Anti-deformation correction removing process for thick plate splicing welding
By using X-shaped welding bevel and jack support technology in thick plate splicing welding, the problems of deformation and high cost after welding are solved, and efficient and flat thick plate splicing welding is achieved, which is suitable for panels of various sizes. Save space resources.
Patent Information
- Application Number
- CN202411230350.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-15
AI Technical Summary
The existing thick-plate splicing welding technology requires a lot of fire correction after welding, resulting in deformation and low efficiency. The customized anti-deforming tire frame covers a large area and is costly, and cannot meet the needs of paneling of multiple sizes.
The X-shaped welding bevel and jack support technology are used to gradually complete the thick plate splicing through submerged arc welding and the position of the plates during the welding process is adjusted to ensure the flatness of the welding and avoid pyrotechnic correction.
It realizes welding flatness without pyrotechnical correction, reduces production costs, is suitable for panels of various sizes, and saves space resources. The deformation amount after welding is basically close to zero.
Smart Images

Figure CN118951441A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel plate splicing, and in particular to a thick plate splicing welding anti-deformation correction process. Background Art
[0002] The torsion box area of large container ships requires a large amount of extra-thick steel plates, with a thickness ranging from 50mm to 100mm. The minimum specified yield strength of EH40 steel plate is 390N / mm 2 , the minimum specified yield strength of EH47 steel plate is 460N / mm 2 Among them, for ships with 16,000 TEUs or more, these grades of steel are also required to have crack arrest requirements, and need to be measured by crack arrest toughness Kca or crack arrest temperature CAT. They are divided into two crack arrest toughness grades, BCA1 and BCA2, and there are strict restrictions on the temperature of pyrotechnic correction. There are two common types of thick plate joint welding. One is placed on a horizontal frame for welding. The advantage is that one frame can be used for multiple purposes and can be used for welding of panels of different sizes. However, the disadvantage is that a large amount of pyrotechnic correction is required after welding, especially when welding the rear welding side. It is necessary to add a pressure iron for strong correction. The pyrotechnic correction causes deformation in a large area, and the compliance rate of the pyrotechnic correction is low. The other type uses a customized anti-deformation frame for welding. The advantage is that the quality of steel plate splicing welding is high, but the disadvantage is that it can only be used for panels of one size, and the anti-deformation frame occupies too much area, the production cost is too high, and the test cycle is long.
[0003] Therefore, it is necessary to provide a thick plate splicing welding anti-deformation correction process to solve the above technical problems. Summary of the invention
[0004] The purpose of the present invention is to provide a thick plate splicing welding anti-deformation correction process in view of the shortcomings of the prior art. The process can be used for multiple purposes, reducing production costs. At the same time, the operation is simple and no pyrotechnic correction is required after welding to meet the splicing welding flatness requirements.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A thick plate splicing welding anti-deformation correction process, wherein the thick plate is used as a crack arrest plate in the torsion box area of a container ship, comprises the following steps:
[0007] Step 1, processing an X-shaped welding groove at the joint end of the thick plate, placing the first thick plate, the second thick plate and the third thick plate to be welded on a horizontally arranged flat frame in sequence, completing the butt joint between the thick plates, forming a first splicing seam at the joint of the first thick plate and the second thick plate, and forming a second splicing seam at the joint of the second thick plate and the third thick plate, wherein the corresponding parameters of the X-shaped welding groove are: the angle of the front groove is 50-55°, the angle of the back groove is 65-70°, the blunt edge is 4-6mm, the root gap is 0-1mm, wherein the front groove is the first welding side, and the back groove is the rear welding side;
[0008] Step 2, using submerged arc welding to weld the first welding side of the first joint seam and the second joint seam at the same time, and completing the welding of the first welding side at one time, at this time, the first thick plate and the third thick plate are affected by welding, and the ends of the first thick plate and the third thick plate away from the second thick plate are in an obliquely upward tilted state;
[0009] Step 3, turn over the first thick plate, the second thick plate and the third thick plate and place them on the tire frame, so that the first welding sides of the first splicing seam and the second splicing seam are placed downward, and the rear welding sides of the first splicing seam and the second splicing seam are placed upward. At this time, the second thick plate is in a suspended state, and the distance between the second thick plate and the top surface of the tire frame is 10 mm;
[0010] Step 4, jacks are placed under the first welding side of the first joint and the second joint respectively, and the jacks are used to press and support along the first joint and the second joint, so that a distance of 10 mm is maintained between the second thick plate and the tire frame, and the influence of the second thick plate on the first thick plate and the third thick plate due to the suspended gravity is offset, so that the three thick plates are in a free expansion and contraction state after the first welding side is connected;
[0011] Step 5, welding the rear welding sides of the first joint seam and the second joint seam, adjusting the jack every time three welding layers are completed, so that the distance between the second thick plate and the tire frame is always maintained at 10 mm; Step 6, completing the welding of the rear welding sides of the first joint seam and the second joint seam;
[0012] Step 7, remove the jacks, so that the first thick plate, the second thick plate and the third thick plate fall completely on the tire frame and fit with the tire frame respectively.
