Preparation method of phenolic resin-based hard carbon microspheres with large interlayer spacing
By preparing highly cross-linked phenolic resin microspheres through a double cross-linking process, the problems of toxicity and small interlayer spacing in sodium-ion battery anode materials were solved, and the high reversible capacity and electrochemical performance were improved.
Patent Information
- Application Number
- CN202411007207.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing sodium-ion battery anode materials suffer from high toxicity, low molecular cross-linking degree, and small interlayer spacing, resulting in low reversible capacity and poor cycle capacity.
A double crosslinking process was adopted, using aminophenol with self-catalytic activity as the phenol source, carboxylic aldehyde as the main crosslinking agent, and organic diamine as the co-crosslinking agent. The crosslinking reaction was carried out in an aqueous solvent to form highly crosslinked phenolic resin microspheres, which were then carbonized to prepare hard carbon microspheres with large interlayer spacing.
A green and environmentally friendly method for preparing highly cross-linked phenolic resin microspheres was achieved, which suppressed the graphitization tendency during the carbonization process, improved the interlayer spacing and reversible capacity of hard carbon microspheres, and enhanced electrochemical performance.
Smart Images

Figure CN118954471A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of negative electrode materials for sodium ion batteries, and in particular to a method for preparing negative electrode materials of phenolic resin microspheres with high cross-linking degree and carbon microspheres with large interlayer spacing by using a double cross-linking process and application thereof. Background Art
[0002] With the application in large-scale energy storage, sodium-ion batteries have gradually become an effective alternative to lithium-ion batteries due to their abundant sodium resources and high safety. However, sodium-ion batteries are still in the research and development stage, especially in the research and development of negative electrode materials. Among the existing negative electrode materials, hard carbon materials have the advantages of rich sodium storage sites, low sodium storage potential, and good chemical and thermal stability, showing great application potential. Therefore, in response to the needs of commercialization of sodium-ion batteries, the development of low-cost, high-performance hard carbon negative electrode materials has become a top priority.
[0003] Among the many precursors for preparing hard carbon materials, phenolic resin is widely used due to its advantages such as strong structural designability, high carbon yield and mature preparation process. However, the cross-linking agent used in the existing synthesis of phenolic resin is often formaldehyde, which is highly toxic and volatile, causing harm to people and the environment, and is not in line with the development concept of green environmental protection. In addition, the molecular cross-linking degree of the phenolic resin synthesized by formaldehyde is relatively low, and phenolic resin-based hard carbon negative electrode materials usually show a high graphitization tendency and a small interlayer spacing. This leads to problems such as low reversible capacity and poor cycle capacity. Summary of the invention
[0004] In view of the above problems, the present invention provides a green, environmentally friendly and simple double cross-linking process for synthesizing phenolic resin microspheres with a high degree of cross-linking and deriving hard carbon microspheres with a large interlayer spacing structure.
[0005] The method of the present invention selects aminophenol with self-catalytic effect as a phenol source, selects carboxylic acid aldehyde as a main cross-linking agent, selects organic diamine as an auxiliary cross-linking agent, and performs a cross-linking reaction at room temperature with water as a solvent to synthesize phenolic resin microspheres. In the reaction, the active hydrogen of the aromatic hydrocarbon of the phenol source reacts with the aldehyde group in the main cross-linking agent through electrophilic substitution to form an -ArCH2COOH structure; then, the negatively charged carboxylic acid in -ArCH2COOH reacts with the positively charged amine group in the auxiliary cross-linking agent, so that the auxiliary cross-linking agent is integrated into the main chain of the phenolic resin. Due to the different action mechanisms and reaction sites of the two cross-linking agents, the synthesized phenolic resin has a developed three-dimensional network structure, and the degree of cross-linking is greatly improved. This will avoid its tendency to excessive graphitization during the carbonization process, so that a hard carbon microsphere negative electrode material with a large interlayer spacing and a high degree of disorder can be prepared.
[0006] The present invention provides the following technical solutions:
[0007] A method for preparing phenolic resin-based hard carbon microspheres with a large interlayer spacing structure using a double cross-linking agent comprises the following steps:
[0008] (1) A phenol source is dissolved in deionized water to prepare solution A; a primary crosslinking agent and an auxiliary crosslinking agent are dissolved in deionized water to prepare solution B; solution B is then added to solution A at a uniform rate, and reacted at room temperature for a period of time, and phenolic resin microspheres are obtained after centrifugation, washing and drying.
