Ternary material and preparation method thereof

Through low-temperature vacuum heat treatment and high-temperature pure oxygen rapid sintering methods, the problems of long sintering time and energy consumption in the ternary material preparation process are solved, and the consistency of the material and battery performance are improved.

CN118954634AInactive Publication Date: 2024-11-15HENAN KELONG NEW ENERGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411451950.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-17
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing ternary material preparation process has a long sintering time, high energy consumption, and the prepared materials are not very consistent.

Method used

The mixture of ternary material precursor and lithium salt is initially calcined by low-temperature vacuum heat treatment, and then the mixture is quickly sintered in a high-temperature pure oxygen atmosphere. It is achieved by rotating vacuum tube furnace or inclined rotary tube furnace to reduce the vacuum degree and oxygen usage .

Benefits of technology

It significantly shortens the sintering time and oxygen consumption, reduces energy consumption, improves the consistency of materials, the first charge and discharge capacity and cycle performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954634A_ABST
    Figure CN118954634A_ABST
Patent Text Reader

Abstract

The invention discloses a ternary material and a preparation method thereof. The preparation method mainly comprises the following steps: pre-treating a precursor and a lithium salt through a rotary vacuum tube furnace and other heating devices which can be vacuumized and enable the materials to move at the same time, and then carrying out subsequent treatment to obtain a ternary positive electrode material. Compared with a conventional method, through the low-temperature vacuum heat treatment technology and high-temperature short-time rapid sintering, the defects that an existing method is uneven in sintering, long in sintering time, large in oxygen consumption and the like are overcome, the ternary material which is efficient, rapid, low in cost, high in capacity and good in circulation is obtained, and the consistency of the produced material is superior to that of a traditional method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery material preparation, and specifically relates to a ternary material and a preparation method thereof. Background Art

[0002] With the development of global new energy technology, more and more portable electronic devices are emerging, the use of batteries is increasing, and lithium batteries using ternary materials are becoming more and more widely used.

[0003] At present, the mainstream ternary material preparation process is to mix the ternary precursor with the lithium salt and directly sinter it in an oxygen atmosphere. This method has a long sintering time, a large amount of oxygen, and a large energy consumption. Patent CN118026281A adopts a method of pre-oxidizing the precursor in an oxygen atmosphere and then mixing it with the lithium salt and sintering it at high temperature. Patent CN116199278B uses a precursor mixed with a lithium salt, and sintering in multiple stages in an oxygen atmosphere to reduce the high-temperature sintering time and achieve the purpose of reducing the sintering time. However, this production method still has a relatively long sintering time, a large amount of oxygen, and a relatively large energy consumption. The conventional production method has a long reaction dehydration time under normal pressure, and oxygen is required as a protective gas. The method of the present invention can greatly reduce the sintering time and reduce the oxygen consumption under low vacuum. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a ternary material, which solves the shortcomings of the existing method such as long sintering time and high energy consumption, and the prepared ternary material has high consistency.

[0005] The present invention provides a method for preparing a ternary material, comprising the following steps:

[0006] The first step is sintering: the ternary material precursor, lithium salt or a mixture of the two are preliminarily calcined by vacuum heat treatment at low temperature;

[0007] The second step is sintering: the product of the first step calcination is mixed evenly with the lithium salt or ternary material precursor and then sintered quickly in a high temperature pure oxygen atmosphere for a short time; in the first step of sintering, the mixture of the ternary material precursor and the lithium salt is vacuum heat treated: the product of the first step is directly sintered quickly in a high temperature pure oxygen atmosphere for a short time;

[0008] The third step is sintering: the product obtained in the second step is crushed, pulverized, coated and sintered to obtain the final ternary material.

[0009] Furthermore, the ternary material precursor contains Ni, Co, and Mn; the lithium salt used in the first sintering step is Li2CO3 or LiOH.

[0010] Furthermore, in the first sintering step, the molar ratio of the metal element in the ternary material precursor to the lithium in the lithium salt is 1:1.01-1.1.

[0011] Furthermore, the first step of calcination temperature is 150-450°C for 1-3 hours, and then the temperature is increased to 400-650°C for 2-4 hours.

[0012] Furthermore, the equipment for the first step of sintering low-temperature vacuum heat treatment is a rotary vacuum tube furnace or an inclined rotary tube kiln.

[0013] Furthermore, the vacuum degree of the first step of sintering low-temperature vacuum heat treatment is -0.02MPa~-0.1MPa; the state during vacuum heat treatment is moving.

[0014] Furthermore, the heating rate of the second step sintering is 3-6°C; the second step sintering temperature is 700-950°C, and the sintering time is 2-6h.

[0015] Furthermore, the second step sintering atmosphere is an oxygen atmosphere with an oxygen content of ≥80% and a furnace pressure of -5-10Pa.

