T2 / O2 / O3 configuration lithium ion battery positive electrode material and rapid preparation method and application thereof
The positive electrode material of T2/O2/O3 configuration lithium-ion battery was prepared by high-temperature calcination method and array microwave-assisted molten salt ion exchange method, which solved the problems of slow and uneven reaction speed in the prior art, and achieved an efficient and uniform preparation process and excellent cycle performance, suitable for large-scale production.
Patent Information
- Application Number
- CN202411033945.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing T2/O2/O3 configuration lithium-ion battery positive electrode material preparation method has slow reaction speed and is uneven, which cannot meet the needs of large-scale production.
High-temperature calcination combined with array microwave auxiliary molten salt ion exchange method, sodium-containing layered oxide is synthesized through high-temperature calcination, and then mixed with lithium-containing composite molten salt, and ion exchange is performed using array microwave heating to prepare high capacity and stable structure T2/O2/O3 configuration lithium-ion battery positive electrode material.
The reaction speed is significantly accelerated, the product cycle stability and consistency is good, the process is simple, the reaction is uniform and sufficient, and it is suitable for industrial production. The capacity retention rate of the prepared materials is as high as more than 97% after 50 cycles.
Smart Images

Figure CN118954626A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion battery positive electrode materials, and in particular relates to a T2 / O2 / O3 configuration lithium ion battery positive electrode material and a rapid preparation method and application thereof. Background Art
[0002] High-power, high-energy-density lithium-ion batteries have become a research hotspot due to their wide applications in electric vehicles, portable electronic devices, and power grids. The cost of lithium-ion batteries is mainly determined by the cathode material, so the development of cathode materials with high performance has become a key point for breakthroughs. So far, the mainstream cathode materials on the market include: LiFePO4, LiCoO2, LiMn2O4, and ternary materials. LiFePO4 batteries have low energy density and poor low-temperature performance, making them unsuitable for industrial production. The scarcity of cobalt resources in LiCoO2 has led to high production costs for LiCoO2 batteries, and their thermal stability is poor, and thermal runaway is prone to occur at high temperatures. Although LiMn2O4 has a relatively low cost, its energy density is low and its cycle life is short. Lithium nickel cobalt manganese oxide Li(Ni,Co,Mn)O2 has a high energy density and good safety performance, and is expected to achieve high performance and long cycles, and has attracted attention and research.
[0003] The positive electrode materials with T2 / O2 / O3 configuration are widely used and studied in the fields of lithium-ion batteries and sodium-ion batteries. Among them, the T2 configuration positive electrode material is a relatively novel structure, and its specific characteristics and applications are still under in-depth research. The T2 configuration lithium nickel cobalt manganese oxide positive electrode material has a two-dimensional lithium ion transmission path. This structure helps the rapid movement of lithium ions in the electrode material, thereby improving the battery's charge and discharge efficiency, and the T2 configuration material can work at high voltage, which means that the battery can store more energy. O2 configuration positive electrode materials generally refer to layered oxide positive electrode materials with a specific oxygen stacking arrangement (such as ABAB stacking). The oxygen atoms in the O2 configuration are arranged in an ABAC stacking manner. Because the Li-O octahedron in the lithium layer and the TM-O octahedron in the transition metal layer are in face-to-face contact, the migration of transition metal ions is avoided, which can effectively inhibit irreversible phase changes and voltage decay. O3-configuration cathode material is the most common structure among layered oxide cathode materials. Its oxygen atoms are arranged in a cubic close-packed manner (i.e., ABCABC stacking). O3-configuration cathode materials have a high capacity and are suitable for electric vehicles, large-scale energy storage, and other fields. The preparation methods of the above three T2 / O2 / O3-configuration cathode materials are mainly molten salt ion exchange methods, that is, through simple solid phase grinding, Li + / Na +The exchange results in T2 / O2 / O3 materials, but this method has an inevitable problem - the reaction speed is slow (the conventional ion exchange method takes about 4h-8h) and uneven (the reaction is incomplete during the ion exchange process and it is difficult to obtain a pure phase), which is particularly obvious in the scale-up experiment. Therefore, exploring a new simple and fast method that allows uniform and complete reactions is an important topic in the field of lithium-ion batteries. Summary of the invention
[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a T2 / O2 / O3 configuration lithium-ion battery positive electrode material and a rapid preparation method and application thereof, so as to solve the technical problems of the existing methods such as slow reaction speed, uneven reaction, and inability to scale up production on a large scale.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The invention discloses a method for rapidly preparing a positive electrode material of a lithium-ion battery with a T2 / O2 / O3 configuration. The invention is that a high-temperature calcination method combined with array microwave-assisted molten salt ion exchange can rapidly prepare a target product with high capacity and stable structure. The method specifically comprises: firstly, a sodium-containing layered oxide Na is synthesized by a high-temperature calcination method. m Ni x Co y Mn 1-x-y O2, and then mixed it with 1 to 10 times the molar amount of lithium-containing composite molten salt, subjected to ion exchange treatment by array microwave heating, and then washed and dried to obtain a T2 / O2 / O3 configuration lithium-ion battery positive electrode material;
[0007] Among them, 0.70≤m≤1.00, 0.00≤x≤1.00; 0.00≤y≤1.00.