[0009] (2) Carbonizing the phenolic resin microspheres obtained in step (1) under an inert gas atmosphere to obtain hard carbon microspheres. Preferably, the phenol source in step (1) is one of 3-aminophenol, 2-aminophenol, 4-aminophenol, 4-methylaminophenol, 3-diethylaminophenol, 4-acetaminophenol, 2-acetaminophenol, 4-methylaminophenol, 6-acetaminophenol, and 4-methylaminophenol.
[0010] Preferably, the concentration of the phenol source in solution A in step (1) is 5-40 g / L.
[0011] Preferably, the main cross-linking agent in step (1) is one of glyoxylic acid, propionaldehyde acid and D-glucuronic acid.
[0012] Preferably, the auxiliary cross-linking agent in step (1) is one of triethylenediamine, diethylenetriamine, triethylenetetramine and hexamethylenetetramine.
[0013] Preferably, the concentrations of the primary crosslinking agent and the auxiliary crosslinking agent in step (1) are 5-50 g / L and 2-35 g / L, respectively, in solution B. Preferably, the molar ratio of the phenol source / primary crosslinking agent / auxiliary crosslinking agent in step (1) is 1:0.2:0.2 to 1:4:4.
[0014] Preferably, the reaction time in step (1) is 5-60 min.
[0015] Preferably, the inert gas in step (2) is nitrogen or argon.
[0016] Preferably, the carbonization temperature in step (2) is 1000-1600°C.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The acetal main cross-linking agent and the auxiliary cross-linking agent used in the phenolic resin prepared by the present invention have low volatility, and the generation of highly toxic formaldehyde gas can be avoided during use, thereby achieving the concept of green environmental protection.
[0019] (2) Compared with the formaldehyde crosslinking agent system, the double crosslinking system gives the phenolic resin molecules a highly crosslinked three-dimensional structure, which effectively inhibits the graphitization tendency during the carbonization process and increases the interlayer spacing of the graphite layer.
[0020] (3) Compared with the hard carbon materials prepared by formaldehyde crosslinking agent, the hard carbon microspheres prepared by the double crosslinking process exhibit higher reversible capacity and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Attached Figure 1 This is a scanning electron microscope (SEM) image of the phenolic resin-based hard carbon microspheres obtained in Example 1.
[0022] Attached Figure 2 This is the SEM image of the phenolic resin-based hard carbon microspheres obtained in Example 2.
[0023] Attached Figure 3 This is a high resolution transmission (HRTEM) image of the phenolic resin hard carbon microspheres obtained in Example 2.
[0024] Attached Figure 4 This is the SEM image of the phenolic resin-based hard carbon microspheres obtained in Comparative Example 1.
[0025] Attached Figure 5 This is the HRTEM image of the phenolic resin-based hard carbon microspheres obtained in Comparative Example 1.
[0026] Attached Figure 6 The constant current charge and discharge curves of the hard carbon microspheres obtained in Example 2 and Comparative Example 1 are shown. DETAILED DESCRIPTION
[0027] The present invention is further explained below by specific examples, but the scope of the present invention is not limited to the following examples. Without departing from the concept of the present invention, various substitutions or changes made according to common technical knowledge and customary means in the art should be included in the scope of the present invention:
[0028] Example 1
[0029] (1) Disperse 4.4 g of 3-aminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.8 g of glyoxylic acid and 1.8 g of triethylenediamine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.4). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0030] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1100° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres. Figure 1 As shown, the reaction is incomplete at this temperature, the hard carbon microspheres are irregular in shape and there is fusion phenomenon.
[0031] Example 2
[0032] (1) Disperse 4.4 g of 3-aminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.8 g of glyoxylic acid and 1.8 g of triethylenediamine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.4). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0033] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres. Figure 1 As shown in Figure 2, the hard carbon microspheres synthesized under the action of the double crosslinking agent are irregularly spherical and have a large average particle size of about 980nm. As attached Figure 2 shown.
