Method for repairing ablation and chipping damage of turbine guide ring
Through three-dimensional scanning and CNC machining technology, complementary defect prefabricated parts are built and brazed and repaired, solving the problem of repairing turbine guide ring ablation and block loss damage, achieving improvement in structural integrity and strength, and extending the use of equipment life.
Patent Information
- Application Number
- CN202411278742.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to effectively repair ablation and block loss damage while ensuring the integrity of the overall structure of the turbine guide ring, and the fusion welding method has limited applicability to complex structures, and overall replacement will lead to a reduction in structural strength.
Through surface treatment and non-destructive testing, surface cutting is constructed using three-dimensional scanning and standard digital-analog comparison, CNC machining programs are generated for five-axis processing, complementary defect prefabricated parts are produced, and repaired through spot welding and brazing to ensure the brazing joints Uniformity and performance.
Accurate repair of turbine guide ring ablation and block loss damage, extends the service cycle of the equipment, avoids damage to the overall structure, and improves the strength and performance after repair.
Smart Images

Figure CN118951593A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of turbine guide ring repair, and in particular relates to a method for repairing turbine guide ring ablation and block falling damage. Background Art
[0002] The turbine guide is the core component of the gas turbine engine. It is located at the rear end of the combustion chamber. The fuel is mixed with compressed air in the combustion chamber and ignited to produce gas. The gas is expanded and accelerated by the guide and converted into a tangential direction to blow the rotor blades to make them rotate at high speed, so as to realize the operation of the engine. In order to pursue higher structural strength, the guide ring can be made into a guide ring by integral casting. Although the guide ring is generally coated with a heat-resistant coating, the guide ring will still suffer from damage such as ablation and falling blocks in harsh service environments, resulting in the entire guide ring being unusable. Due to the expensive price and long cycle of new parts, it is generally hoped that the guide ring can be repaired, but fusion welding generally has certain requirements for the repair angle. When facing a guide ring with a complex structure, fusion welding cannot be carried out due to the shielding of different structures. The overall replacement of the damaged arc segment of the guide ring will introduce a brazing seam that penetrates the guide ring, resulting in a reduction in the overall structural strength of the guide ring. In order to avoid the scrapping of the guide ring, a method is needed to repair the damage such as ablation and falling blocks on it while ensuring that the overall structure of the guide ring is as intact as possible. For this purpose, the present invention proposes a method for repairing the damage of ablation and falling blocks of a turbine guide ring. Summary of the invention
[0003] The object of the present invention is to provide a method for repairing turbine guide ring ablation and chipping damage to solve the problems raised in the above-mentioned background technology.
[0004] To achieve the above object, the present invention provides the following technical solution: a method for repairing turbine guide ring ablation and block fall damage, the specific steps comprising:
[0005] S1: Perform surface treatment and non-destructive testing on the guide ring after service, remove surface attachments and coatings, and mark defects;
[0006] S2: Perform a three-dimensional scan on the guide ring, compare the point cloud data obtained by the three-dimensional scan with the standard digital model, and according to the comparison result, construct a curved surface along the edge of the serious missing area to cut the standard digital model. The cut part is the defective digital model, and the remaining part is the matrix digital model. Compare the point cloud data with the matrix digital model to confirm that the serious missing area has been cut off;
[0007] S3: Convert the base model into a CNC machining program used by a five-axis machining center to remove the missing area and process the machined surface into the constructed curved surface shape;
[0008] S4: Convert the defect digital model into a CNC machining program used by a five-axis machining center to process the raw material into a defect prefabricated part that matches the matrix digital model;
[0009] S5: Assemble the defective prefabricated part on the guide ring, fix it by spot welding and add brazing material, and then put it into the furnace for brazing;
[0010] S6: Use non-destructive testing to inspect the repaired area to confirm that there are no defects exceeding the standard;
[0011] S7: Polish or machine the blade to restore the surface profile, then perform a 3D scan on the guide ring and compare it with the standard digital model to confirm that its dimensions meet the standards.
[0012] Preferably, in step S2, when the curved surface is constructed and cut to the standard digital model, sharp angles and cross-sectional structures should be avoided to ensure the wetting and spreading of the solder and the absence of stress concentration points in the brazed joint during service.
[0013] Preferably, in step S2, a processing allowance of 0.1-0.3 mm is added to the outer surface of the cut defective digital model.
[0014] Preferably, step S2: the standard for severe notch needs to be formulated according to the blade structure, and areas with chipping, ablation exceeding 0.5 mm, and other notches exceeding 1 / 2 of the wall thickness may be selected.
