Casting method for reducing cracks of boron-containing peritectic steel continuous casting billet
By adjusting the crystallizer parameters and controlling the argon blowing scheme of plug rods, and optimizing the casting machine operation, the problem of skin-curtaining defects of hot-rolled plates is solved, significantly reducing the crack rate and skin-curtaining rate of casting billets, improving product quality and production stability .
Patent Information
- Application Number
- CN202411041310.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
During the steel metallurgical steelmaking process, hot-rolled plate skin defects frequently appear, affecting the product pass rate. The existing solutions increase the workload and may produce additional defects, and the cleaning process produces a large amount of dust.
By adjusting the cross-sectional parameters of the crystallizer, using protective slag, controlling the argon blowing scheme of plug rods and immersive water outlet socket depth, the casting machine operation is optimized to reduce the occurrence of transverse cracks at the corners of the casting blank and the surface longitudinal cracks, and improve the quality of the casting blank.
It effectively reduces the crack rate and skin production rate of casting billets, improves the surface quality of rolled products, and ensures the quality of steel and the stability of mass production.
Smart Images

Figure CN118950968A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of iron and steel metallurgy and steelmaking, and in particular to a casting method for reducing cracks in a boron-containing peritectic steel continuous casting billet. Background Art
[0002] With the advancement of production technology in the steel industry, the quality of hot-rolled strip steel products has been significantly improved in recent years. However, hot-rolled plate defects still occur frequently in recent years, especially the most serious peeling defect, which has become the main reason affecting the qualification rate of hot-rolled plates. According to the different forms of peeling during rolling, the causes of peeling are analyzed. The surface cracks of the ingot cannot be welded during the pressure processing and deformation process, forming intermittent "peeling" near the edge along the rolling direction. At present, the main method to solve the cracks of the ingot is to flame clean the longitudinal cracks on the surface of the ingot off the line, cut the corners of the transverse cracks at the corners, and perform surface finishing and removal before rolling into the furnace. The workload is increased. At the same time, during the cleaning process, if the operator does not master the correct skills, additional defects may occur. These defects may reduce the quality of the ingot and increase the difficulty and cost of subsequent processing. In addition, a large amount of dust will be generated during the cleaning process. Summary of the invention
[0003] Aiming at the problem of warping of peritectic steel during rolling, the present invention analyzes the influence of parameter setting on transverse cracks at corners of ingot and slag inclusions under the skin of ingot according to the solidification characteristics of peritectic boron-containing steel under different pulling speeds, pouring temperatures and other process operations, and finally analyzes the cause of warping of peritectic boron-containing steel during rolling, and proposes a casting method for reducing cracks in continuous casting ingots of boron-containing peritectic steel, thereby correspondingly improving the quality of ingots.
[0004] The technical solution of the present invention:
[0005] A casting method for reducing cracks in a boron-containing peritectic steel continuous casting billet comprises the following steps:
[0006] S1. Adjust the cross-sectional parameters of the crystallizer during the casting machine preparation stage, and adjust the crystallizer taper during the width adjustment process;
[0007] S2. Prepare the materials and the mold protection slag for adjusting the parameters;
[0008] S3. After the ladle is poured, open the stopper rod to start pouring the tundish; use the pouring slag after the molten steel has submerged the diversion hole of the invasive nozzle. When the pouring slag is completely melted, add the protective slag;
[0009] S4, control the liquid level of the crystallizer to be stable;
[0010] S5. After the casting machine starts, increase the casting speed according to the key points of operation and adjust the depth of the immersion nozzle;
[0011] S6. After the pulling speed reaches the normal pulling speed, the plug rod adjustment and argon blowing scheme is adopted.
[0012] Preferably, in S6, the stopper rod argon blowing scheme is adopted, the argon sealing pressure flow is controlled to be 10-20NL / min, the pressure is above 0.2Mpa, the stopper rod and nozzle argon blowing amount is 1-5NL / min, the pressure is above 0.2Mpa, and the continuous casting nitrogen addition amount is controlled at 5ppm±1ppm.
[0013] Preferably, the immersion socket depth in S5 is 150-160 mm.
[0014] Preferably, the liquid level fluctuation of the crystallizer in S4 is controlled within ±5 mm.