[0034] Example 3
[0035] (1) Disperse 4.4 g of 3-aminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.8 g of glyoxylic acid and 1.8 g of triethylenediamine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.4). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0036] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1500° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0037] Example 4
[0038] (1) Disperse 4.4 g of 3-aminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.8 g of glyoxylic acid and 1.6 g of triethylenediamine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.35). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0039] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0040] Example 5
[0041] (1) Disperse 4.4 g of 3-aminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.8 g of glyoxylic acid and 1.2 g of triethylenediamine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.25). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0042] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0043] Example 6
[0044] (1) Disperse 4.4 g of 4-aminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.8 g of glyoxylic acid and 2.0 g of hexamethylenetetramine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.35). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0045] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0046] Example 7
[0047] (1) Disperse 4.4 g of 4-aminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.8 g of glyoxylic acid and 1.4 g of hexamethylenetetramine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.25). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0048] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0049] Example 8
[0050] (1) Disperse 4.4 g of 3-aminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.8 g of glyoxylic acid and 1.0 g of diethylenetriamine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.25). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0051] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0052] Example 9
[0053] (1) Disperse 4.4 g of 3-aminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.8 g of glyoxylic acid and 1.5 g of triethylenetetramine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.25). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0054] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0055] Example 10
[0056] (1) Disperse 4.4 g of 3-aminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.8 g of glyoxylic acid and 1.4 g of hexamethylenetetramine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.25). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0057] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0058] Embodiment 11
[0059] (1) Disperse 4.4 g of 4-aminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.8 g of glyoxylic acid and 1.6 g of triethylenediamine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.35). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0060] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0061] Example 12
[0062] (1) Disperse 4.4 g of 4-methylaminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.0 g of glyoxylic acid and 1.4 g of triethylenediamine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.35). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0063] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0064] Embodiment 13
[0065] (1) Disperse 4.4 g of 3-diethylaminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 3.7 g of glyoxylic acid and 1.1 g of triethylenediamine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.35). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0066] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0067] Embodiment 14
[0068] (1) Disperse 4.4 g of 3-diethylaminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 4.0 g of glyoxylic acid and 1.3 g of hexamethylenetetramine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.2:0.35). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0069] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0070] Embodiment 15
[0071] (1) Disperse 4.4 g of 4-methylaminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.0 g of glyoxylic acid and 1.3 g of hexamethylenetetramine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.25). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0072] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0073] Example 16
[0074] (1) Disperse 4.4 g of 4-methylaminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 6.0 g of glyoxylic acid and 1.3 g of hexamethylenetetramine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.8:0.25). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0075] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0076] Embodiment 17
[0077] (1) Disperse 4.4 g of 4-methylaminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.2 g of D-glucuronic acid and 1.6 g of triethylenediamine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1:0.35). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0078] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0079] Embodiment 18
[0080] (1) Disperse 4.4 g of 3-diethylaminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 3.7 g of glyoxylic acid and 1.3 g of hexamethylenetetramine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.5:0.35). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0081] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0082] Embodiment 19
[0083] (1) Disperse 4.4 g of 3-diethylaminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.5 g of glyoxylic acid and 1.3 g of hexamethylenetetramine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1.8:0.35). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0084] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0085] Embodiment 20
[0086] (1) Disperse 4.4 g of 3-diethylaminophenol in 300 mL of deionized water and stir for 15 min to obtain a clear solution. Disperse 5.2 g of D-glucuronic acid and 1.6 g of triethylenediamine in 200 mL of deionized water and stir for 15 min to obtain a clear solution (phenol source / primary crosslinking agent / auxiliary crosslinking agent molar ratio 1:1:0.35). Then, mix the two solutions at a uniform speed and react for 30 min. Finally, centrifuge, wash with water and dry to obtain phenolic resin microspheres.
[0087] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0088] Comparative Example 1
[0089] (1) 2 g of 3-aminophenol was dispersed in 300 mL of deionized water and stirred for 15 min until a clear solution was obtained. Then, 1.6 mL of formaldehyde (phenol source / formaldehyde molar ratio was 1:2.4) was dropped into the solution and reacted for 30 min. Finally, the phenolic resin microspheres were obtained by centrifugation, washing with water and drying.
[0090] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres. Figure 2 As shown, the hard carbon microspheres synthesized in the presence of formaldehyde crosslinking agent are regular spherical with a small average particle size of about 668nm. Comparative Example 2
[0091] (1) 2 g of 3-aminophenol was dispersed in 300 mL of deionized water and stirred for 15 min until a clear solution was obtained. Then, 2.0 mL of formaldehyde (phenol source / formaldehyde molar ratio was 1:3) was dropped into the solution and reacted for 50 min. Finally, the phenolic resin microspheres were obtained by centrifugation, washing with water and drying.
[0092] (2) The phenolic resin microspheres obtained in step (1) are carbonized at 1300° C. for 2 h under an argon atmosphere to obtain phenolic resin-based hard carbon microspheres.