[0015] Preferably, step S2, step S3 and step S4 use NX software to cut the digital model, and generate a CNC machining program used by a five-axis machining center based on the digital model. Step S3 and step S4 use Vericut multi-axis machining simulation software to simulate the CNC machining program to avoid overcutting, undercutting and machine tool collision during the guide ring machining process.
[0016] Preferably, in step S4, the raw material is a casting that is cast in the same furnace as the guide ring or has the same material as the guide ring, and the casting is rough-processed using methods such as wire cutting before five-axis machining to reduce the time required for five-axis machining.
[0017] Preferably, in step S5, the solder and brazing system used are determined according to the composition of the guide ring substrate and the structure of the assembly surface. For an assembly surface with a simple structure, paste solder can be directly added to the outer surface of the assembly. For an assembly surface with a complex structure, a solder strip with a thickness of 0.05-0.20 mm needs to be pasted on the assembly surface in advance, and then paste solder is added to the outer surface of the assembly.
[0018] Compared with the prior art, the beneficial effects of the present invention are: through comparison between three-dimensional scanning and standard digital models, the missing data of different areas can be obtained quickly and accurately, the defective areas can be accurately divided, damage to the overall structure of the guide ring can be avoided, and the service life of the guide ring can be effectively extended.
[0019] Different curved surfaces can be constructed as needed during standard digital model cutting. Through appropriate shape and structural design, it can ensure the wetting and spreading of the solder and the absence of stress concentration points in the brazed joints during service.
[0020] By converting the complementary digital models into five-axis machining programs respectively, and utilizing the flexible machining capabilities and precise dimensional control capabilities of the five-axis machining center, it is possible to machine defective preforms that are completely complementary to the surface after defect removal, thereby ensuring the uniformity of the brazing gap, and being able to obtain qualified brazing joints in one go, with higher performance in the brazed joints.
[0021] Defective prefabricated parts are not limited by materials and molds, and there is no need to consider the preparation method of the raw materials of the prefabricated parts. As long as the material can be vacuum brazed, it can be repaired using this method. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the method flow of the present invention. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] See also Figure 1 , provides a technical solution: a method for repairing turbine guide ring ablation and block falling damage, the specific steps include:
[0025] S1: Perform surface treatment and non-destructive testing on the guide ring after service, remove surface attachments and coatings, and mark defects;
[0026] S2: Perform a three-dimensional scan on the guide ring, compare the point cloud data obtained by the three-dimensional scan with the standard digital model, and according to the comparison result, construct a curved surface along the edge of the serious missing area to cut the standard digital model. The cut part is the defective digital model, and the remaining part is the matrix digital model. Compare the point cloud data with the matrix digital model to confirm that the serious missing area has been cut off;
[0027] S3: Convert the base model into a CNC machining program used by a five-axis machining center to remove the missing area and process the machined surface into the constructed curved surface shape;
[0028] S4: Convert the defect digital model into a CNC machining program used by a five-axis machining center to process the raw material into a defect prefabricated part that matches the matrix digital model;
[0029] S5: Assemble the defective prefabricated part on the guide ring, fix it by spot welding and add brazing material, and then put it into the furnace for brazing;
[0030] S6: Use non-destructive testing to inspect the repaired area to confirm that there are no defects exceeding the standard;
[0031] S7: Polish or machine the blade to restore the surface profile, then perform a 3D scan on the guide ring and compare it with the standard digital model to confirm that its dimensions meet the standards.
[0032] In this embodiment, preferably, in step S2, when constructing the curved surface to cut the standard digital model, sharp angles and cross-sectional structures should be avoided to ensure the wetting and spreading of the brazing material and the absence of stress concentration points in the brazed joint during service. In this embodiment, preferably, in step S2, a machining allowance of 0.1-0.3mm is added to the outer surface of the defective digital model cut out. In this embodiment, preferably, step S2: The standard for severe missing quantity needs to be formulated according to the blade structure, and the area where the block is dropped, the ablation exceeds 0.5mm, and the remaining missing quantity exceeds 1 / 2 of the wall thickness can be selected. In this embodiment, preferably, steps S2, S3 and S4 use NX software to cut the digital model, and generate the CNC machining program used for the five-axis machining center according to the digital model. Steps S3 and S4 use Vericut multi-axis machining simulation software to simulate the CNC machining program to avoid overcutting, undercutting and machine tool collision during the guide ring machining process. In this embodiment, preferably, in step S4, the raw material is a casting cast in the same furnace as the guide ring or of the same material, and the casting is rough-machined using a wire cutting method before five-axis machining to reduce the time used for five-axis machining. In this embodiment, preferably, in step S5, the solder and brazing system used are determined according to the composition of the guide ring substrate and the structure of the assembly surface. For an assembly surface with a simple structure, paste solder can be directly added to the outer surface of the assembly. For an assembly surface with a complex structure, a solder strip with a thickness of 0.05-0.20 mm needs to be pasted on the assembly surface in advance, and then a paste solder is added to the outer surface of the assembly.