[0015] Preferably, the stopper rod is opened 100 seconds after the pouring in S3 to start pouring in the tundish.
[0016] Preferably, the moisture content of the protective slag in S2 is not greater than 0.50%, the viscosity of the protective slag is 1.21P under working conditions of 1300°C, the melting temperature is adjusted to 1082°C, and the basicity is adjusted to 1.25.
[0017] Preferably, the inverted taper of the crystallizer in S1 is adjusted to 0.98% / m.
[0018] Beneficial effects of the present invention:
[0019] The present invention effectively reduces the occurrence of transverse cracks at the corners of the ingot and longitudinal cracks on the surface by taking process measures such as adjusting the taper of the crystallizer, adjusting the physical and chemical properties of the protective slag, and controlling the argon flow rate of the stopper rod; and adopts a pulling speed increase scheme that matches the casting machine to effectively prevent the occurrence of cracks in the ingot. Through tracking and adjustment, after taking the above measures, the comprehensive crack rate of boron peritectic steel slabs is reduced to 1.2% or less, and the rate of steel rolling warping is reduced to 3.8% or less, which greatly improves the surface quality of the rolled products, ensures the quality improvement and mass production of this type of steel, and has great promotion value. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 These are pictures of the warping defects formed on the surface of the slab of sample 1# of the present invention after slag inclusion and rolling deformation at different magnifications.
[0021] Figure 2 These are the warping defect images of sample 2 of the present invention at different magnifications of the slab that is locally overheated and formed after rolling.
[0022] Figure 3 These are typical warping defect images of sample 3# of the present invention at different magnifications of the transverse cracks at the corners of the slab formed after heating and rolling deformation.
[0023] Figure 4 The corner cracks formed by improper rolling width adjustment at different magnifications of the 4# sample of the present invention cannot be welded during the rolling process to form a warping pattern. DETAILED DESCRIPTION
[0024] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation method, structure, characteristics and effects of the present invention are described in detail below in combination with the accompanying drawings and preferred examples of modified conditions.
[0025] According to the typical characteristics of peeling skin, common peeling skin types can be divided into four categories, and their manifestations are rough scratches, linear peeling skin, local peeling skin and intermittent strip peeling skin. Different types of samples are taken separately and marked as 1#, 2#, 3#, and 4# samples for electron microscopy analysis.
[0026] like Figure 1 As shown in the figure, sample 1#: the defect depth is only 50-100 microns, the structure at the defect is obviously deformed and fragmented; there is foreign non-metal rolling in the local area. This shows that the rolling temperature of the defect area is below the recrystallization temperature. It is speculated that it may be the uneven surface (pitted surface) formed by local bonding and scratching, which is caused by multiple rolling passes. The rolled non-metallic inclusions are likely to be caused by bonded foreign particles or subcutaneous slag of the ingot rolling into the surface of the steel plate.
[0027] like Figure 2 As shown, sample 2#: the defect cross-section morphology is a crack, with a depth of about 200-500 microns, more than one layer, and the entire defect area is severely decarburized. The organization is equiaxed ferrite, while the matrix organization is F+a small amount of P organization. The interlayer is iron oxide, the thickness of the interlayer varies, and the cross-section morphology cracks are bifurcated. The microscopic morphology shows that the defect is generated in the ingot, which may be formed by the transverse cracks at the corners of the continuous casting ingot after heating and rolling deformation. This defect is not like a subcutaneous bubble, because the entire defect area is severely decarburized, not just around the crack, and the end of the defect is sharp.
[0028] like Figure 3 As shown in the figure, sample 3#: the defect area is a pit left after the peeling off. There is a layer of iron oxide at the bottom of the pit, and there are still layers below. The interlayer is full of iron oxide. The defect area has obvious stratification. The surface layer is all decarburized with coarse grains, while the matrix structure has fine grains. According to the characteristics of the structure and grains, it is speculated that the defect is likely to be a protruding or warped part of the slab, which is formed after rolling due to local overheating in the heating furnace.
