Flat welding method for penetration fillet weld of ring rib structure of high-strength steel cylinder
By opening weld bevels on the edge of the inner ring of the high-strength steel cylinder and the ring ribs and positioning welding and fixing, combining the welding cart to perform argon-rich gas protection welding and multi-layer multi-pass welding processes, the poor quality of the flat welding of the high-strength steel is solved. The problem of this problem has achieved efficient and stable welding effect and met the requirements of ultrasonic and magnetic powder flaw detection.
Patent Information
- Application Number
- CN202411191544.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the flat welding quality of high-strength steel cylinders and ring ribs is poor, especially workpieces with nominal yield strength of 785MPa or above, the welding quality is not high, and it is greatly affected by the welder's technical level, and it is difficult to meet ultrasonic flaw detection level I and magnetic powder. Requirements for level I flaw detection.
The permeable corner weld flat welding method is adopted for high-strength steel cylinder ring rib structure, including opening a weld bevel on the edge of the inner ring of the ring rib, embedding the cylinder, positioning welding and fixing, and using a welding trolley for argon-rich gas protection welding, combined with Multi-layer multi-pass welding process, preheating and post-heat treatment ensure the quality of the weld.
The welding efficiency and quality are improved, the welder's technical requirements are reduced, and the weld quality meets the standards of ultrasonic flaw detection level I and magnetic powder flaw detection level I, meeting the mechanical performance requirements.
Smart Images

Figure CN118951243A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of welding methods, and in particular relates to a method for flat welding of a penetration fillet weld of a high-strength steel cylinder ring rib structure. Background Art
[0002] For high-strength steel cylinders and high-strength steel ring ribs with a nominal yield strength of more than 785MPa and a carbon equivalent of 0.6% to 0.7%, the ring ribs are sleeved outside the cylinder, and the ring ribs and the cylinder are flat-welded together. Ultrasonic flaw detection and magnetic particle flaw detection are required after flat welding, and the ultrasonic flaw detection level I and magnetic particle flaw detection level I must be qualified, and the welding quality requirements are relatively high.
[0003] In the related technology, manual arc welding and manual semi-automatic gas shielded welding are usually used for flat welding. The above two methods are greatly affected by the technical level of the welder, have high requirements on the technical level of the welder, and after welding, the welding quality is not high. Summary of the invention
[0004] The present application aims to at least to some extent solve the technical problem of poor welding quality when flat welding high-strength steel workpieces with a nominal yield strength of more than 785 MPa and a carbon equivalent of 0.6% to 0.7% in the related art. To this end, the present application provides a method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet welds.
[0005] The present application provides a method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet welds, which is used to weld a cylinder and a ring rib with a nominal yield strength of 785 MPa or more and a carbon equivalent of 0.6% to 0.7%. The method comprises:
[0006] A weld groove is provided on the inner edge of the ring rib and the cylinder is embedded in the ring rib to form a horizontal fillet weld;
[0007] Performing tack welding on the back side of the weld groove to fix the cylinder and the ring rib together;
[0008] Using a welding trolley to perform argon-rich gas shielded flat welding on the inner side of the weld groove;
[0009] Performing a root cleaning process on the back side of the weld groove, and forming a root cleaning groove on the back side of the weld groove through the root cleaning process;
[0010] Using a welding trolley to perform argon-rich gas shielded flat welding on the inner side of the root cleaning groove;
[0011] Among them, when performing the argon-rich gas shielded welding, a multi-layer and multi-pass welding process is adopted. The welding gun does not swing during the welding process. The welding current of the base welding, filling welding and cap welding is 220-290A, the arc voltage is 23-28V, the welding speed is 230-500mm / min, and the gas flow rate is 18-25L / min.
[0012] In some embodiments, the weld groove angle α ensures that when performing the base welding, the welding wire reaches the bottom of the weld groove when the dry extension is 12 to 18 mm. The weld groove angle α is controlled at 50° to 55°, and the groove gap L is controlled at 0 to 3 mm.
[0013] In some embodiments, the argon-rich gas shielded welding uses an equal-strength matching gas shielded welding wire, and the diameter of the welding wire is 1.2 mm.
