 0.1 to 3% by weight of particulate, amorphous silicon dioxide,
[0354] and in order to simplify the disintegration of the casting mold or the core and / or to increase the reproducibility,
[0355] - one or more particulate layered silicates in a total amount of 0.05% to 1.5% by weight, wherein d 90 The value is less than 45μm,
[0356] The percentages are based on the total amount of the molding compound mixture.
[0357] - shaping the molding compound mixture,
[0358] The molding compound mixture is solidified by a chemical reaction of the components of the molding compound mixture with one another, so that the casting mold or the core is produced.
[0359] 2. According to any one of the methods described in the above notes,
[0360] The water glass in the molding compound mixture has a molar modulus SiO 2 / M 2 O in the range of 1.6 to 4.0, preferably in the range of 1.8 to 2.5, wherein M 2 O represents the sum of lithium oxide, sodium oxide and potassium oxide.
[0361] 3. According to any one of the above-mentioned methods,
[0362] The average diameter of the molding base material particles is in the range of 100 μm to 600 μm.
[0363] 4. According to any one of the above-mentioned methods,
[0364] The molding compound mixture contains fumed, granular, amorphous silicon dioxide and / or the granular, amorphous silicon dioxide is fumed, granular, amorphous silicon dioxide.
[0365] 5. According to the method described in Note 1,
[0366] The molding compound mixture contains one or more particulate layered silicates in a total amount of 0.1% to 0.4% by weight, preferably 0.1% to 0.3% by weight, wherein the total amount of the layered silicates is d 90 The value is less than 45μm.
[0367] 6. The method according to any one of the above notes, comprising providing or manufacturing a molding compound mixture, wherein the molding compound mixture comprises:
[0368] - Moulding base material,
[0369] - a solution or dispersion comprising water glass,
[0370] - one or more particulate layered silicates in a total amount of 0.1% to 0.4% by weight, preferably 0.1% to 0.3% by weight, wherein d 90 The value is less than 45μm,
[0371] - 0.3% to 3% by weight, preferably 0.57% to 0.77% by weight, of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide, and
[0372] - 0.01 to 1% by weight of graphite,
[0373] The percentages are respectively based on the total amount of the molding compound mixture.
[0374] 7. According to any one of the above notes,
[0375] The molding base material contains quartz sand, preferably at least 50% by weight, particularly preferably at least 80% by weight, based on the total amount of the molding base material.
[0376] and / or
[0377] The curing of the molding compound mixture
[0378] - is promoted or caused by heating the molded molding compound mixture, preferably by heating in a heated molding tool, preferably in a heated molding tool at a temperature in the range of 100° C. to 300° C., and / or by gas treatment with hot air, wherein preferably by heating and / or gas treatment a temperature in the range of 120° C. to 180° C. is set at least in some regions of the molded molding compound mixture,
[0379] - promoted or caused by saponification of esters, wherein preferably at least one of the esters is selected from: intramolecular or intermolecular reaction products of alcohols and acids, wherein
[0380] The alcohol is selected from the group consisting of C1-C8 monohydric alcohol, C1-C8 dihydric alcohol, preferably C2-C8 dihydric alcohol, and C1-C8 trihydric alcohol, preferably C3-C8 trihydric alcohol, preferably selected from the group consisting of ethylene glycol, 1,2-propylene glycol and glycerol,
[0381] as well as
[0382] The acid is selected from the group consisting of organic C2-C8 monocarboxylic acids, organic C2-C8 dicarboxylic acids, organic C2-C8 tricarboxylic acids, preferably organic C4-C8 tricarboxylic acids, and inorganic acids, preferably selected from the group consisting of formic acid, acetic acid, propionic acid, lactic acid, oxalic acid, succinic acid, malonic acid, phosphoric acid, sulfuric acid, boric acid and carbonic acid,
[0383] Preferably, at least one of the esters is propylene carbonate or γ-butyrolactone,
[0384] or
[0385] - being promoted or caused by gassing the shaped molding compound mixture with a gas or a gas mixture which contains less than 1 mol % of CO2.