[0029] like Figure 4As shown, sample 4#: the defect is in the shape of a sandwich, about 100 microns deep, with iron oxide in the sandwich, the defect area is connected to the matrix, the defect organization is full ferrite, and is obviously deformed, while the matrix organization is an equiaxed F+P organization. (F is ferrite, P is pearlite, and the room temperature equilibrium organization of low and medium carbon steel is generally F+P) This indicates that the metal in the defect area has been rolled in a low temperature area. It is inferred that the defect is likely to be caused by the low temperature area at the corner of the intermediate billet under a certain side pressure of the vertical roll, which has caused deformation beyond the thermoplastic tolerance of the slab material, forming a corner crack. This crack cannot be welded during rolling during the subsequent deformation process, forming an intermittent "warping" near the edge along the rolling direction.
[0030] Through electron microscope analysis, the causes of "warping" were analyzed, and it was found that the "warping" defect was formed after the surface of the slab of sample 1# was deformed by slag inclusion and rolling. The transverse cracks at the corners of the sample 2# were typical "warping" defects formed after heating and rolling deformation. The "warping" defect was formed after the slab of sample 3# was locally heated and overheated, and the slab of sample 4# was locally heated and overheated, and the "warping" defect was formed after rolling. Through analysis, the formation of "warping" defects is closely related to the surface quality of the ingot. Most of the defects of "warping" are distributed on the two sides of the ingot, and some are distributed in the center. Through the on-site surface quality inspection of the same batch of slabs, the transverse cracks and longitudinal cracks at the corners of the continuous casting ingot are the main causes of "warping". From the perspective of continuous casting, controlling the warping defects of peritectic boron-containing steel should start from improving the surface quality of the ingot, and reducing the transverse cracks at the corners of the ingot and the subcutaneous slag inclusions has become the main measure to improve the warping defects. Therefore, the parameters and conditions in these aspects are adjusted, as shown in the embodiments, comparative examples and condition change examples.
[0031] Example 1
[0032] The following specific process is adopted to reduce cracks in B-containing peritectic steel.
[0033] The steel grade A36-B is produced, and the casting machine crystallizer has a cross-sectional width of 1265mm, a thickness of 200mm, and a length of 12000mm.
[0034] During the preparation stage of the casting machine, the cross-sectional parameters of the crystallizer are adjusted, and the inverted taper of the crystallizer is adjusted to 0.98% / m during the width adjustment process; prepare the materials and the crystallizer protective slag with adjusted parameters. The monitoring value of the melting temperature of the protective slag is 1082°C, the viscosity is 1.21P (1300°C), the basicity is 1.25, and the viscosity of the protective slag is 1.21P under the working conditions of 1300°C. The melting temperature and basicity are adjusted to 1082°C and 1.25 respectively, and the moisture content of the protective slag is controlled. If moisture-proof measures are taken, the moisture content of the protective slag is guaranteed to be below 0.5%. After the ladle is poured, open the stopper rod 100 seconds after the pouring starts to start pouring in the tundish; use the pouring slag after the molten steel has submerged the diversion hole of the immersion nozzle, and add the protective slag when the pouring slag is completely melted; control the liquid level of the crystallizer to be stable, and the liquid level fluctuation of the crystallizer is controlled within ±5mm; after the casting machine is started, increase the drawing speed to 0.8m / min according to the operating points, and adjust the depth of the immersion nozzle plug to 150mm; after the drawing speed increases to the normal drawing speed, adjust the stopper rod argon blowing plan, the argon sealing pressure flow is controlled to 20NL / min, the pressure is 0.45Mpa, the argon blowing amount of the stopper rod and nozzle is 5NL / min, the pressure is 0.28Mpa, and the continuous casting nitrogen addition amount is controlled at 5ppm±1ppm.
[0035] After tracking, in this example, during the casting process of the casting machine, the liquid level of the crystallizer was stable, the normal pulling speed was controlled at 1.2-1.4m / min, and the batch production was successfully completed. The surface quality of the ingot was good. In this casting, two head ingots had corner transverse cracks that needed to be cleaned, and another one had a more serious longitudinal crack. The crack ratio accounted for 1.2% of the total batch ratio, and the rate of steel rolling warping was reduced to 3.8%.
[0036] It can be seen that this method effectively reduces the occurrence of cracks in the ingot and effectively prevents the risk of warping during the ingot rolling process.