[0013] Preferably, the thickness of the thick plate is 50-100 mm.
[0014] Preferably, in step 2, when welding the first welding side of the first joint and the second joint, the process parameters of the base layer on the first welding side are: welding current is 750-850A, arc voltage is 27-33V, welding speed is 26-30m / h, and heat input is 2.35-3.88KJ / mm.
[0015] Preferably, in step 5, when welding the rear welding sides of the first splicing seam and the second splicing seam, the process parameters of the rear welding side base layer are: welding current is 900-1000A, arc voltage is 34-38V, welding speed is 26-30m / h, and heat input is 3.24-5.26KJ / mm.
[0016] Preferably, in step 2 and step 5, when welding the first welding side and the second welding side of the first splicing seam and the second splicing seam, the process parameters of the filling layer of the first welding side and the rear welding side are: welding current is 700-800A, arc voltage is 27-33V, welding speed is 25-29m / h, and heat input is 2.35-3.80KJ / mm.
[0017] Preferably, in step 2 and step 5, when welding the first welding side and the rear welding side of the first splicing seam and the second splicing seam, the process parameters of the cover layer of the first welding side and the rear welding side are: welding current is 650-750A, arc voltage is 25-31V, welding speed is 26-29m / h, and heat input is 2.02-3.22KJ / mm.
[0018] Preferably, the number of weld layers on the first weld side is less than the number of weld layers on the last weld side.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] 1. The tire rack space is not expanded, and one rack can be used for multiple purposes, saving space resources.
[0021] 2. With the help of the external force of the jack, the jack is adjusted several times during the welding process to keep the second thick plate always at a distance of 10mm from the tire frame. After welding, the jack is removed. The deformation of the rear welding side is basically close to the deformation of the first welding side, and the operation is simple.
[0022] 3. No pyrotechnic correction is required after welding, and the flatness pass rate is 100%. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a structural schematic diagram of the X-shaped groove in the present invention;
[0024] Figure 2 It is a process diagram of step 1 of the present invention;
[0025] Figure 3 It is a process diagram of step 2 of the present invention;
[0026] Figure 4 It is a process diagram of step 3 of the present invention;
[0027] Figure 5 It is a process diagram of step 4 of the present invention;
[0028] Figure 6 It is a process diagram of step 7 of the present invention;
[0029] Among them, 1-first thick plate, 2-second thick plate, 3-third thick plate, 4-cradle, 5-jack, 6-base layer, 7-filling layer, 8-covering layer, 9-first welding side, 10-later welding side DETAILED DESCRIPTION
[0030] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.
[0031] In the present invention, unless otherwise clearly stipulated and limited, the terms such as "installation", "setting", "connection", "fixed connection" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements. Unless otherwise clearly defined, ordinary technicians in this field can understand the specific meanings of the above terms in the present invention according to the specific circumstances.
[0032] In the present invention, the directions or positional relationships indicated by terms such as "upper", "lower", "bottom", "top", etc. are based on the directions or positional relationships shown in the accompanying drawings. They are relational words determined only for the convenience of describing the structural relationships of the various parts or elements of the present invention. They do not specifically refer to any part or element in the present invention and cannot be understood as limitations on the present invention.