[0386] 8. The method according to any one of the above notes, wherein the produced casting mold or the produced core is temporarily heated at least in some areas to a temperature of >900° C., so that subsequent disintegration is simplified, wherein heating to a temperature of <1600° C. is preferred, and heating to a temperature in the range of 900° C. and 1600° C. is particularly preferred,
[0387] and / or
[0388] The produced casting mold or the produced core is temporarily heated to a temperature of >900° C. at least in some regions by contact with a metal melt during casting, so that subsequent disintegration is simplified, preferably heating to a temperature of <1600° C., particularly preferably heating to a temperature in the range of 900° C. and 1600° C., preferably using a metal melt consisting of iron, an iron alloy, steel, a steel alloy, brass or a brass alloy.
[0389] 9. The method according to Supplementary Note 8, in order to produce a regenerated molding base material from the produced casting mold or the produced core after heating, the method has the following additional steps:
[0390] - mechanically acting on the produced casting mold or the produced core so that the casting mold or the core collapses,
[0391] - producing the regenerated moulding base from the disintegrated casting mould or the disintegrated core, preferably including separation and removal of dust, wherein the separation preferably includes physical separation.
[0392] 10. A method according to any one of the above notes,
[0393] wherein the provided or produced molding material mixture contains a proportion of recycled molding base material produced according to supplementary note 9,
[0394] and / or
[0395] wherein the molding of the molding material mixture and / or the curing of the molding material mixture is carried out by means of a 3D printer,
[0396] and / or
[0397] The molding compound mixture is shaped by a 3D printing method, and the molding compound mixture is cured during and / or after the 3D printing process.
[0398] 11. A mixture for use in combination with a solution or dispersion containing water glass for producing a casting mold and / or a core, the mixture comprising:
[0399] - 10 to 98% by weight of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide,
[0400] - 0 to 15% by weight of graphite,
[0401] one or more particulate, mixed metal oxides, each comprising at least one aluminum oxide and / or at least one zirconium oxide in a total amount of 0% to 80% by weight,
[0402] and, in order to simplify the disintegration of the casting mold or the core or to improve reproducibility,
[0403] - one or more particulate layered silicates, in a total amount of 2% to 80% by weight, wherein d 90 The value is less than 45μm,
[0404] The percentages are based on the total amount of the mixture, preferably comprising:
[0405] 25 to 95% by weight, preferably 40 to 95% by weight, of particulate, amorphous silicon dioxide, preferably pyrogenic, particulate, amorphous silicon dioxide,
[0406] - 1.5 to 12.5% by weight, preferably 1.5 to 6% by weight, of graphite,
[0407] one or more particulate, mixed metal oxides, each comprising at least one aluminum oxide and / or at least one zirconium oxide in a total amount of 0% to 65.5% by weight, preferably 0% to 45% by weight,
[0408] - one or more particulate layered silicates in a total amount of 5 to 50% by weight, preferably 15 to 50% by weight, wherein d 90 The value is less than 45μm,
[0409] The percentages are based on the total amount of the mixture.
[0410] The mixture is particularly preferably a solid mixture or a dispersion consisting of two or more phases.
[0411] 12. A multi-component adhesive system comprising components which are spatially separate or mixed with one another,
[0412] (A) the mixture according to Supplementary Note 11,
[0413] (B) A solution or dispersion comprising water glass, preferably water glass having a molar modulus SiO2 / M2O in the range of 1.6 to 4.0, preferably in the range of 1.8 to 2.5, wherein M2O represents the total amount of lithium oxide, sodium oxide and potassium oxide.
[0414] 13. A molding compound mixture, comprising:
[0415] - at least components (A) and (B) as defined in Supplementary Note 12,
[0416] as well as
[0417] - a refractory molding base as component (D),
[0418] Preferably, a recycled basic molding compound is contained as a refractory basic molding compound or as a component of a refractory basic molding compound, wherein the recycled basic molding compound is particularly preferably producible by a method according to supplementary note 9.
[0419] 14. Use of a certain amount of a granular sheet silicate having a d90 value of less than 45 μm or a mixture according to supplementary note 11 as an additive for producing a molding mixture comprising water glass and granular, amorphous silicon dioxide, preferably pyrogenic, granular, amorphous silicon dioxide, the molding mixture being cured by chemical reaction of the components of the molding mixture with one another,
[0420] When making a mold or core,
[0421] To simplify the dismantling of the casting mold or the core and / or to increase the reproducibility.