[0008] The present invention discloses a method for preparing a positive electrode material of a T2 / O2 / O3 structured lithium-ion battery, which specifically comprises the following steps:
[0009] 1) Weighing
[0010] According to Na m Ni x Co y Mn 1-x-y The precursor particles and the sodium source are weighed and then mixed thoroughly to obtain a mixture; wherein 0.70≤m≤1.00, 0.00≤x≤1.00; 0.00≤y≤1.00;
[0011] 2) High temperature calcination
[0012] The mixture obtained in step 1) is pre-calcined at 400-600° C. for 2-5 hours, then calcined at 700-900° C. for 5-30 hours, and then naturally cooled to room temperature to obtain a sodium-containing intermediate product;
[0013] 3) Array microwave-assisted molten salt ion exchange
[0014] The sodium-containing intermediate product is uniformly mixed with 1 to 10 times the molar amount of lithium-containing composite molten salt, and array microwave heating is performed at 200 to 300° C. for 5 to 60 minutes. The product is then filtered, washed, and dried to obtain a T2 / O2 / O3 configuration lithium-ion battery positive electrode material.
[0015] Preferably, in step 1), the precursor particles include a nickel source, a cobalt source and a manganese source;
[0016] The nickel source is selected from any one of Ni(NO3)2·6H2O, Ni(CH3COO)2·4H2O, NiO, Ni(OH)2, NiCO3 and NiC2O4;
[0017] The cobalt source is selected from any one of Co(NO3)2·6H2O, Co(CH3COO)2·4H2O, Co3O4, Co(OH)2, CoCO3 and CoC2O4;
[0018] The manganese source is selected from any one of Mn(NO3)2·4H2O, Mn(CH3COO)2·4H2O, Mn3O4, MnO2, Mn(OH)2, MnCO3 and MnC2O4.
[0019] Preferably, in step 1), the sodium salt is selected from any one of Na2CO3, NaOH, NaNO3 or CH3COONa.
[0020] Preferably, in step 2), the temperature is raised from room temperature to 400-600° C. at a heating rate of 3-10° C. / min, pre-fired for 2-5 h, and then calcined at 700-900° C. for 5-30 h.
[0021] Preferably, in step 3), the lithium-containing composite molten salt is a mixture of LiNO3 and other molten salts, and the other molten salts are selected from any one of LiCl, KCl, NaCl, KNO3 and NaNO3.
[0022] Preferably, in step 3), the temperature is increased from room temperature to 200-300° C. at a heating rate of 10-30° C. / min, and the reaction time is 5-60 min.
[0023] The present invention also discloses a T2 / O2 / O3 configuration lithium ion battery positive electrode material prepared by the above preparation method, characterized in that the T2 / O2 / O3 configuration lithium ion battery positive electrode material is composed of micron-sized particles.
[0024] Preferably, the capacity retention rate of the T2 / O2 / O3 lithium-ion battery positive electrode material is as high as 97% or more after 50 cycles under the conditions of 2.0-4.8V and 0.1C.