[0014] In some embodiments, the method for flat welding of full penetration fillet welds of a high-strength steel cylinder ring rib structure also includes preheating the welding area before performing argon-rich gas shielded welding. When the thickness of the cylinder and the ring rib is t<40mm, the preheating temperature is controlled at 100-130°C. When the thickness of the cylinder and the ring rib is t≥40mm, the preheating temperature is controlled at 120-150°C. When the thickness of the cylinder and the ring rib is different, the thickness of the larger one shall prevail.
[0015] In some embodiments, during the argon-rich gas shielded welding process, the inter-pass temperature is controlled. When the thickness of the cylinder and the ring rib is t < 40 mm, the inter-pass temperature is controlled at 100-130°C. When the thickness of the cylinder and the ring rib is t ≥ 40 mm, the inter-pass temperature is controlled at 120-150°C. When the thickness of the cylinder and the ring rib is different, the thickness of the larger one shall prevail.
[0016] In some embodiments, after the argon-rich gas shielded welding, the high-strength steel workpiece is subjected to post-heat treatment, the temperature of the post-heat treatment is controlled at 200-250° C., and the insulation time of the post-heat treatment is controlled at more than 2 hours.
[0017] In some embodiments, during the root cleaning process, the root cleaning depth D=t / 3+5mm, wherein t / 3 represents the thickness of the blunt edge of the weld groove, and the bottom of the root cleaning groove is arc-shaped with a radius of 3.5mm.
[0018] In some embodiments, if multiple welding carriages are used for simultaneous welding, the staggered distance of the welding joints in the middle of the weld is greater than 25 mm. Before welding the same weld joint, the ends of the joints are polished to a slope of no more than 1:5, and the weld joints are polished smooth after welding.
[0019] In some embodiments, the welding length of a single welding carriage is no more than 6 m.
[0020] In some embodiments, before using a welding carriage to perform argon-rich gas shielded welding on the inner side of the weld groove, the weld groove and the area within 30-50 mm on both sides are polished to reveal a metallic luster; before using a welding carriage to perform argon-rich gas shielded welding on the inner side of the root cleaning groove, the root cleaning groove and the area within 30-50 mm on both sides are polished to reveal a metallic luster.
[0021] The present invention has at least the following beneficial effects:
[0022] The method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet weld is suitable for welding cylinders and ring ribs with a nominal yield strength of 785 MPa or more and a carbon equivalent of 0.6% to 0.7%. The method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet weld is firstly to open a weld groove at the inner edge of the ring rib and embed the cylinder in the ring rib to form a horizontal fillet weld, and then to perform a tack welding operation on the back of the weld groove, so that the cylinder and the ring rib are fixed, and the continuity and stability of the bottom weld between the weld grooves are ensured. The method firstly welds the inner side of the weld groove, and after the welding of the inner side of the weld groove is completed, the back side of the weld groove is root-cleaned to form a root-cleaned groove, and then the inner side of the root-cleaned groove is welded, so that the cylinder and the ring rib are fully welded to form a full penetration fillet weld, and the connection strength of the cylinder and the ring rib after welding is ensured. When welding the weld groove and the root groove, the welding trolley is used for automated argon-rich gas shielded welding, which improves the overall welding efficiency and welding quality, and the welding cost is also lower than that of welding robots.
[0023] When welding the weld groove and the root groove, a multi-layer and multi-pass welding process is adopted. The welding current of the base welding, the filling welding and the cover welding is 220-290A, the arc voltage is 23-28V, the welding speed is 230-500mm / min, and the gas flow rate is 18-25L / min. The flat welding method for the high-strength steel cylinder ring rib structure of the present invention strictly controls the welding process parameters of the high-strength steel cylinder ring rib structure, thereby ensuring the quality of the weld. The quality of the weld after welding can meet the requirements of ultrasonic flaw detection level I and magnetic particle flaw detection level I, and its mechanical properties can also meet the technical requirements.
[0024] In summary, the flat welding method for full penetration fillet welds of the high-strength steel cylinder ring rib structure of the present invention can effectively improve the welding efficiency during the horizontal welding of high-strength steel workpieces, has low requirements on the technical level of welders, has high weld quality, and can meet the welding quality requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following is a brief introduction to the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 A schematic flow chart of a method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet welds in one or more embodiments of the present application is shown.