[0016] Furthermore, in the third step, the coating element is one or more of B, Al, Zr, Mg, Si, P, Ti, Co, Mn, Sr, Y, Nb, Ba, and W.

[0017] The invention also provides a ternary material, which is prepared by the above method. Beneficial effects:

[0018] The innovative use of vacuum heat treatment technology in the first sintering step greatly speeds up the dehydration, mixing and homogenization of the ternary precursor and lithium salt, and does not use oxygen, which reduces energy consumption. The first sintering step shortens the sintering time and oxygen consumption of the second step, which reduces energy consumption and production costs. It also ensures that the performance of the battery positive electrode material can be fully utilized, fully taps the capacity of the positive electrode material, and can prepare a high-capacity, good cycle performance ternary positive electrode material, thereby improving the battery's first charge and discharge capacity, battery first efficiency and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The XRD pattern of the sample prepared in Example 3;

[0020] Figure 2 SEM images of samples prepared in Example 3 and Comparative Example 1;

[0021] Figure 3 The cycle diagrams were obtained from button cells assembled from samples prepared in Example 3 and Comparative Examples 1 and 2. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments.

[0023] In order to better evaluate the superiority of the material prepared by the present invention compared with the material prepared by the conventional method, the material capacity and cycle were evaluated by preparing CR2016 battery buckle test. The battery preparation and evaluation method is as follows:

[0024] The positive electrode materials prepared in the examples and comparative examples were mixed with Super-P, RS-6, and PVDF in a mass ratio of 92%:3%:2%:3% and a certain amount of NMP using a high-speed mixer, and the mixed slurry was coated on aluminum foil using a coater. The electrode was dried at 120°C for 6 hours and rolled using a roller press until the electrode was compacted to 3.2-3.3 g / cm 3 , cut into a 14mm diameter positive electrode sheet using a cutter; use metal lithium for the negative electrode, cut into a 16mm diameter negative electrode sheet, use LiPF6 / EC / EMC electrolyte (LiPF6 is lithium salt, EC is ethylene carbonate, EMC is methyl ethyl carbonate, LiPF6 is 1mol / L, EC / EMC volume ratio = 1:1) and PE separator, assemble in a nitrogen-filled glove box in the order of negative electrode shell / gasket / liquid sheet / 0.02g electrolyte / diaphragm / 0.01g electrolyte / positive electrode sheet / positive electrode shell to obtain a CR2016 button cell. After the above battery is left overnight, the capacity and charge-discharge cycle performance are tested on a blue electric tester.

[0025] Capacity test: Test conditions: At room temperature of 25°C, current 0.1C charge and discharge test (1C=190mAh / g), voltage range of 3.0-4.3V, measured charge and discharge specific capacity and first efficiency.

[0026] Cycle performance test: Test conditions: at room temperature of 25°C, 0.5C charge and 1C discharge (1C=190mAh / g), voltage range of 3.0-4.3V, and cycle number of 200 cycles. Example 1

[0027] Ni 0.83 Co 0.12 Mn 0.05 The (OH)2 precursor is added to a rotary vacuum tube furnace, heated to 400°C, kept warm for 1 hour, and then heated to 650°C and kept warm for 3 hours. During the entire heating process, the vacuum degree of the vacuum heating equipment is maintained at -0.09-(-0.1MPa), the material is kept in motion throughout the process, and then the material is discharged. The sintered material is mixed evenly with LiOH in proportion, the mixed material is placed in a sagger, and the temperature is quickly raised to 800°C at a heating rate of 4°C / min and sintered for 5 hours. The sintering atmosphere is oxygen, and the oxygen concentration is greater than or equal to 85%. The second sintered product is crushed and pulverized, the crushed material is mixed evenly with a certain amount of Al2O3, and sintered at 500°C for 5 hours to obtain the final product. Example 2

[0028] Li2CO3 and LiOH are added into a rotary vacuum tube furnace in proportion (the molar ratio of Li in Li2CO3 and LiOH is 1:2), heated to 300℃, and kept warm for 1.5h. During the whole heating process, the vacuum degree of the vacuum heating equipment is kept at -0.05-(-0.07MPa), and the materials are kept in motion throughout the whole process, and then the materials are discharged. 0.83 Co 0.12 Mn 0.05 The (OH)2 precursors are mixed evenly in proportion, and the mixed materials are placed in a sagger, and the temperature is rapidly increased to 800°C at a heating rate of 5°C / min and sintered for 5 hours. The sintering atmosphere is oxygen, and the oxygen concentration is greater than or equal to 90%. The second sintered product is crushed and pulverized, and the pulverized material is evenly mixed with a certain amount of Li2WO4, and sintered at 450°C for 4 hours to obtain the final product. Example 3