[0025] The invention also discloses the application of the above-mentioned T2 / O2 / O3 configuration lithium ion battery positive electrode material in the preparation of lithium ion batteries.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The rapid preparation method disclosed by the present invention adopts Li + / Na + Ion exchange method, firstly synthesizes sodium-containing layered oxide Na by high temperature calcination m Ni x Co y Mn 1-x-y O2, and then fully mix it with molten salt, perform ion exchange through rapid array microwave heating, and obtain T2 / O2 / O3 Li after filtering, washing and drying. m Ni x Co y Mn 1-x-y O2 layered oxide. Since the array microwave has higher heating power, fast and uniform heating speed, the T2 / O2 / O3 phase layered structure positive electrode material prepared by this method has excellent cycle stability. This method provides an effective and feasible way to prepare lithium nickel cobalt manganese layered positive electrode materials, and is expected to play an important role in the field of lithium ion batteries; the preparation method has good consistency, extremely fast reaction speed, simple process, uniform and sufficient reaction, and the product yield of the process for preparing T2 / O2 / O3 configuration lithium nickel cobalt manganese positive electrode materials by the method of the present invention is as high as 90%, the operation is simple, and it is conducive to scale-up industrial production.
[0028] The T2 / O2 / O3 configuration lithium ion battery positive electrode material prepared by the method of the present invention is a type of lithium nickel cobalt manganese positive electrode material Li(Ni, Co, Mn)O2, which has excellent cycle performance. Under the conditions of 2.0-4.8V and 0.1C, the capacity retention rate of the material is still as high as over 97% after 50 cycles. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Schematic diagram of the reaction device used in the preparation method of the present invention.
[0030] Figure 2 This is the first charge and discharge curve of the O2-type positive electrode material prepared in Example 1 of the present invention at a rate of 0.1C.
[0031] Figure 3 This is the X-ray diffraction spectrum of the O2-type positive electrode material sodium electrode precursor prepared in Example 2 of the present invention.
[0032] Figure 4 This is a scanning electron microscope image of the O2-type positive electrode material sodium electrode precursor prepared in Example 3 of the present invention.
[0033] Figure 5 This is the X-ray diffraction spectrum of the T2 type positive electrode material prepared in Example 4 of the present invention.
[0034] Figure 6 This is the X-ray diffraction spectrum of the O2 type positive electrode material prepared in Example 5 of the present invention.
[0035] Figure 7 This is the X-ray diffraction spectrum of the O3 type positive electrode material prepared in Example 6 of the present invention.
[0036] Figure 8 This is a scanning electron microscope image of the T2 type positive electrode material prepared in Example 7 of the present invention.
[0037] Fig. 9 This is the first charge and discharge curve of the O2-type positive electrode material prepared in Example 8 of the present invention at a rate of 0.1C.
[0038] Fig.10 This is a cycle performance diagram of the O2 type positive electrode material prepared in Example 8 of the present invention. DETAILED DESCRIPTION
[0039] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0040] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0041] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0042] Example 1
[0043] In this embodiment, the ingredients are prepared according to the chemical formula LiCoO2.
[0044] A method for preparing an O2 type lithium nickel cobalt manganese positive electrode material comprises the following steps:
[0045] Step 1. Weighing:
[0046] A certain mass of CoCO3 and Na2CO3 was weighed according to the molar ratio, and then placed in a ball mill and mixed thoroughly for 5 h.
[0047] Step 2. High temperature calcination:
[0048] The mixture obtained in step 1 is heated to 400° C. at a heating rate of 8° C. / min, pre-calcined for 3 h, and then calcined at 900° C. for 10 h, and then naturally cooled to room temperature to obtain a sodium-containing intermediate product.
[0049] Step 3. Array microwave-assisted molten salt ion exchange:
[0050] The sodium-containing intermediate product obtained in step 3 was evenly mixed with 3 times the molar amount of LiNO3 / NaCl molten salt by ball milling, and microwave heating was reacted at 200°C for 30 minutes, and then the product was filtered, washed and dried to obtain the target product. The specific reaction device diagram is shown in Figure 1 .
[0051] The charging and discharging performance test process of the positive electrode material prepared in this example is as follows:
[0052] The O2-type positive electrode material, acetylene black and polyvinylidene fluoride (PVDF) prepared in this embodiment were weighed at a mass ratio of 80:10:10, added to N-methylpyrrolidone to form a slurry, evenly coated on an aluminum foil, and dried in a drying oven at 80°C and a vacuum degree of -0.094 MPa for 12 hours. Then, the electrodes were cut into electrodes with a diameter of 12 mm using a mold, and the electrodes were compacted under a pressure of 20 MPa to form the final positive electrode electrodes. Metal lithium sheets were used as negative electrodes and Celgard2400 was used as diaphragms, and button batteries with a model of CR2032 were assembled in a glove box filled with inert gas.
