BOPP (Biaxially-oriented Polypropylene) heat-sealing film and preparation method thereof

Through the design of a three-layer structure film, combined with components such as anti-adhesive, heat sealing, antistatic agent and matting material, the problem of poor heat sealing of BOPP film is solved, the heat sealing strength and gloss are improved, and it is suitable for food packaging.

CN118952803AInactive Publication Date: 2024-11-15TIANJIN HUAHENG PACKAGING MATERIALS

Patent Information

Application Number
CN202411448456.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-17
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Bidirectional tensile polypropylene film (BOPP) has poor heat sealing properties and low heat sealing strength, resulting in a degradation in the performance of packaging films and the inability to achieve long-term protection.

Method used

Using a three-layer structural film formed by polypropylene compositions A, B and C, polypropylene composition A includes anti-adhesive agent, heat seal, homopolypolypropylene and copolymer polypropylene, composition B contains antistatic agent and homopolypolypropylene. Polypropylene, composition C contains matting material and modified nanosilicon dioxide, BOPP heat sealing film is prepared by coextrusion, casting, longitudinal and transverse tensile treatment.

Benefits of technology

It improves the mechanical and physical properties of BOPP heat seal film, heat seal strength, gloss and low haze, and is suitable for various food and fruit and vegetable packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a BOPP (biaxially-oriented polypropylene) heat-sealing film and a preparation method thereof. The heat-sealing film comprises a film A formed by a polypropylene composition A, a film B formed by a polypropylene composition B and a film C formed by a polypropylene composition C, wherein the polypropylene composition A comprises an anti-sticking agent, a heat sealing material, homo-polypropylene, co-polypropylene and chlorinated polypropylene in parts by weight, and the anti-sticking agent comprises an organic anti-sticking agent and an inorganic anti-sticking agent in a mass ratio of (3-5): 1; the polypropylene composition B comprises an antistatic agent and homo-polypropylene; the polypropylene composition C comprises a matting material, an antioxidant and modified nano silicon dioxide, and the matting material comprises high-density polyethylene and polypropylene in a mass ratio of 1: 10. The BOPP heat-sealing film not only has good mechanical and physical properties, but also has higher heat-sealing strength, high glossiness and small haze, and is suitable for packaging various foods, fruits and vegetables and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of packaging films, and in particular relates to a BOPP heat-sealing film and a preparation method thereof. Background Art

[0002] Biaxially oriented polypropylene film (BOPP) has the advantages of being light, transparent, non-toxic, moisture-proof, water-resistant, and having good thermal stability, and is therefore widely used in the packaging of food, candy, cigarettes, tea, medicine, juice, milk, textiles, and the production of adhesive tapes for electrical appliances. However, biaxially oriented polypropylene has poor heat sealing properties and low heat sealing strength. When the heat sealing temperature is too high, the structure of the BOPP film is damaged, resulting in reduced performance of the packaging film and failure to meet the requirements for long-term protection. Summary of the invention

[0003] In view of this, the present invention aims to provide a BOPP heat-sealing film and a preparation method thereof to solve the above problems.

[0004] To achieve the above object, the technical solution of the present invention is achieved as follows: A BOPP heat-sealing film comprises a film A formed by a polypropylene composition A, a film B formed by a polypropylene composition B and a film C formed by a polypropylene composition C; wherein, by weight, the polypropylene composition A comprises 3-5 parts of an anti-sticking agent, 20-30 parts of a heat-sealing material, 60-70 parts of homopolypropylene, 30-50 parts of copolymer polypropylene and 15-25 parts of chlorinated polypropylene, the anti-sticking agent comprises an organic anti-sticking agent and an inorganic anti-sticking agent in a mass ratio of 3-5:1; the polypropylene composition B comprises 1-5 parts of an antistatic agent and 80-100 parts of homopolypropylene; the polypropylene composition C comprises 80-90 parts of a matting material, 1-5 parts of an antioxidant and 1-5 parts of modified nano silicon dioxide, and the matting material comprises high-density polyethylene and polypropylene in a mass ratio of 1:10.

[0005] Further, film A is 2-3 μm, film B is 5-7 μm, film C is 3-4 μm, and film B is sandwiched between film A and film C.