[0027] Figure 2 1 is a dimensional diagram showing a weld groove of a high-strength steel workpiece in one or more embodiments of the present application.
[0028] Figure 3 1 is a dimensional diagram showing the root cleaning groove of a high-strength steel workpiece in one or more embodiments of the present application.
[0029] Figure numerals: 10 - weld groove, 20 - root groove, 30 - cylinder, 40 - ring rib. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] It should be noted that all directional indications in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between various components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0032] In the present invention, unless otherwise clearly specified and limited, the terms "connection", "fixation", etc. should be understood in a broad sense. For example, "fixation" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0033] In addition, in the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0034] For high-strength steel cylinders and high-strength steel ring ribs with a nominal yield strength of more than 785MPa and a carbon equivalent of 0.6% to 0.7%, the ring ribs are sleeved outside the cylinder, and the ring ribs and the cylinder are flat-welded together. Ultrasonic flaw detection and magnetic particle flaw detection are required after flat welding, and the ultrasonic flaw detection level I and magnetic particle flaw detection level I must be qualified, and the welding quality requirements are relatively high.
[0035] In the related technology, manual arc welding and manual semi-automatic gas shielded welding are usually used for flat welding. The above two methods are greatly affected by the technical level of the welder, have high requirements on the technical level of the welder, and after welding, the welding quality is not high.
[0036] In the related art, there is a technical problem of poor welding quality when flat welding a high-strength steel cylinder with a nominal yield strength of more than 785MPa and a carbon equivalent of 0.6% to 0.7% and a high-strength steel ring rib. The embodiment of the present application provides a method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet welds, which can at least solve the technical problem of poor welding quality to a certain extent.
[0037] For high-quality welds, ultrasonic flaw detection level I and magnetic particle flaw detection level I must be qualified after welding, and the welding quality requirements are high. The use of automatic welding is conducive to ensuring welding quality, improving welding efficiency, and reducing welder strength. Automatic welding has the advantages of controllable welding speed, continuous and stable welding process, and is not affected by the welder's physical strength. However, the process parameters and process requirements of manual arc welding and manual semi-automatic gas shielded welding cannot meet the requirements of automatic welding. Therefore, under the demand of improving welding efficiency and ensuring welding quality as much as possible, the process requirements of automatic welding such as welding speed, welding voltage and current need to be optimized in a targeted manner.
[0038] The method for flat welding of full penetration fillet welds of a high-strength steel cylinder ring rib structure of the present application is suitable for welding a cylinder 30 and a ring rib 40 with a nominal yield strength of more than 785 MPa and a carbon equivalent of 0.6% to 0.7%.
[0039] like Figure 1As shown, an embodiment of the present invention provides a method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet welds, comprising steps S100, S200, S300, S400 and S500.
[0040] Step S100, as Figure 2 As shown, a weld groove 10 is provided on the inner edge of the ring rib 40 and the cylinder 30 is embedded in the ring rib 40 to form a horizontal fillet weld.
[0041] Flat welding refers to a welding process in which the welding position is in a horizontal position or at a small inclination angle, the welding rod is located above the workpiece, and the welder looks down at the workpiece. Therefore, before flat welding, the cylinder 30 needs to be embedded in the ring rib 40 to form a horizontal fillet weld.
[0042] S200, performing positioning welding on the back side of the weld groove 10 to fix the cylinder 30 and the ring rib 40 together.
[0043] When tack welding is performed at the weld groove 10, the welding continuity and welding process stability of the base weld will be affected due to the different states of the weld groove 10 in the tack welding and non-tack welding areas. Therefore, tack welding on the back of the weld groove 10 helps to ensure the continuity of the base weld and the stability of the welding process. Through tack welding, the cylinder 30 and the ring rib 40 are fixed together to ensure that the positions of the two high-strength steel workpieces will not change during the welding process, which is convenient for the subsequent formal argon-rich gas shielded welding.
[0044] S300, a welding carriage is used to perform argon-rich gas shielded flat welding on the inner side of the weld groove 10.
[0045] S400, such as Figure 3 As shown, the back side of the weld groove 10 is subjected to a root cleaning process, and a root cleaning groove 20 is formed on the back side of the weld groove 10 through the root cleaning process.