[0053] The battery electrical performance test was carried out at a voltage range of 3 to 4.6 V and a current density of 0.1 C. The results showed that the positive electrode material prepared in this embodiment had an initial discharge capacity of more than 210 mAh / g at a rate of 0.1 C. Figure 2 .
[0054] Example 2
[0055] In this embodiment, according to the chemical formula Li 0.8 NiO2 ingredients.
[0056] A method for preparing an O2 type lithium nickel cobalt manganese positive electrode material comprises the following steps:
[0057] Step 1. Weighing:
[0058] A certain mass of Ni(OH)2 and NaOH were weighed according to the molar ratio, and then placed in a ball mill and mixed thoroughly for 2 h.
[0059] Step 2. High temperature calcination:
[0060] The mixture obtained in step 1 is heated to 500° C. at a heating rate of 3° C. / min, pre-calcined for 2 h, and then calcined at 700° C. for 30 h, and then naturally cooled to room temperature to obtain a sodium-containing intermediate product.
[0061] Step 3. Array microwave-assisted molten salt ion exchange
[0062] The sodium-containing intermediate product obtained in step 2 was evenly mixed with 8 times the molar amount of LiNO3 / LiCl molten salt by ball milling, and microwave heating was reacted at 300°C for 20 minutes, and then the product was filtered, washed and dried to obtain the target product. The specific reaction device diagram is shown in Figure 1 .
[0063] The Na prepared in this example 0.8 The X-ray diffraction spectrum of NiO2 is shown in Figure 3 , it can be seen from the figure that all the diffraction peaks belong to the P2 type structure.
[0064] Charge and discharge performance test: The test method is the same as that in Example 1. The results show that the first discharge capacity of the positive electrode material prepared in this example at 0.1C is above 200 mAh / g.
[0065] Example 3
[0066] In this embodiment, according to the chemical formula Li 0.9 MnO2 ingredients.
[0067] A method for preparing an O2 type lithium nickel cobalt manganese positive electrode material comprises the following steps:
[0068] Step 1. Weighing:
[0069] Weigh a certain mass of MnO2 and NaNO3 according to the molar ratio, then place them in a ball mill and mix them thoroughly for 2 hours.
[0070] Step 2. High temperature calcination:
[0071] The mixture obtained in step 1 is heated to 450° C. at a heating rate of 10° C. / min, pre-calcined for 5 h, and then calcined at 800° C. for 20 h, and then naturally cooled to room temperature to obtain a sodium-containing intermediate product.
[0072] Step 3. Array microwave-assisted molten salt ion exchange:
[0073] The sodium-containing intermediate product obtained in step 2 was evenly mixed with 2 times the molar amount of LiNO3 / KCl molten salt by ball milling, and microwave heating was reacted at 200°C for 40 minutes, and then the product was filtered, washed and dried to obtain the target product. The specific reaction device diagram is shown in Figure 1 .
[0074] The Na prepared in this example 0.9 The scanning electron microscope image of MnO2 positive electrode material is shown in Figure 4 It can be seen that the obtained block particles are evenly distributed and the particle size is about 10μm.
[0075] Charge and discharge performance test: The test method is the same as that in Example 1. The results show that the first discharge capacity of the positive electrode material prepared in this example at 0.1C is above 175 mAh / g.
[0076] Example 4
[0077] In this embodiment, according to the chemical formula Li 0.7 (Ni 0.8 Co 0.1 Mn 0.1 )O2 ingredients.
[0078] A method for preparing a T2 type lithium nickel cobalt manganese positive electrode material comprises the following steps:
[0079] Step 1. Weighing:
[0080] A certain mass of Ni(NO3)2·6H2O, Co(CH3COO)2·4H2O, Mn(NO3)2·4H2O and CH3COONa was weighed according to the molar ratio, then placed in a ball mill and mixed thoroughly for 5 h.
[0081] Step 2. High temperature calcination:
[0082] The mixture obtained in step 1 is heated to 600° C. at a heating rate of 5° C. / min, pre-calcined for 3 h, and then calcined at 750° C. for 16 h, and then naturally cooled to room temperature to obtain a sodium-containing intermediate product.
[0083] Step 3. Array microwave-assisted molten salt ion exchange:
[0084] The sodium-containing intermediate product obtained in step 2 was evenly mixed with 10 times the molar amount of LiNO3 / KNO3 molten salt by ball milling, and then microwave-heated at 300°C for 5 minutes, and then the product was filtered, washed, and dried to obtain the target product. The specific reaction device diagram is shown in Figure 1 .