[0006] Furthermore, the organic anti-sticking agent is polymethyl methacrylate and / or polysiloxane, the inorganic anti-sticking agent is silicon dioxide and / or glass microbeads, and the particle size of the inorganic anti-sticking agent is 5-10 μm.

[0007] Furthermore, the heat sealing material is a terpolymer of ethylene, propylene and butene, and the mass ratio of ethylene, propylene and butene is 2:4:1; the chlorine content of chlorinated polypropylene is 20-30%.

[0008] Furthermore, the antistatic agent is a mixture of a cationic antistatic agent and a nonionic antistatic agent, the mass ratio of the two is 1:(6-8), the cationic antistatic agent is a quaternary ammonium salt, and the nonionic antistatic agent is monoglyceride.

[0009] Furthermore, the isotacticity of the polypropylene in the matting material is 75-80%.

[0010] Furthermore, the antioxidant is any one of Antioxidant F802, Antioxidant 168, Antioxidant 626, and Antioxidant 1001.

[0011] Furthermore, the modified nano-silica is prepared by adding silane coupling agent KH570 during the process of preparing nano-silica by sol-gel method, and the particle size of the modified nano-silica is 3-5 μm.

[0012] The present invention also provides a method for preparing the BOPP heat-sealing film as described above, wherein the raw materials of film A, film B and film C are subjected to co-extrusion, casting, longitudinal stretching and transverse stretching to obtain the BOPP heat-sealing film.

[0013] Further, the method specifically includes the following steps: 1) adding the raw material of polypropylene composition B into the main extruder in proportion, and heating to a molten state to prepare the main extrusion melt of polypropylene composition B; adding the raw materials of polypropylene composition A and polypropylene composition C into two auxiliary extruders in proportion, and heating and melting to prepare melts; 2) filtering the melts prepared in step 1) respectively, and then extruding them into a film in a three-layer die head, and then cooling them in a water bath to remove water to obtain a cast sheet; 3) longitudinally stretching the cast sheet obtained in step 2) into a thick sheet, with the preheating temperature being 110-120° C., the stretching temperature being 105-120° C., and the stretching ratio being 4.0-5.0 times; 4) The thick sheet obtained in step 3) is transversely stretched into a film, with a preheating temperature of 165-180°C, a stretching temperature of 155-165°C, a stretching ratio of 5.5-6.5 times, and a setting temperature of 160-170°C; 5) The film obtained in step 4) is subjected to air cooling, flattening, edge trimming, thickness measurement, corona treatment, and then rolled up to obtain a BOPP heat-sealing film.

[0014] Compared with the prior art, the BOPP heat-sealing film of the present invention has the following advantages: The BOPP heat-sealing film of the present invention not only has good mechanical and physical properties, but also has high heat-sealing strength, high gloss and low haze, and is suitable for packaging various foods, fruits and vegetables, etc. DETAILED DESCRIPTION

[0015] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0017] Example 1

[0018] A BOPP heat-sealing film, comprising a film A formed of a polypropylene composition A, a film B formed of a polypropylene composition B, and a film C formed of a polypropylene composition C; the film A is 2 μm, the film B is 5.5 μm, the film C is 3 μm, and the film B is sandwiched between the film A and the film C; Wherein, by weight, the polypropylene composition A comprises 3 parts of anti-adhesive agent, 20 parts of heat-sealing material, 60 parts of homopolypropylene, 40 parts of copolymer polypropylene, and 20 parts of chlorinated polypropylene, the anti-adhesive agent comprises polysiloxane and silicon dioxide in a mass ratio of 3:1, and the silicon dioxide particle size is 10 μm; the heat-sealing material is a terpolymer of ethylene, propylene, and butene, and the mass ratio of ethylene, propylene, and butene is 2:4:1; the chlorine content of the chlorinated polypropylene is 25%; The polypropylene composition B comprises 1.5 parts of an antistatic agent and 80 parts of homopolypropylene; the antistatic agent is a mixture of SH-105 antistatic agent and monoglyceride, with a mass ratio of 1:6; The polypropylene composition C comprises 80 parts of a matting material, 1 part of an antioxidant, and 1.5 parts of modified nano-silica. The matting material comprises high-density polyethylene and polypropylene in a mass ratio of 1:10, the isotacticity of the polypropylene is 80%, the antioxidant is antioxidant F802, and the modified nano-silica is prepared by adding a silane coupling agent KH570 during the preparation of nano-silica by a sol-gel method, and the particle size of the modified nano-silica is 3 μm.