[0046] The back side of the weld groove 10 can be cleaned mechanically or by other cleaning methods.
[0047] S500, use a welding carriage to perform argon-rich gas shielded flat welding on the inner side of the root groove 20.
[0048] Welding parameters are an important basis for determining welding process and welding quality. The success of any welding method and welding process must be determined through welding process assessment tests. Welding parameters include: wire diameter, shielding gas flow, welding current, arc voltage, welding speed, arc length, weld groove form, etc., which must be taken into account at the same time during welding. Any inappropriate selection of any of these parameters will have a great impact on welding quality, and none of them can be missing. Welding current, arc voltage and welding speed influence and restrict each other.
[0049] When the welding current is too large, although the arc penetration and arc stiffness increase, the welding speed needs to be increased accordingly in order to control the welding line energy. When the welding speed is too fast, the stability of the welding arc decreases, which is not conducive to ensuring the welding quality; when the welding current is too small, the arc stiffness and the penetration depth and width decrease, which is not conducive to eliminating the defects between passes and affects the welding quality. In addition, when the current is too small, the welding efficiency decreases, and it is difficult to reflect the advantages of automatic welding.
[0050] The welding process and process parameters of the argon-rich gas shielded welding in step S300 are the same as the welding process and process parameters of the argon-rich gas shielded welding in step S500.
[0051] Specifically, in step S300 and step S500, when argon-rich gas shielded welding is performed on high-strength steel, the following control is performed: a multi-layer and multi-pass welding process is adopted during welding, the welding gun does not swing during the welding process, the welding current of the base welding, filling welding and cap welding is 220-290A, the arc voltage is 23-28V, the welding speed is 230-500mm / min, and the gas flow rate is 18-25L / min.
[0052] The structures of the welding trolley are various and known to those skilled in the art. In some embodiments, the welding trolley uses an automatic walking trolley with a profiling function, and the trolley has a follow-up tracking function to ensure that the walking trajectory of the automatic walking trolley is consistent with the weld. The welding trolley can use a magnetic suction method to walk along the curved surface of the cylinder, and at the same time, the trolley guide wheel mechanism walks on the ring rib to achieve XYZ three-dimensional weld tracking. In these embodiments, the welding trolley can use an automatic walking trolley with a profiling function. This trolley has a follow-up tracking function, which helps to ensure that the walking trajectory of the automatic walking trolley is consistent with the weld.
[0053] In this embodiment, the weld groove 10 is grooved according to the general groove size of gas shielded welding or related special standards, and the angle α of the weld groove 10 ensures that when the welding wire is extended to 12-18 mm during the base welding, it reaches the bottom of the weld groove 10, and the weld groove 10 should be uniform. Specifically, in this embodiment, the angle α of the weld groove 10 is controlled at 50°-55°, and the groove gap L is controlled at 0-3 mm.
[0054] In this embodiment, the welding wire for argon-rich gas shielded welding uses an equal-strength matching gas shielded welding wire, and the diameter of the welding wire is 1.2 mm.
[0055] Iso-strength matched gas shielded welding wire refers to a gas shielded welding wire that matches the strength grade of the base material. This welding wire not only has a strength level equivalent to that of the base material, but also can be effectively protected by the gas during the welding process, thereby ensuring the quality and performance of the weld. This matching method helps to improve the overall strength and service life of the welded joint and meet the use requirements under various complex working conditions.
[0056] Preheating before welding can reduce the thermal stress and deformation generated during welding, improve the fusion quality of weld metal and base material, prevent welding cracks, and improve the mechanical properties of welded joints. Preheating can make the welding area reach a certain temperature, thereby slowing down the cooling rate during welding, which helps to fully melt and mix the welding materials and ensure welding quality.
[0057] Therefore, before performing argon-rich gas shielded welding, the welding area is preheated. When the thickness t of the cylinder 30 and the ring rib 40 is less than 40 mm, the preheating temperature is controlled at 100-130°C. When the thickness t of the cylinder 30 and the ring rib 40 is greater than or equal to 40 mm, the preheating temperature is controlled at 120-150°C. When the thicknesses of the cylinder 30 and the ring rib 40 are different, the larger thickness shall prevail.