Claims
1. A mixture for combining with a solution or dispersion containing water glass for producing a casting mold and / or a core, the mixture comprising: - 10 to 98% by weight of particulate, amorphous silicon dioxide, - 0 to 15% by weight of graphite, one or more particulate, mixed metal oxides, each comprising at least one aluminum oxide and / or at least one zirconium oxide in a total amount of 0% to 80% by weight, and, in order to simplify the disintegration of the casting mould or the core and / or to improve reproducibility, - one or more particulate layered silicates, in a total amount of 2% to 80% by weight, wherein d 90 The value is less than 45μm, The percentages are based on the total amount of the mixture.
2. The mixture according to claim 1, The particulate, amorphous silica is fumed, particulate, amorphous silica.
3. The mixture according to claim 1, The percentages are based on the total amount of the mixture, which comprises: - 25 to 95% by weight of particulate, amorphous silicon dioxide, - 1.5 to 12.5% by weight of graphite, - one or more particulate, mixed metal oxides, each comprising at least one aluminum oxide and / or at least one zirconium oxide in a total amount of 0% to 65.5% by weight - one or more particulate layered silicates, in a total amount of 5 to 50% by weight, wherein d 90 The value is less than 45μm.
4. The mixture according to claim 3, The particulate, amorphous silica is fumed, particulate, amorphous silica.
5. The mixture according to claim 3, The mixture comprises 40% to 95% by weight of particulate, amorphous silicon dioxide.
6. The mixture according to claim 3, The mixture comprises 1.5 wt % to 6 wt % graphite.
7. The mixture according to claim 3, The mixture includes a total amount of 0% to 45% by weight of one or more particulate, mixed metal oxides.
8. The mixture according to claim 3, The mixture comprises one or more particulate layered silicates in a total amount of 15% to 50% by weight.
9. The mixture according to claim 1, The mixture is a solid mixture or a dispersion consisting of two or more phases.
10. A multi-component adhesive system comprising spatially separate components, (A) a mixture according to any one of claims 1 to 9, (B) A solution or dispersion comprising water glass.
11. The multi-component adhesive system according to claim 10, The water glass has a molar modulus SiO in the range of 1.6 to 4.0 2 / M 2 O, where M 2 O represents the total amount of lithium oxide, sodium oxide and potassium oxide.
12. The multi-component adhesive system according to claim 11, The water glass has a molar modulus SiO in the range of 1.8 to 2.
5. 2 / M 2 O.
13. A molding compound mixture, comprising: - at least component (A), which is a mixture according to any one of claims 3 to 7, and component (B) as defined in any one of claims 10 to 12, as well as - Refractory moulding bases as component (D).
14. The molding compound mixture according to claim 13, The molding compound mixture contains a recycled molding base compound as a refractory molding base compound or as a component of a refractory molding base compound.
15. The molding compound mixture according to claim 14, The recycled molding base material can be produced by a method comprising the following steps for producing a casting mold or a core: - Providing a molding compound mixture, the molding compound mixture comprising: - Moulding base material, - a solution or dispersion comprising water glass, - 0.1 to 3% by weight of particulate, amorphous silicon dioxide, and in order to simplify the disintegration of the casting mold or the core and / or to increase the reproducibility, - one or more particulate layered silicates in a total amount of 0.05% to 0.4% by weight, wherein d 90 The value is less than 45μm, The percentages are based on the total amount of the molding compound mixture. - shaping the molding compound mixture, - curing of the molding compound mixture by chemical reaction of the components of the molding compound mixture with one another, so that the casting mold or the core is produced, wherein the produced casting mold or the produced core is temporarily heated at least in some regions to a temperature of >900° C., so that subsequent disintegration is simplified, and / or wherein the produced casting mold or the produced core is temporarily heated to a temperature of >900° at least in some regions by contact with the metal melt during casting, so that subsequent disintegration is simplified, and In order to produce a regenerated molding base material from the produced casting mold or the produced core after heating, the method has the following additional steps: - mechanically acting on the produced casting mold or the produced core so that the casting mold or the core collapses, - producing the regenerated molding base material from the disintegrated casting mold or the disintegrated core.
16. Use of a mixture according to any one of claims 1 to 9 as an additive for producing a molding mixture comprising water glass and particulate, amorphous silicon dioxide, which hardens by chemical reaction of the components of the molding mixture with one another, When making a mold or core, To simplify the dismantling of the casting mold or the core and / or to increase the reproducibility.
17. The use according to claim 16, wherein the granular, amorphous silica is fumed, granular, amorphous silica.