[0019] The preparation method of the above BOPP heat-sealing film comprises the following steps: 1) adding the raw material of polypropylene composition B into the main extruder in proportion, and heating to a molten state to prepare the main extrusion melt of polypropylene composition B; adding the raw materials of polypropylene composition A and polypropylene composition C into two auxiliary extruders in proportion, and heating and melting to prepare melts; 2) filtering the melts prepared in step 1) respectively, and then extruding them into a film in a three-layer die head, and then cooling them in a water bath to remove water to obtain a cast sheet; 3) longitudinally stretching the cast sheet obtained in step 2) into a thick sheet, with a preheating temperature of 110° C., a stretching temperature of 105° C., and a stretching ratio of 4.5 times; 4) The thick sheet obtained in step 3) is transversely stretched into a film, with a preheating temperature of 170°C, a stretching temperature of 165°C, a stretching ratio of 5.5 times, and a setting temperature of 160°C; 5) The film obtained in step 4) is subjected to air cooling, flattening, edge trimming, thickness measurement, corona treatment, and then rolled up to obtain a BOPP heat-sealing film.

[0020] Example 2

[0021] A BOPP heat-sealing film, comprising a film A formed of a polypropylene composition A, a film B formed of a polypropylene composition B, and a film C formed of a polypropylene composition C; the film A is 2.5 μm, the film B is 7 μm, the film C is 3.5 μm, and the film B is sandwiched between the film A and the film C; In terms of weight, the polypropylene composition A comprises 4 parts of anti-adhesive agent, 25 parts of heat-sealing material, 65 parts of homopolymer polypropylene, 30 parts of copolymer polypropylene, and 18 parts of chlorinated polypropylene, wherein the anti-adhesive agent comprises polysiloxane and glass microbeads in a mass ratio of 4:1, and the particle size of the glass microbeads is 7 μm; the heat-sealing material is a terpolymer of ethylene, propylene, and butene, and the mass ratio of ethylene, propylene, and butene is 2:4:1; the chlorine content of the chlorinated polypropylene is 25%; The polypropylene composition B comprises 3 parts of an antistatic agent and 90 parts of homopolypropylene; the antistatic agent is a mixture of SH-105 antistatic agent and monoglyceride, with a mass ratio of 1:7; The polypropylene composition C includes 85 parts of a matting material, 1.5 parts of an antioxidant, and 3 parts of modified nano-silica. The matting material includes high-density polyethylene and polypropylene in a mass ratio of 1:10, the isotacticity of the polypropylene is 80%, the antioxidant is antioxidant F802, and the modified nano-silica is prepared by adding a silane coupling agent KH570 during the preparation of nano-silica by a sol-gel method, and the particle size of the modified nano-silica is 4.5 μm.

[0022] The preparation method is the same as Example 1.

[0023] Example 3

[0024] A BOPP heat-sealing film, comprising a film A formed of a polypropylene composition A, a film B formed of a polypropylene composition B, and a film C formed of a polypropylene composition C; the film A is 3 μm, the film B is 7 μm, the film C is 4 μm, and the film B is sandwiched between the film A and the film C; In terms of weight, the polypropylene composition A comprises 5 parts of an anti-adhesive agent, 30 parts of a heat-sealing material, 70 parts of a homopolymer polypropylene, 40 parts of a copolymer polypropylene, and 25 parts of a chlorinated polypropylene, wherein the anti-adhesive agent comprises polymethyl methacrylate and silicon dioxide in a mass ratio of 5:1, and the silicon dioxide particle size is 5 μm; the heat-sealing material is a terpolymer of ethylene, propylene, and butene, and the mass ratio of ethylene, propylene, and butene is 2:4:1; the chlorine content of the chlorinated polypropylene is 30%; The polypropylene composition B comprises 3 parts of an antistatic agent and 100 parts of homopolypropylene; the antistatic agent is a mixture of SH-105 antistatic agent and monoglyceride, with a mass ratio of 1:8; The polypropylene composition C includes 90 parts of a matting material, 3 parts of an antioxidant, and 5 parts of modified nano-silica. The matting material includes high-density polyethylene and polypropylene in a mass ratio of 1:10, the isotacticity of the polypropylene is 75%, the antioxidant is antioxidant 626, and the modified nano-silica is prepared by adding a silane coupling agent KH570 during the preparation of nano-silica by a sol-gel method, and the particle size of the modified nano-silica is 5 μm.