[0037] Example 2
[0038] The following specific process is adopted to reduce cracks in B-containing peritectic steel.
[0039] The steel grade A36-B is produced, and the casting machine crystallizer has a cross-sectional width of 1265mm, a thickness of 200mm, and a length of 12000mm.
[0040] During the preparation stage of the casting machine, the cross-sectional parameters of the crystallizer are adjusted, and the inverted taper of the crystallizer is adjusted to 0.98% / m during the width adjustment process; prepare the materials and the crystallizer protective slag with adjusted parameters. The monitoring value of the melting temperature of the protective slag is 1082°C, the viscosity is 1.21P (1300°C), the basicity is 1.25, and the viscosity of the protective slag is 1.21P under the working conditions of 1300°C. The melting temperature and basicity are adjusted to 1082°C and 1.25 respectively, and the moisture content of the protective slag is controlled. If moisture-proof measures are taken, the moisture content of the protective slag is guaranteed to be below 0.5%. After the ladle is poured, open the stopper rod 100 seconds after the pouring starts to start pouring in the tundish; use the pouring slag after the molten steel has submerged the diversion hole of the immersion nozzle, and add the protective slag when the pouring slag is completely melted; control the liquid level of the crystallizer to be stable, and the liquid level fluctuation of the crystallizer is controlled within ±5mm; after the casting machine is started, increase the drawing speed to 0.8m / min according to the operating points, and adjust the depth of the immersion nozzle plug to 160mm; after the drawing speed increases to the normal drawing speed, adjust the stopper rod argon blowing plan, the argon sealing pressure flow is controlled to 10NL / min, the pressure is 0.20Mpa, the argon blowing amount of the stopper rod and nozzle is 1NL / min, the pressure is 0.20Mpa, and the continuous casting nitrogen addition amount is controlled at 5ppm±1ppm.
[0041] After tracking, in this example, during the casting process of the casting machine, the liquid level of the crystallizer was stable, the normal pulling speed was controlled at 1.2-1.4m / min, and the batch production was successfully completed. The surface quality of the ingot was good. In this casting, one head ingot had a corner transverse crack that needed to be cleaned, and another serious longitudinal crack appeared. The crack ratio accounted for 0.81% of the total batch ratio, and the rate of steel rolling warping was reduced to 3.2%.
[0042] It can be seen that the method effectively reduces the occurrence of cracks in the ingot and effectively prevents the ingot from warping during the rolling process.
[0043] Comparative Example 1
[0044] The steel grade A36-B is produced, and the casting machine crystallizer has a cross-sectional width of 1265mm, a thickness of 200mm, and a length of 12000mm.
[0045] During the preparation stage of the casting machine, the cross-sectional dimensions of the crystallizer are adjusted, the taper is set to 1.05%, and protective slag is prepared. The monitoring value of the melting temperature of the protective slag is 1059°C, the viscosity is 1.08P (1300°C), and the basicity is 1.30. 100 seconds after the ladle starts pouring, the temperature of the molten steel in the tundish is measured to be 1568°C. The stopper rod is opened to start pouring in the tundish, and the emergence time is controlled within the specified requirements. When the pouring slag is completely melted, the protective slag is added; the liquid level of the crystallizer is controlled to be stable, and the liquid level fluctuation of the crystallizer is controlled within ±5mm; the casting machine pulling speed is slowly increased from the starting pulling speed of 0.3m / min to 0.6m / min, and the depth of the immersed water nozzle is adjusted to 170mm; after the pulling speed increases to the normal pulling speed, the stopper rod argon blowing plan is adopted, and the argon sealing pressure flow is controlled to be 20NL / min, and the pressure is not required. The argon blowing amount of the stopper rod and the water nozzle is 10-20NL / min, and the pressure is not required;
[0046] After tracking, in this example, during the casting process of the casting machine, the liquid level of the crystallizer was stable, the normal pulling speed was controlled at 1.2-1.4m / min, and the batch production was successfully completed. The surface quality of the ingot was inspected and it was found that the surface cracked ingots were cleaned off the line. A total of 11 transverse cracks at the corners and 4 longitudinal cracks were cleaned off the line. The crack ratio accounted for 6% of the total batch ratio, and the rate of steel rolling warping was reduced to 9.6%.