[0058] That is to say, before performing step S300 of flat welding with argon-rich gas shielded welding on the inner side of the weld groove 10 using a welding carriage, and before performing step S500 of flat welding with argon-rich gas shielded welding on the inner side of the root cleaning groove 20 using a welding carriage, the welding area is preheated. When the thickness t of the cylinder 30 and the ring rib 40 is less than 40 mm, the preheating temperature is controlled at 100-130°C. When the thickness t of the cylinder 30 and the ring rib 40 is greater than or equal to 40 mm, the preheating temperature is controlled at 120-150°C. When the thickness of the cylinder 30 and the ring rib 40 is different, the larger thickness shall prevail. For example, if the thickness of the cylinder 30 is 50 mm and the thickness of the ring rib 40 is 30 mm, the preheating temperature shall be controlled at 120-150°C based on 50 mm; for another example, if the thickness of the cylinder 30 and the ring rib 40 are both 30 mm, the preheating temperature shall be controlled at 100-130°C.
[0059] Interpass temperature control can ensure that each layer of weld is kept within a suitable temperature range before welding the next layer during multi-layer welding. This control helps to reduce welding stress and deformation, improve the fusion quality and mechanical properties of the weld, and prevent welding defects such as cracks and lack of fusion caused by excessively high or low temperatures, thereby ensuring the overall quality and stability of multi-layer welding.
[0060] Therefore, during the argon-rich gas shielded welding process, the inter-pass temperature is controlled. When the thickness of the cylinder 30 and the ring rib 40 is t<40mm, the inter-pass temperature is controlled at 100-130°C. When the thickness of the cylinder 30 and the ring rib 40 is t≥40mm, the inter-pass temperature is controlled at 120-150°C. When the thickness of the cylinder 30 and the ring rib 40 are different, the thickness of the larger one shall prevail.
[0061] That is to say, in the process of performing argon-rich gas shielded welding flat welding on the inner side of the weld groove 10 using a welding carriage in step S300, and in the process of performing argon-rich gas shielded welding flat welding on the inner side of the root cleaning groove 20 using a welding carriage in step S500, the interpass temperature is controlled. When the thickness of the cylinder 30 and the ring rib 40 is t<40mm, the interpass temperature is controlled at 100~130℃, and when the thickness of the cylinder 30 and the ring rib 40 is t≥40mm, the interpass temperature is controlled at 120~150℃. When the thickness of the cylinder 30 and the ring rib 40 is different, the thickness of the larger one shall prevail. For example, if the thickness of the cylinder 30 is 50mm and the thickness of the ring rib 40 is 30mm, the interpass temperature is controlled at 120~150℃ based on 50mm; for another example, if the thickness of the cylinder 30 and the ring rib 40 are both 30mm, the interpass temperature is controlled at 100~130℃.
[0062] Post-heat treatment can improve the microstructure and properties of the welded joint, reduce residual stress and improve the dimensional stability of the welded joint.
[0063] Therefore, after argon-rich gas shielded welding, the high-strength steel workpiece is subjected to post-heat treatment, the temperature of the post-heat treatment is controlled at 200-250°C, and the holding time of the post-heat treatment is controlled at more than 2 hours.
[0064] That is, after performing step S300 of flat welding with argon-rich gas shielded welding on the inner side of the weld groove 10 using a welding carriage, and after performing step S500 of flat welding with argon-rich gas shielded welding on the inner side of the root groove 20 using a welding carriage, post-heat treatment is performed. The temperature of the post-heat treatment is controlled at 200-250°C, and the holding time of the post-heat treatment is controlled at more than 2 hours.
[0065] In this embodiment, during the root cleaning process in step S400, the root cleaning depth D=t / 3+5mm, t / 3 represents the thickness of the blunt edge of the weld groove 10, the bottom of the root cleaning groove 20 is arc-shaped, and the arc radius is 3.5mm. t represents the thickness of the annular rib.
[0066] If multiple trolleys are used for simultaneous welding during argon-rich gas shielded welding, the weld joints in the middle of the weld should be staggered, with a staggered distance greater than 25mm. Before welding the same weld joint, the joint end should be polished to a gentle slope (height: length) of no more than 1:5, and the weld joint should be polished smooth after welding.