[0025] The preparation method is the same as Example 1.

[0026] Comparative Example 1 The difference from Example 2 is that the polypropylene in the polypropylene composition A only uses homopolypropylene.

[0027] Comparative Example 2 The difference from Example 2 is that the polypropylene in the polypropylene composition A only uses copolymerized polypropylene.

[0028] Comparative Example 3 The difference from Example 2 is that the polypropylene in the polypropylene composition A only uses chlorinated polypropylene.

[0029] Comparative Example 4 The difference from Example 2 is that the polypropylene composition A includes 3 parts of anti-sticking agent, 20 parts of heat sealing material, 18 parts of homopolypropylene, 25 parts of copolymer polypropylene, and 70 parts of chlorinated polypropylene, and the rest is the same as Example 2.

[0030] Comparative Example 5 The difference from Example 2 is that the chlorine content of the chlorinated polypropylene is 50%.

[0031] Comparative Example 6 The difference from Example 2 is that the anti-sticking agent is polysiloxane.

[0032] Comparative Example 7 The difference from Example 2 is that the anti-sticking agent is glass microbeads.

[0033] Comparative Example 8 The difference from Example 2 is that the anti-sticking agent is polysiloxane and glass microbeads in a mass ratio of 2:1.

[0034] Comparative Example 9 The difference from Example 2 is that the polypropylene composition C does not add modified nano-silica.

[0035] Effect test The BOPP heat-sealing films prepared in Test Examples 1-3 and Comparative Examples 1-9 were tested for tensile strength, heat shrinkage, and heat-sealing strength according to standard GBT10003-2008. The results are shown in Table 1.

[0036] Table 1 Performance test of BOPP heat-sealing films prepared in Examples 1-3 and Comparative Examples 1-11

[0037] As can be seen from the above table, the tensile strength, heat sealing strength, haze and gloss of the BOPP heat-sealing film prepared according to the present invention are better than those of the comparative examples, and have good advantages. By comparing the examples and comparative examples 1-4, it can be found that the comprehensive performance of homopolypropylene, copolymer polypropylene and chlorinated polypropylene is better when used together. If the proportion of these three exceeds the proportion specified in this application, it will also lead to performance degradation; it can be seen from comparative example 5 that the chlorine content of chlorinated polypropylene will affect the heat sealing strength; the main function of the anti-adhesive agent is to prevent the film from sticking to each other. The films of Examples 1-3 do not have the phenomenon of film sticking to each other, while comparative examples 6-8 have different degrees of adhesion, indicating that the anti-adhesive agent can better solve the adhesion phenomenon by using organic anti-adhesive agent and inorganic anti-adhesive agent according to the specified mass ratio. In addition, it can be seen from Table 1 that the anti-adhesive agent will also affect the haze and gloss; the polypropylene composition C of comparative example 9 does not add modified nano-silica, which will affect the tensile strength and heat sealing strength of the film to a certain extent.

[0038] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A BOPP heat-sealing film, characterized in that: The invention comprises a film A formed by a polypropylene composition A, a film B formed by a polypropylene composition B and a film C formed by a polypropylene composition C; wherein, by weight, the polypropylene composition A comprises 3-5 parts of an anti-sticking agent, 20-30 parts of a heat-sealing material, 60-70 parts of homopolypropylene, 30-50 parts of copolymer polypropylene and 15-25 parts of chlorinated polypropylene, and the anti-sticking agent comprises an organic anti-sticking agent and an inorganic anti-sticking agent in a mass ratio of 3-5:1; the polypropylene composition B comprises 1-5 parts of an antistatic agent and 80-100 parts of homopolypropylene; the polypropylene composition C comprises 80-90 parts of a matting material, 1-5 parts of an antioxidant and 1-5 parts of modified nano-silicon dioxide, and the matting material comprises high-density polyethylene and polypropylene in a mass ratio of 1:

10.