[0033] A thick plate splicing welding anti-deformation correction process, wherein the thick plate is used as a crack arrest plate in a torsion box area of a container ship, comprises the following steps.
[0034] Step 1, such as Figure 1 to Figure 2 As shown, an X-shaped welding groove is processed at the joint end of the thick plate, and the first thick plate 1, the second thick plate 2 and the third thick plate 3 to be welded are placed on a horizontally arranged flat frame 4 in sequence, and the thickness of the first thick plate, the second thick plate and the third thick plate are all 80mm, and the thick plates are butted against each other, and the first thick plate and the second thick plate form a first joint seam at the joint, and the second thick plate and the third thick plate form a second joint seam at the joint, wherein the corresponding parameters of the X-shaped welding groove are: the angle of the front groove is 50-55°, the angle of the back groove is 65-70°, the blunt edge is 4-6mm, and the root gap is 0-1mm, wherein the front groove is the first welding side 9, and the back groove is the rear welding side 10;
[0035] Step 2, such as Figure 3As shown, the first welding side of the first joint seam and the second welding side are welded by submerged arc welding at the same time. The welding is preheated before welding, and the preheating temperature is 90°C. The bottom layer 6 of the first welding side is welded. The process parameters of the bottom layer of the first welding side are: welding current is 800A, arc voltage is 29V, welding speed is 28m / h, and heat input is 3.26KJ / mm. After the bottom layer of the first welding side is completed, the welding of the filling layer 7 of the first welding side is continued. The process parameters of the filling layer of the first welding side are: welding current is 75 0A, arc voltage is 29V, welding speed is 27m / h, heat input is 3.35KJ / mm, and finally the side cover layer 8 is welded first. The process parameters of the side cover layer are as follows: welding current is 700A, arc voltage is 28V, welding speed is 27m / h, heat input is 2.75KJ / mm, and the welding of the side cover is completed at one time. At this time, the first thick plate and the third thick plate are affected by welding, and the ends of the first thick plate and the third thick plate away from the second thick plate are in an obliquely upward tilted state;
[0036] Step 3, such as Figure 4 As shown, the first thick plate, the second thick plate and the third thick plate are turned over and placed on the tire frame, so that the first welding side of the first splicing seam and the second splicing seam is placed downward, and the rear welding side of the first splicing seam and the second splicing seam is placed upward. At this time, the second thick plate is in a suspended state, and the distance between the second thick plate and the top surface of the tire frame is 10mm;
[0037] Step 4, such as Figure 5 As shown, jacks are placed under the first welding side of the first joint and the second joint respectively, and the jacks are used to press and support along the first joint and the second joint, so that the second thick plate is kept at a distance of 10 mm from the tire frame, offsetting the influence of the second thick plate on the first thick plate and the third thick plate due to the suspended gravity, so that the three thick plates are in a free expansion and contraction state after the first welding side is connected;
[0038] Step 5, welding the rear welding side of the first joint seam and the second joint seam, firstly, welding the base layer on the rear welding side, the process parameters of the base layer on the rear welding side are: welding current is 790A, arc voltage is 28V, welding speed is 27m / h, heat input is 3.15KJ / mm, after the base layer on the rear welding side is completed, continue to weld the back welding side filling layer, adjust the jack once after completing three filling layers, so that the second thick plate and the tire frame always maintain a distance of 10mm, the process parameters of the back welding side filling layer are: welding current is 740A, arc voltage is 28V, welding speed is 27m / h, heat input is 3.22KJ / mm, finally, welding of the back welding side cover layer is carried out, the process parameters of the back welding side cover layer are: welding current is 700A, arc voltage is 28V, welding speed is 27m / h, heat input is 2.75KJ / mm;
[0039] Step 6, completing the welding of the rear welding sides of the first joint seam and the second joint seam, wherein the number of welding layers on the first welding side is less than the number of welding layers on the rear welding side;
[0040] Step 7, such as Figure 6 As shown, the jack is removed, so that the first thick plate, the second thick plate and the third thick plate completely fall on the tire frame and fit with the tire frame respectively, completing the splicing welding operation of the first thick plate, the second thick plate and the third thick plate.
[0041] The above description shows and describes the preferred embodiments of the present invention. As mentioned above, it should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the invention concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not depart from the spirit and scope of the present invention, and should be within the scope of protection of the claims attached to the present invention.