[0085] The Li prepared in this example 0.7 (Ni 0.8 Co 0.1 Mn 0.1 ) The X-ray diffraction spectrum of O2 positive electrode material is shown in Figure 5 , it can be seen from the figure that all the diffraction peaks belong to the T2 type structure.
[0086] Charge and discharge performance test: The test method is the same as that in Example 1. The results show that the first discharge capacity of the positive electrode material prepared in this example at 0.1C reaches 205 mAh / g.
[0087] Example 5
[0088] In this embodiment, according to the chemical formula Li 0.7 (Ni 0.8 Co 0.1 Mn 0.1 )O2 ingredients.
[0089] A method for preparing an O2 type lithium nickel cobalt manganese positive electrode material comprises the following steps:
[0090] Step 1. Weighing:
[0091] A certain mass of Ni(NO3)2·6H2O, Co(CH3COO)2·4H2O, Mn(NO3)2·4H2O and CH3COONa was weighed according to the molar ratio, then placed in a ball mill and mixed thoroughly for 5 h.
[0092] Step 2. High temperature calcination:
[0093] The mixture obtained in step 1 is heated to 600° C. at a heating rate of 5° C. / min, pre-calcined for 3 h, and then calcined at 750° C. for 16 h, and then naturally cooled to room temperature to obtain a sodium-containing intermediate product.
[0094] Step 3. Array microwave-assisted molten salt ion exchange:
[0095] The sodium-containing intermediate product obtained in step 2 was evenly mixed with 10 times the molar amount of LiNO3 / KNO3 molten salt by ball milling, and then microwave-heated at 300°C for 35 minutes, and then the product was filtered, washed, and dried to obtain the target product. The specific reaction device diagram is shown in Figure 1 .
[0096] The Li prepared in this example 0.7 (Ni 0.8 Co 0.1 Mn 0.1 ) The X-ray diffraction spectrum of O2 positive electrode material is shown in Figure 6 From the figure, we can see that all the diffraction peaks belong to the O2 type structure without any impurities, which proves that the reaction process is sufficient and uniform.
[0097] Charge and discharge performance test: The test method is the same as that in Example 1. The results show that the first discharge capacity of the positive electrode material prepared in this example at 0.1C reaches 200 mAh / g.
[0098] Example 6
[0099] In this embodiment, according to the chemical formula Li 0.7 (Ni 0.8 Co 0.1 Mn 0.1 )O2 ingredients.
[0100] A method for preparing an O3 type lithium nickel cobalt manganese positive electrode material comprises the following steps:
[0101] Step 1. Weighing:
[0102] A certain mass of Ni(NO3)2·6H2O, Co(CH3COO)2·4H2O, Mn(NO3)2·4H2O and CH3COONa was weighed according to the molar ratio, then placed in a ball mill and mixed thoroughly for 5 h.
[0103] Step 2. High temperature calcination:
[0104] The mixture obtained in step 1 is heated to 600° C. at a heating rate of 5° C. / min, pre-calcined for 3 h, and then calcined at 750° C. for 16 h, and then naturally cooled to room temperature to obtain a sodium-containing intermediate product.
[0105] Step 3. Array microwave-assisted molten salt ion exchange:
[0106] The sodium-containing intermediate product obtained in step 2 was evenly mixed with 10 times the molar amount of LiNO3 / KNO3 molten salt by ball milling, and then subjected to microwave heating at 300°C for 60 minutes. The product was then filtered, washed, and dried to obtain the target product. The specific reaction device diagram is shown in Figure 1 .
[0107] The Li prepared in this example 0.7 (Ni 0.8 Co 0.1 Mn 0.1 ) The X-ray diffraction spectrum of O2 positive electrode material is shown in Figure 7 , it can be seen from the figure that all the diffraction peaks belong to the O3 type structure.
[0108] Charge and discharge performance test: The test method is the same as that in Example 1. The results show that the first discharge capacity of the positive electrode material prepared in this example at 0.1C reaches 210 mAh / g.
[0109] Example 7
[0110] In this embodiment, according to the chemical formula Li 0.8 Ni 0.5 Co 0.2 Mn 0.3 O2 ingredients.
[0111] A method for preparing a T2 type lithium nickel cobalt manganese positive electrode material comprises the following steps:
[0112] Step 1. Weighing:
[0113] Weigh a certain amount of NiO and Co3O according to the molar ratio 4、 Mn3O4 and NaOH were then placed in a ball mill and mixed thoroughly for 0.5h.