2. The BOPP heat-sealing film according to claim 1, characterized in that: Film A is 2-3 μm, film B is 5-7 μm, film C is 3-4 μm, and film B is sandwiched between film A and film C.

3. The BOPP heat-sealing film according to claim 1, characterized in that: The organic anti-sticking agent is polymethyl methacrylate and / or polysiloxane, the inorganic anti-sticking agent is silicon dioxide and / or glass microbeads, and the particle size of the inorganic anti-sticking agent is 5-10 μm.

4. The BOPP heat-sealing film according to claim 1, characterized in that: The heat sealing material is a terpolymer of ethylene, propylene and butene, and the mass ratio of ethylene, propylene and butene is 2:4:1; the chlorine content of chlorinated polypropylene is 20-30%.

5. The BOPP heat-sealing film according to claim 1, characterized in that: The antistatic agent is a mixture of a cationic antistatic agent and a nonionic antistatic agent, and the mass ratio of the two is 1: (6-8). The cationic antistatic agent is a quaternary ammonium salt, and the nonionic antistatic agent is a monoglyceride.

6. The BOPP heat-sealing film according to claim 1, characterized in that: The isotacticity of polypropylene in the matting material is 75-80%.

7. The BOPP heat-sealing film according to claim 1, characterized in that: The antioxidant is any one of antioxidant F802, antioxidant 168, antioxidant 626, and antioxidant 1001.

8. The BOPP heat-sealing film according to claim 1, characterized in that: The modified nano silicon dioxide is prepared by adding silane coupling agent KH570 during the process of preparing nano silicon dioxide by sol-gel method. The particle size of the modified nano silicon dioxide is 3-5 μm.

9. A method for preparing a BOPP heat-sealing film according to any one of claims 1 to 8, characterized in that: The raw materials of film A, film B and film C are subjected to co-extrusion, sheet casting, longitudinal stretching and transverse stretching to obtain the BOPP heat-sealing film.

10. The method for preparing a BOPP heat-sealing film according to claim 9, characterized in that: The specific steps include: 1) adding the raw material of polypropylene composition B into the main extruder in proportion, and heating to a molten state to prepare the main extrusion melt of polypropylene composition B; adding the raw materials of polypropylene composition A and polypropylene composition C into two auxiliary extruders in proportion, and heating and melting to prepare melts; 2) filtering the melts prepared in step 1) respectively, and then extruding them into a film in a three-layer die head, and then cooling them in a water bath to remove water to obtain a cast sheet; 3) longitudinally stretching the cast sheet obtained in step 2) into a thick sheet, with the preheating temperature being 110-120° C., the stretching temperature being 105-120° C., and the stretching ratio being 4.0-5.0 times; 4) The thick sheet obtained in step 3) is transversely stretched into a film, with a preheating temperature of 165-180°C, a stretching temperature of 155-165°C, a stretching ratio of 5.5-6.5 times, and a setting temperature of 160-170°C; 5) The film obtained in step 4) is subjected to air cooling, flattening, edge trimming, thickness measurement, corona treatment, and then rolled up to obtain a BOPP heat-sealing film.

Citation Information

Patent Citations

  • Matte BOPP film and preparation method thereof

    CN105128472A

  • BOPP heat-seal film for matte metallized label and preparation method thereof

    CN111703164A

  • Polypropylene composition as well as preparation method and application thereof

    CN115403870A

Cited By

  • Composite film, packaging material containing composite film, packaging mode and application of packaging material

    CN119567687A

  • A composite film, a packaging material comprising the composite film, a packaging method thereof, and its application.

    CN119567687B

  • BOPP (Biaxially-oriented Polypropylene) high-haze extinction type heat-sealing film and preparation method thereof

    CN120348043A