[0033] Although embodiments of the present invention have been shown and described (see the above detailed description for details), it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for repairing turbine guide ring ablation and block falling damage, Features: The specific steps include: S1: Perform surface treatment and non-destructive testing on the guide ring after service, remove surface attachments and coatings, and mark defects; S2: Perform a three-dimensional scan on the guide ring, compare the point cloud data obtained by the three-dimensional scan with the standard digital model, and according to the comparison result, construct a curved surface along the edge of the serious missing area to cut the standard digital model. The cut part is the defective digital model, and the remaining part is the matrix digital model. Compare the point cloud data with the matrix digital model to confirm that the serious missing area has been cut off; S3: Convert the base model into a CNC machining program used by a five-axis machining center to remove the missing area and process the machined surface into the constructed curved surface shape; S4: Convert the defect digital model into a CNC machining program used by a five-axis machining center to process the raw material into a defect prefabricated part that matches the matrix digital model; S5: Assemble the defective prefabricated part on the guide ring, fix it by spot welding and add brazing material, and then put it into the furnace for brazing; S6: Use non-destructive testing to inspect the repaired area to confirm that there are no defects exceeding the standard; S7: Polish or machine the blade to restore the surface profile, then perform a 3D scan on the guide ring and compare it with the standard digital model to confirm that its dimensions meet the standards.
2. A method for repairing turbine guide ring ablation and chipping damage according to claim 1, Features: In step S2, when the curved surface is constructed and cut to the standard digital model, sharp angles and cross-sectional structures should be avoided to ensure the wetting and spreading of the solder and the absence of stress concentration points in the brazed joint during service.
3. A method for repairing turbine guide ring ablation and chipping damage according to claim 1, Features: In step S2, a processing allowance of 0.1-0.3 mm is added to the outer surface of the cut defective digital model.
4. A method for repairing turbine guide ring ablation and chipping damage according to claim 1, Features: In step S2, the standard for severe missing volume needs to be formulated according to the blade structure, and the areas where the pieces are lost, the ablation exceeds 0.5 mm, and the other missing volume exceeds 1 / 2 of the wall thickness can be selected.
5. A method for repairing turbine guide ring ablation and chipping damage according to claim 1, Features: Step S2, step S3 and step S4 use NX software to cut the digital model and generate the CNC machining program used by the five-axis machining center based on the digital model. Step S3 and step S4 use Vericut multi-axis machining simulation software to simulate the CNC machining program to avoid overcutting, undercutting and machine tool collision during the guide ring machining process.
6. A method for repairing turbine guide ring ablation and chipping damage according to claim 1, Features: In step S4, the raw material is a casting that is cast in the same furnace as the guide ring or has the same material. Before five-axis machining, the casting is rough-machined using a wire cutting method to reduce the time used for five-axis machining.
7. A method for repairing turbine guide ring ablation and chipping damage according to claim 1, Features: In step S5, the solder and brazing system used are determined according to the composition of the guide ring substrate and the structure of the assembly surface. For an assembly surface with a simple structure, paste solder can be directly added to the outer surface of the assembly. For an assembly surface with a complex structure, a solder strip with a thickness of 0.05-0.20 mm must be pasted on the assembly surface in advance, and then paste solder is added to the outer surface of the assembly.
Citation Information
Patent Citations
Method for repairing damaged precision part of turbine
CN105149861A
Double-laser forging remanufacturing and repairing device for damaged mortises of high-temperature alloy small-size structure turbine disc and application method thereof
CN108754490A
Automatic repairing and remanufacturing method of turbine blade
CN111922621A
Brazing repair method for crack damage of multi-union hollow turbine guide blade
CN115709361A
Nozzle segments and method of repairing the same
US20080267775A1
Cited By
Repair method for overtemperature damage of flame tube
CN119589285A
Subway framework welding repair method
CN121223403A
A subway frame repair method
CN121223403B