[0047] Changing Conditions Example 1 Effect of Nitrogen Content in Molten Steel
[0048] Existing studies on B-containing microalloyed steels show that during the casting process of B-containing microalloyed steels, B will first precipitate coarse BN particles under high temperature conditions, and inhibit the precipitation of AIN, thereby reducing the pinning effect on the grain boundary caused by AIN and improving the growth capacity of the grains. In addition, a small amount of solid solution B will gather around the boundary of austenite, blocking Fe and inhibiting the formation of ferrite, and finally coarsening the grains and reducing the yield strength of the microalloyed steel. This will lead to cracks in the casting and deterioration of the surface quality. Therefore, it is particularly important to control the nitrogen addition of molten steel during the casting process.
[0049] The conditions of this modified condition example remain unchanged relative to those of Example 1, except that the stopper rod argon blowing scheme is adopted to reduce the pressure from 0.3 MPa to 0.2 MPa, the argon blowing amount of the stopper rod and the nozzle is adjusted from 30 NL / min to 1-5 NL / min, the ladle casing is modified, and the improvement measures are taken to enhance the ladle casting protection effect and the continuous casting nitrogen increase amount control. Table 1 is a table showing the N content control effect of gas samples extracted from 10 furnaces of steel using this scheme and the original argon blowing control scheme:
[0050] Table 1 Nitrogen content control effect table
[0051]
[0052]
[0053] Conditions before adjustment: pressure 0.3 MPa, argon blowing rate of stopper rod and water inlet 30 NL / min.
[0054] Adjusted conditions: pressure 0.2 MPa, argon blowing rate of stopper rod and water inlet 1-5 NL / min.
[0055] Changing Conditions Example 2: Insertion Depth of Submerged Nozzle
[0056] The insertion depth of the submerged nozzle has a direct impact on the distribution of molten steel in the crystallizer, and is very important for the uniform growth of the ingot. If the depth is too deep, the molten steel flowing out from both sides of the long nozzle will not have enough heat to enter the molten steel surface, causing uneven melting of the protective slag, which will affect the uniform formation of the ingot. If the depth of the nozzle is too shallow, during the flow of molten steel, the molten steel and the protective slag will solidify directly at the front, unable to reach the molten steel surface, and subcutaneous slag inclusions will appear on the surface of the ingot. It is also not conducive to solving the warping defect. The conditions of this modified condition example remain unchanged relative to those of Example 1, and only the depth control of the submerged nozzle for the B-containing microalloyed steel ingot is shown in Table 2.
[0057] Table 2 Immersion socket depth control table
[0058] Section width (mm) Less than 1150 1200-1400 Greater than 1450 Insertion depth (mm) 140-150 Example 1 150-160 160-170
[0059] Changing Conditions Example 3: Stable Crystallizer Level Control
[0060] Effect of mold level fluctuation on corner cracks of ingot
[0061] The slag inclusion on the surface of the ingot is mainly determined by the fluctuation of the liquid level in the crystallizer. The conditions of this modified example remain unchanged relative to those of Example 1, and only the liquid level fluctuation control is improved.
[0062] The effect of liquid level fluctuation on subcutaneous depth is shown in Table 3.
[0063] Table 3 Relationship between liquid level fluctuation and subcutaneous slag depth
[0064]
[0065]
[0066] Changing Conditions Example 4 Suitable Mold Flux Properties
[0067] The accumulation of inclusions on the surface of the ingot is related to the slag entanglement in the crystallizer. Under the influence of the eddy current of the molten steel in the crystallizer and the rising bubbles around the nozzle, the unmelted protective slag or slag strips are easily drawn into the shell of the green ingot.
[0068] The performance of the protective slag also has a certain influence on the generation of transverse cracks in the corners. For example, for peritectic steel that is prone to cracking, it is necessary to use a protective slag with a higher melting temperature and alkalinity. At the same time, the moisture content of the protective slag also has a direct impact on its use effect. When the moisture content is greater than 0.50%, the melting performance will deteriorate; when the moisture content is greater than 0.75%, the qualified rate of the ingot will decrease. Therefore, it is recommended to use a moisture meter to control the moisture content of the protective slag, thereby effectively improving the quality of the ingot. The conditions of this change example remain unchanged relative to those of Example 1, and only two types of protective slags are selected to compare the effects on cracks as shown in Table 4.