[0067] At the welding arc starting and arc ending, defects such as pores are easily generated due to arc instability. If the defects are not removed, they will be mixed into the weld joint, resulting in unqualified weld quality. In addition, if the slope of the arc starting or arc ending end of the weld at the welding joint is too steep, it is difficult to fuse the joint when connecting the weld bead, which is easy to form defects. Therefore, the joint end needs to be polished to a gentle slope (height: length) of no more than 1:5.
[0068] The welding length of a single welding carriage shall not exceed 6m to ensure that the interlayer temperature of the weld is not lower than 100℃.
[0069] Before using the welding carriage to perform argon-rich gas shielded welding on the inner side of the weld groove 10, the weld groove 10 and the area within 30-50mm on both sides should be polished to reveal the metallic luster; before using the welding carriage to perform argon-rich gas shielded welding on the inner side of the root cleaning groove 20, the root cleaning groove 20 and the area within 30-50mm on both sides should be polished to reveal the metallic luster.
[0070] By grinding, impurities in the weld groove 10 and the root groove 20 are removed, which helps to reduce pores and cracks in welding, improve the strength and durability of the welded structure, and thus ensure the quality and stability of the welded joint.
[0071] In some embodiments, the thickness of the cylinder 30 is 25 mm, the thickness of the ring rib 40 is 18 mm, and the high-strength steel cylinder ring rib structure is welded according to the above-mentioned penetration fillet weld flat welding method. After welding, non-destructive testing and mechanical property tests are carried out according to relevant technical requirements, and the technical requirements are met. The specific results are as follows:
[0072] The results of non-destructive testing are shown in Table 1:
[0073] Table 1 Nondestructive testing results
[0074] Inspection methods standard Test results Ultrasonic testing NB / T 47013.3 Level I, qualified Magnetic Particle Testing NB / T 47013.4-2015 Level I, qualified
[0075] The joint hardness test results are shown in Table 2:
[0076] Table 2 Joint hardness test results table Evaluation index: Hardness HV ≤ 450
[0077]
[0078] The hardness of the samples was ≤450, and the results were qualified.
[0079] For ease of understanding, it should be noted that 1, 2, and 3 in the column where the sample number is located in Table 2 represent three different sections of the welded joint, and ① and ② represent two different areas on each section. It is easy to understand that the three values in each grid represent the hardness values of three points in each part. As shown in the first row of data in Table 2, in the first area of the first section of the weld, the hardness values of the three points on the first parent material are 307, 300, and 299, respectively, the hardness values of the three points in the first heat-affected zone are 361, 365, and 367, respectively, the hardness values of the three points in the weld area are 343, 339, and 348, respectively, the hardness values of the three points on the second heat-affected zone are 378, 380, and 372, respectively, and the hardness values of the three points on the second parent material are 315, 309, and 308, respectively.
[0080] The results of macroscopic metallographic examination are shown in Table 3:
[0081] Table 3 Macroscopic metallographic examination results
[0082] Sample No. crack Pores Slag inclusion Unfused Unwelded head 1 none none none none none 2 none none none none none 3 none none none none none
[0083] The results of macroscopic metallographic examination are qualified
[0084] For ease of understanding, it should be noted that 1, 2, and 3 in the column of sample numbers in Table 3 represent three different cross-sections of the welded joint.
[0085] To summarize, the cylinder and the ring ribs are welded according to the flat welding method of the full penetration fillet weld of the high-strength steel cylinder ring rib structure of this application. After the cylinder and the ring ribs are welded, the welding quality of the welded joint can meet the requirements of ultrasonic flaw detection level I and magnetic particle flaw detection level I, and the results of the hardness test and metallographic inspection of the welded joint meet the technical requirements.
[0086] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0087] In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the fact that they can be implemented by ordinary technicians in this field. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.
[0088] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.