[0114] Step 2. High temperature calcination:
[0115] The mixture obtained in step 1 is heated to 400° C. at a heating rate of 3° C. / min, pre-calcined for 2 h, and then calcined at 850° C. for 12 h, and then naturally cooled to room temperature to obtain a sodium-containing intermediate product.
[0116] Step 3. Array microwave-assisted molten salt ion exchange:
[0117] The sodium-containing intermediate product obtained in step 3 is evenly mixed with 1 molar amount of LiNO3 / NaNO3 molten salt by ball milling, and microwave heating is reacted at 280°C for 10 minutes, and then the product is filtered, washed and dried to obtain the target product. The specific reaction device diagram is shown in Figure 1 .
[0118] The Li prepared in this example 0.8 Ni 0.5 Co 0.2 Mn 0.3 The morphology of O2 cathode material is shown in Figure 8 It can be clearly seen that the particles are mainly hexagonal and the particle size is about 10μm.
[0119] Charge and discharge performance test: The test method is the same as that in Example 1. The results show that the positive electrode material prepared in this example has a first discharge specific capacity of more than 190 mAh / g at 0.1C.
[0120] Example 8
[0121] In this embodiment, according to the chemical formula Li 0.9 Ni 0.1625 Co 0.1625 Mn 0.675 O2 ingredients.
[0122] A method for preparing an O2 type lithium nickel cobalt manganese positive electrode material comprises the following steps:
[0123] Step 1. Weighing:
[0124] Weigh a certain mass of NiC2O according to the molar ratio 4、 CoC2O 4、 MnC2O4 and Na2CO3 were then placed in a ball mill and mixed thoroughly for 4h.
[0125] Step 2. High temperature calcination:
[0126] The mixture obtained in step 1 is heated to 600° C. at a heating rate of 6° C. / min, pre-calcined for 2 h, and then calcined at 750° C. for 30 h, and then naturally cooled to room temperature to obtain a sodium-containing intermediate product.
[0127] Step 3. Array microwave-assisted molten salt ion exchange:
[0128] The sodium-containing intermediate product obtained in step 2 was evenly mixed with 6 times the molar amount of LiNO3 / KCl molten salt by ball milling, and microwave heating was reacted at 230°C for 25 minutes, and then the product was filtered, washed and dried to obtain the target product. The specific reaction device diagram is shown in Figure 1 .
[0129] Charge and discharge performance test: The test method is the same as that of Example 1. The results show that the positive electrode material Li prepared in this example has a high charge and discharge performance at a voltage range of 2.0 to 4.8 V and a charge and discharge performance of 0.1 C. 1.1 Ni 0.1625 Co 0.1625 Mn 0.675The first charge and discharge capacity of O2 at 0.1C rate is 267mAh / g, the first coulombic efficiency is about 100%, and the capacity retention rate is still as high as more than 97% after 50 cycles. Fig. 9 , as shown in 10.
[0130] In summary, the advantages of the present invention are:
[0131] 1. The present invention adopts high-temperature calcination to prepare the sodium-containing intermediate product, and then uses array microwave heating to heat the molten salt for ion exchange. The preparation method has good consistency, extremely fast reaction speed, simple process, uniform and sufficient reaction.
[0132] 2. The lithium nickel cobalt manganese positive electrode material Li(Ni, Co, Mn)O2 prepared by the method of the present invention using high-temperature calcination-array microwave-assisted molten salt ion exchange method has excellent cycle performance. Under the conditions of 2.0-4.8V and 0.1C, the capacity retention rate of the material after 50 cycles is still as high as over 97%.
[0133] 3. The product yield of the process for preparing T2 / O2 / O3 configuration lithium nickel cobalt manganese positive electrode material by the method of the present invention is as high as 90%; the method is simple to operate; and is conducive to scale-up industrial production.
[0134] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A rapid preparation method for a T2 / O2 / O3 configuration lithium-ion battery cathode material, It is characterized in that include: First, a sodium-containing layered oxide Na was synthesized by high-temperature calcination. m Ni x Co y Mn 1-x-y O 2 , then mixed with 1 to 10 times the molar amount of lithium-containing composite molten salt, subjected to ion exchange treatment by array microwave heating, and then washed and dried to obtain a T2 / O2 / O3 configuration lithium-ion battery positive electrode material; Among them, 0.70≤m≤1.00, 0.00≤x≤1.00; 0.00≤y≤1.