[0093] The hard carbon, carbon black and binder obtained in Examples 1-20 and Comparative Examples 1-2 were respectively mixed and ground in a mass ratio of 8:1:1, and NMP was added dropwise to make a uniform slurry which was coated on copper foil, and then vacuum dried, cut into pieces and assembled into batteries for electrochemical testing.
[0094] The following table compares the interlayer spacing and reversible capacity of the phenolic resin-based hard carbon microsphere materials obtained in Examples 1-20 and Comparative Examples 1-2.
[0095]
[0096]
[0097] It can be seen from the table that the interlayer spacing and reversible capacity of the hard carbon material prepared using the double cross-linking agent are higher than those of the hard carbon material prepared using the formaldehyde system.
[0098] It can be seen from Comparative Example 1 that under the condition of the presence of only formaldehyde crosslinking agent, the interlayer spacing and reversible capacity of the hard carbon are greatly reduced; even if the amount of crosslinking agent is increased and the reaction time is prolonged (Comparative Example 2), the interlayer spacing and reversible capacity of the hard carbon are only slightly increased, indicating that the presence of a single crosslinking agent limits the crosslinking degree of the phenolic resin molecules.
[0099] From Examples 1-20, we can see the influence of the double crosslinking agent on the interlayer spacing and electrochemical performance of hard carbon materials. In Examples 1-3, as the carbonization temperature increases, the interlayer spacing of hard carbon gradually increases, while the reversible capacity increases first and then decreases, which indicates that the carbonization temperature affects the development of the graphite layer. When the interlayer spacing is small, it is not conducive to the Na + Intercalation, while too large will form pseudo adsorption. In Example 2 and Examples 4-7, as the content of the auxiliary crosslinking agent decreases, the interlayer spacing and reversible capacity of the hard carbon material gradually decrease, indicating that the presence of the auxiliary crosslinking agent can indeed affect the microstructure of the hard carbon, which can change the crosslinking degree of the phenolic resin molecular structure. In Examples 8-20, by changing the ratio and type of phenol source / main crosslinking agent / auxiliary crosslinking agent, the interlayer spacing and reversible capacity of the hard carbon material also change, indicating that the crosslinking activity is affected by the structure of the monomer and the crosslinking agent.
Claims
1. A method for preparing large interlayer spacing phenolic resin-based hard carbon microspheres, characterized in that: The specific steps include: Step 1: dissolving a phenol source in deionized water to prepare solution A; then dissolving a primary crosslinking agent and an auxiliary crosslinking agent in deionized water to prepare solution B; then adding solution B to solution A at a uniform rate, reacting at room temperature for a period of time, and obtaining phenolic resin microspheres after centrifugation, washing and drying. Step 2: Carbonizing the phenolic resin microspheres obtained in step 1 under an inert gas atmosphere to obtain hard carbon microspheres.
2. The preparation method according to claim 1, characterized in that The phenol source in step 1 is one of 3-aminophenol, 2-aminophenol, 4-aminophenol, 4-methylaminophenol, 3-diethylaminophenol, 4-acetaminophenol, o-acetaminophenol, and 4-methyl-6-acetaminophenol.
3. The preparation method according to claim 1, characterized in that The concentration of the phenol source in the solution A in step 1 is 5-40 g / L.
4. The preparation method according to claim 1, characterized in that The main cross-linking agent in step 1 is one of glyoxylic acid, propionaldehyde acid and D-glucuronic acid.
5. The preparation method according to claim 1, characterized in that The auxiliary cross-linking agent in step 1 is one of triethylenediamine, diethylenetriamine, triethylenetetramine and hexamethylenetetramine.
6. The preparation method according to claim 1, characterized in that The concentrations of the main cross-linking agent and the auxiliary cross-linking agent in solution B in step 1 are 5-50 g / L and 2-35 g / L respectively.
7. The preparation method according to claim 1, characterized in that The molar ratio of the phenol source / main cross-linking agent / auxiliary cross-linking agent in step 1 is 1:0.2:0.2 to 1:4:
4.
8. The preparation method according to claim 1, characterized in that The reaction time in step 1 is 5-60 min.
9. The preparation method according to claim 1, characterized in that The inert gas in step 2 is nitrogen or argon.
10. The preparation method according to claim 1, characterized in that The carbonization temperature in step 2 is 1000-1600°C.
Citation Information
Patent Citations
Carbon material, use thereof in a battery, method for preparing said material and electrode comprising said material
CN115279689A
Crosslinking agent, crosslinked polymer and their uses
JP2010077385A
Cited By
Hard carbon negative electrode material and preparation method and application thereof
CN122136357A