Claims
1. A thick plate splicing welding anti-deformation correction process, the thick plate is used as a crack arrest plate in the torsion box area of a container ship, characterized in that: The following steps are involved: Step 1, processing an X-shaped welding groove at the joint end of the thick plate, placing the first thick plate, the second thick plate and the third thick plate to be welded on a horizontally arranged flat frame in sequence, completing the butt joint between the thick plates, forming a first splicing seam at the joint of the first thick plate and the second thick plate, and forming a second splicing seam at the joint of the second thick plate and the third thick plate, wherein the corresponding parameters of the X-shaped welding groove are: the angle of the front groove is 50-55°, the angle of the back groove is 65-70°, the blunt edge is 4-6mm, the root gap is 0-1mm, wherein the front groove is the first welding side, and the back groove is the rear welding side; Step 2, using submerged arc welding to weld the first welding side of the first joint seam and the second joint seam at the same time, and completing the welding of the first welding side at one time, at this time, the first thick plate and the third thick plate are affected by welding, and the ends of the first thick plate and the third thick plate away from the second thick plate are in an obliquely upward tilted state; Step 3, turn over the first thick plate, the second thick plate and the third thick plate and place them on the tire frame, so that the first welding sides of the first splicing seam and the second splicing seam are placed downward, and the rear welding sides of the first splicing seam and the second splicing seam are placed upward. At this time, the second thick plate is in a suspended state, and the distance between the second thick plate and the top surface of the tire frame is 10 mm; Step 4, jacks are placed under the first welding side of the first joint and the second joint respectively, and the jacks are used to press and support along the first joint and the second joint, so that a distance of 10 mm is maintained between the second thick plate and the tire frame, and the influence of the second thick plate on the first thick plate and the third thick plate due to the suspended gravity is offset, so that the three thick plates are in a free expansion and contraction state after the first welding side is connected; Step 5, welding the rear welding sides of the first joint seam and the second joint seam, adjusting the jack every time three welding layers are completed, so that the distance between the second thick plate and the tire frame is always maintained at 10 mm; Step 6, completing the welding of the rear welding sides of the first joint seam and the second joint seam; Step 7, remove the jacks, so that the first thick plate, the second thick plate and the third thick plate fall completely on the tire frame and fit with the tire frame respectively.
2. A thick plate splicing welding anti-deformation correction process according to claim 1, characterized in that: The thickness of the thick plate is 50-100 mm.
3. The thick plate splicing welding anti-deformation correction process according to claim 1 is characterized in that: In step 2, when welding the first welding side of the first joint and the second joint, the process parameters of the first welding side base layer are: welding current is 750-850A, arc voltage is 27-33V, welding speed is 26-30m / h, and heat input is 2.35-3.88KJ / mm.
4. A thick plate splicing welding anti-deformation correction process according to claim 1, characterized in that: In step 5, when welding the rear welding sides of the first joint and the second joint, the process parameters of the rear welding side base layer are: welding current is 900-1000A, arc voltage is 34-38V, welding speed is 26-30m / h, and heat input is 3.24-5.26KJ / mm.
5. The thick plate splicing welding anti-deformation correction process according to claim 1 is characterized in that: In step 2 and step 5, when welding the first welding side and the second welding side of the first joint seam and the second joint seam, the process parameters of the filling layer of the first welding side and the rear welding side are: welding current is 700-800A, arc voltage is 27-33V, welding speed is 25-29m / h, and heat input is 2.35-3.80KJ / mm.
6. The thick plate splicing welding anti-deformation correction process according to claim 1 is characterized in that: In step 2 and step 5, when welding the first welding side and the second welding side of the first joint seam and the second joint seam, the process parameters of the cover layer of the first welding side and the rear welding side are: welding current is 650-750A, arc voltage is 25-31V, welding speed is 26-29m / h, and heat input is 2.02-3.22KJ / mm.
7. The thick plate splicing welding anti-deformation correction process according to claim 1 is characterized by: The number of weld layers on the first weld side is less than the number of weld layers on the last weld side.
Citation Information
Cited By
Welding method for ship bent outer plate
CN119658202A