00.
2. The rapid preparation method of the T2 / O2 / O3 configuration lithium ion battery positive electrode material according to claim 1, It is characterized in that The following steps are involved: 1) According to Na m Ni x Co y Mn 1-x-y O 2 The precursor particles and the sodium source are weighed and then mixed thoroughly to obtain a mixture; wherein 0.70≤m≤1.00, 0.00≤x≤1.00; 0.00≤y≤1.00; 2) pre-calcining the mixture obtained in step 1) at 400-600° C. for 2-5 h, then calcining at 700-900° C. for 5-30 h, and then naturally cooling to room temperature to obtain a sodium-containing intermediate product; 3) The sodium-containing intermediate product is uniformly mixed with 1 to 10 times the molar amount of lithium-containing composite molten salt, and array microwave heating is performed at 200 to 300° C. for 5 to 60 minutes, and then the product is filtered, washed, and dried to obtain a T2 / O2 / O3 configuration lithium-ion battery positive electrode material.
3. The rapid preparation method of the T2 / O2 / O3 configuration lithium ion battery positive electrode material according to claim 2, It is characterized in that In step 1), the precursor particles include a nickel source, a cobalt source and a manganese source; The nickel source is selected from Ni(NO 3 ) 2 6H 2 O.Ni(CH 3 COO 2 ·4H 2 O, NiO, Ni(OH) 2 、NiCO 3 and NiC 2 O 4 Any of; The cobalt source is selected from Co(NO 3 ) 2 6H 2 O、Co(CH 3 COO 2 ·4H 2 O、Co 3 O 4 、Co(OH) 2 、CoCO 3 and CoC 2 O 4 Any of; The manganese source is selected from Mn(NO 3 ) 2 ·4H 2 O、Mn(CH 3 COO 2 ·4H 2 O、Mn 3 O 4 、MnO 2 、Mn(OH) 2 、MnCO 3 and MnC 2 O 4 Any of .
4. The rapid preparation method of the T2 / O2 / O3 configuration lithium ion battery positive electrode material according to claim 2, It is characterized in that In step 1), the sodium salt is selected from Na 2 CO 3 , NaOH, NaNO 3 or CH 3 Any of COONa.
5. The rapid preparation method of the T2 / O2 / O3 configuration lithium ion battery positive electrode material according to claim 2, It is characterized in that In step 2), the temperature is raised from room temperature to 400-600° C. at a heating rate of 3-10° C. / min, pre-fired for 2-5 hours, and then calcined at 700-900° C. for 5-30 hours.
6. The rapid preparation method of the T2 / O2 / O3 configuration lithium ion battery positive electrode material according to claim 2, It is characterized in that In step 3), the lithium-containing composite molten salt is LiNO 3 Mixed with other molten salts, the other molten salts are selected from LiCl, KCl, NaCl, KNO 3 and NaNO 3 Any of .
7. The rapid preparation method of the T2 / O2 / O3 configuration lithium ion battery positive electrode material according to claim 2, It is characterized in that In step 3), the temperature is raised from room temperature to 200-300° C. at a heating rate of 10-30° C. / min, and the reaction time is 5-60 min.
8. A T2 / O2 / O3 configuration lithium ion battery positive electrode material prepared by the rapid preparation method according to any one of claims 1 to 7, It is characterized in that The T2 / O2 / O3 configuration lithium-ion battery positive electrode material is composed of micron-sized particles.
9. The T2 / O2 / O3 configuration lithium ion battery positive electrode material according to claim 8, It is characterized in that The capacity of the T2 / O2 / O3 lithium-ion battery cathode material is maintained at more than 97% after 50 cycles under the conditions of 2.0-4.8V and 0.1C.
10. Use of the T2 / O2 / O3 configuration lithium ion battery positive electrode material according to claim 8 or 9 in the preparation of lithium ion batteries.
Citation Information
Patent Citations
Local strengthening of glass by ion exchange
CN103391903A
Layered high-nickel ternary lithium ion battery positive electrode material, preparation method and application
CN115050935A
Method for preparing electrode material for battery
US20090114527A1
T2-type lithium cobalt oxide positive electrode material with space group of cmca and preparation method therefor
WO2023245880A1
Cited By
Surface-doped layered battery positive electrode material as well as preparation method and application thereof