[0069] Table 4 Comparison of crack formation in slabs using two types of mold slag
[0070]
[0071] Changing Conditions Example 5: Optimization of Mold Taper
[0072] The crystallizer taper is an important parameter of the slab continuous casting machine. If the taper is too small, the air gap is large, which affects the heat transfer of the billet to the crystallizer and restricts the increase in the drawing speed; if the taper is too large, it will increase the billet drawing resistance and the wear of the crystallizer wall, which can easily cause the billet to shake, causing the billet vibration mark trough segregation to be stressed and form transverse cracks. Therefore, it is necessary to select a suitable crystallizer inverted taper according to the billet cross-sectional dimensions, molten steel characteristics, and actual shrinkage ratio. The conditions of this modified condition example remain unchanged relative to those of Example 1, except that the crystallizer inverted taper is adjusted during the casting of boron-containing steel in the continuous casting operation area of the hot rolled coil division, as shown in Tables 5 and 6.
[0073] Table 5 Taper table before optimization
[0074]
[0075] Table 6 Optimized taper table
[0076]
[0077] Embodiment 1: The cold billet width is 1265 mm, the upper opening width of the crystallizer is 1280.4 mm, the lower opening width of the crystallizer is 1270.4 mm, the single-side taper is 6.3 mm, and the taper is 0.98% / m.
[0078] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A casting method for reducing cracks in a boron-containing peritectic steel continuous casting billet, It is characterized in that The following steps are involved: S1. Adjust the cross-sectional parameters of the crystallizer during the casting machine preparation stage, and adjust the crystallizer taper during the width adjustment process; S2. Prepare the materials and the mold protection slag for adjusting the parameters; S3. After the ladle is poured, open the stopper rod to start pouring the tundish; use the pouring slag after the molten steel has submerged the diversion hole of the immersion nozzle. When the pouring slag is completely melted, add the protective slag; S4, control the liquid level of the crystallizer to be stable; S5. After the casting machine starts, increase the casting speed according to the key points of operation and adjust the depth of the immersion nozzle; S6. After the pulling speed reaches the normal pulling speed, the plug rod adjustment and argon blowing scheme is adopted.
2. A casting method for reducing cracks in a boron-containing peritectic steel continuous casting billet according to claim 1, It is characterized in that In S6, the stopper rod argon blowing scheme is adjusted, the argon sealing pressure flow is controlled to 10-20 NL / min, the pressure is above 0.2Mpa, the stopper rod and nozzle argon blowing volume is 1-5NL / min, the pressure is above 0.2Mpa, and the continuous casting nitrogen addition amount is controlled at 5ppm±1ppm.
3. A casting method for reducing cracks in a boron-containing peritectic steel continuous casting billet according to claim 1, It is characterized in that After the S5 casting machine is started, the pulling speed is increased to 0.8 m / min according to the operating points, and the immersion plug depth is 150-160 mm.
4. A casting method for reducing cracks in a boron-containing peritectic steel continuous casting billet according to claim 1, It is characterized in that The liquid level fluctuation of the crystallizer in S4 is controlled at ±5mm.
5. A casting method for reducing cracks in a boron-containing peritectic steel continuous casting billet according to claim 1, It is characterized in that When pouring starts in S3 for 100 seconds, the stopper rod is opened to start pouring in the tundish.
6. A casting method for reducing cracks in a boron-containing peritectic steel continuous casting billet according to claim 1, It is characterized in that The moisture content of the protective slag in S2 is not more than 0.50%, the viscosity of the protective slag is 1.21P under the working conditions of 1300℃, the melting temperature is adjusted to 1082℃, and the alkalinity is adjusted to 1.
25.
7. A casting method for reducing cracks in a boron-containing peritectic steel continuous casting billet according to claim 1, It is characterized in that The inverted taper of the crystallizer in S1 was adjusted to 0.98% / m.
Citation Information
Cited By
Crack control method for steel casting blank for new energy automobile battery pack