Claims
1. A method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet welds, characterized in that: Used for welding a cylinder (30) and a ring rib (40) with a nominal yield strength of 785 MPa or more and a carbon equivalent of 0.6% to 0.7%, the method comprises: A weld groove (10) is provided on the inner edge of the ring rib (40) and the cylinder (30) is embedded in the ring rib (40) to form a horizontal fillet weld; Performing tack welding on the back side of the weld groove (10) to fix the cylinder (30) and the annular rib (40) together; Using a welding trolley to perform argon-rich gas shielded flat welding on the inner side of the weld groove (10); Performing a root cleaning process on the back side of the weld groove (10), and forming a root cleaning groove (20) on the back side of the weld groove (10) through the root cleaning process; Using a welding trolley to perform argon-rich gas shielded flat welding on the inner side of the root cleaning groove (20); Among them, when performing the argon-rich gas shielded welding, a multi-layer and multi-pass welding process is adopted. The welding gun does not swing during the welding process. The welding current of the base welding, filling welding and cap welding is 220-290A, the arc voltage is 23-28V, the welding speed is 230-500mm / min, and the gas flow rate is 18-25L / min.
2. The method for flat welding of high-strength steel cylinder ring rib structure with full penetration fillet weld according to claim 1, characterized in that: The angle α of the weld groove (10) ensures that when the base welding is performed, the welding wire reaches the bottom of the weld groove (10) when the dry extension length is 12 to 18 mm. The angle α of the weld groove (10) is controlled at 50° to 55°, and the groove gap L is controlled at 0 to 3 mm.
3. The method for flat welding of high-strength steel cylinder ring rib structure with full penetration fillet weld according to claim 1, characterized in that: The argon-rich gas shielded welding adopts equal strength matching gas shielded welding wire, and the diameter of the welding wire is 1.2 mm.
4. The method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet weld according to any one of claims 1 to 3, characterized in that: The method for flat welding of a full penetration fillet weld of a high-strength steel cylinder ring rib structure also includes preheating the welding area before performing argon-rich gas shielded welding. When the thickness t of the cylinder (30) and the ring rib (40) is less than 40 mm, the preheating temperature is controlled at 100 to 130° C.; when the thickness t of the cylinder (30) and the ring rib (40) is greater than or equal to 40 mm, the preheating temperature is controlled at 120 to 150° C.; when the thickness of the cylinder (30) and the ring rib (40) is different, the larger thickness shall prevail.
5. The method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet weld according to any one of claims 1 to 3, characterized in that: During the argon-rich gas shielded welding process, the interpass temperature is controlled. When the thickness of the cylinder (30) and the ring rib (40) is t<40 mm, the interpass temperature is controlled at 100-130° C.; when the thickness of the cylinder (30) and the ring rib (40) is t≥40 mm, the interpass temperature is controlled at 120-150° C.; when the thickness of the cylinder (30) and the ring rib (40) is different, the thickness of the larger one shall prevail.
6. The method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet weld according to any one of claims 1 to 3, characterized in that: After the argon-rich gas shielded welding, the high-strength steel workpiece is subjected to post-heat treatment, the temperature of the post-heat treatment is controlled at 200-250° C., and the insulation time of the post-heat treatment is controlled at more than 2 hours.
7. The method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet weld according to any one of claims 1 to 3, characterized in that: During the root cleaning process, the root cleaning depth D=t / 3+5mm, wherein t / 3 represents the thickness of the blunt edge of the weld groove (10), and the bottom of the root cleaning groove (20) is arc-shaped with a radius of 3.5mm.
8. The method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet weld according to any one of claims 1 to 3, characterized in that: If multiple welding carriages are used for welding at the same time, the staggered distance of the welding joints in the middle of the weld is greater than 25 mm. Before welding the joints of the same weld, the ends of the joints are ground smoothly to a slope of no more than 1:5, and the weld joints are ground smooth after welding.
9. The method for flat welding of high-strength steel cylinder ring rib structure penetration fillet weld according to claim 8, characterized in that: The welding length of a single welding carriage is not more than 6m.
10. The method for flat welding of a high-strength steel cylinder ring rib structure with full penetration fillet weld according to any one of claims 1 to 3, characterized in that: Before using a welding trolley to perform argon-rich gas shielded welding on the inner side of the weld groove (10), the weld groove (10) and the area within 30-50 mm on both sides are polished to obtain a metallic luster; before using a welding trolley to perform argon-rich gas shielded welding on the inner side of the root cleaning groove (20), the root cleaning groove (20) and the area within 30-50 mm on both sides are polished to obtain a metallic luster.