[0029] Ni 0.83 Co 0.12 Mn 0.05 After the (OH)2 precursor and LiOH are mixed evenly in proportion (molar ratio (Ni+Co+Mn):Li=1:1.03), the mixed materials are added to the rotary vacuum tube furnace equipment, heated to 250℃, kept warm for 1h, and then heated to 600℃ and kept warm for 4h. During the whole heating process, the vacuum degree of the vacuum heating equipment is kept at -0.02-(-0.04MPa), the material is kept in motion throughout the whole process, and then the material is discharged. The sintered material is placed in a sagger, and the temperature is quickly raised to 800℃ at a heating rate of 3℃ / min and sintered for 4h. The sintering atmosphere is oxygen, and the oxygen concentration is greater than or equal to 95%. The second sintered product is crushed and pulverized, and the pulverized material is mixed evenly with a certain amount of H3BO3, and sintered at 350℃ for 6h to obtain the final product. Comparative Example 1

[0030] Ni 0.83 Co 0.12 Mn 0.05 After the (OH)2 precursor and LiOH are mixed evenly in proportion (molar ratio (Ni+Co+Mn):Li=1:1.03), the mixed materials are placed in a sagger and heated to 800℃ at a heating rate of 2.5℃, kept warm for 12h, with oxygen flowing throughout the process, with an oxygen concentration of more than 95%, then cooled, crushed and pulverized. The pulverized material is mixed evenly with a certain amount of H3BO3 and sintered at 350℃ for 6h to obtain the final product. Comparative Example 2

[0031] Ni 0.83Co 0.12 Mn 0.05 After the (OH)2 precursor and LiOH are mixed evenly in proportion (molar ratio (Ni+Co+Mn):Li=1:1.03), the mixed materials are placed in a sagger, heated to 200℃ at a rate of 2.5℃, and kept warm for 2h; then heated to 600℃ at a rate of 3℃, kept warm for 3h, then heated to 800℃ at the same rate and kept warm for 3h, cooled to 750℃ and kept warm for 6h, and finally cooled to room temperature. Then cool down, crush and grind. The crushed material is mixed evenly with a certain amount of H3BO3, and sintered at 350℃ for 6h to obtain the final product.

[0032] Table 1 shows the capacity data of button cells assembled from samples prepared in the examples and comparative examples measured on a blue-power system. Example 3 and comparative examples 1 and 2 show that the capacity of the samples prepared by the method of the present invention is not lower than that of materials prepared by the mainstream methods currently on the market. Table 1 Capacity data of button-type batteries assembled from samples prepared in the embodiments and comparative examples measured on the blue power system

[0033] Figure 1 The XRD pattern of the sample prepared in Example 3 is as follows: Figure 1 It can be seen that the ternary material prepared using the present invention has high crystallinity. Figure 2 The SEM images of samples prepared for Example 3 and Comparative Example 1 are shown below. Figure 2 It can be seen that the primary particle uniformity of the ternary material prepared in Example 3 is better than that of the ternary material prepared in Comparative Example 1. Figure 3 The cycle diagrams are obtained from button cells assembled from samples prepared in Example 3 and Comparative Examples 1 and 2. Figure 3 It can be seen that the cycle of Example 3 is better than that of the comparative example.

Claims

1. A method for preparing a ternary material, characterized in that: The following steps are involved: The first step is sintering: the ternary material precursor, lithium salt or a mixture of the two are preliminarily calcined by vacuum heat treatment at low temperature; The second step is sintering: the product of the first step calcination is mixed evenly with the lithium salt or ternary material precursor and then sintered quickly in a high temperature pure oxygen atmosphere for a short time; in the first step of sintering, the mixture of the ternary material precursor and the lithium salt is vacuum heat treated: the product of the first step is directly sintered quickly in a high temperature pure oxygen atmosphere for a short time; The third step is sintering: the product obtained in the second step is crushed, pulverized, coated and sintered to obtain the final ternary material.

2. The method for preparing the ternary material according to claim 1, characterized in that: The ternary material precursor contains Ni, Co and Mn; the lithium salt used in the first sintering step is Li2CO3 or LiOH.

3. The method for preparing the ternary material according to claim 2, characterized in that: In the first step of sintering, the molar ratio of the metal element in the ternary material precursor to the lithium in the lithium salt is 1:1.01-1.

1.

4. The method for preparing the ternary material according to claim 3, characterized in that: The first step of calcination is at a temperature of 150-450°C for 1-3 hours, and then the temperature is raised to 400-650°C for 2-4 hours.

5. The method for preparing the ternary material according to claim 4, characterized in that: The equipment for the first step of sintering low-temperature vacuum heat treatment is a rotary vacuum tube furnace or a tilting rotary tube kiln.

6. The method for preparing the ternary material according to claim 5, characterized in that: The vacuum degree of the first step of sintering low-temperature vacuum heat treatment is -0.02MPa~-0.1MPa; the state during vacuum heat treatment is moving.

7. The method for preparing the ternary material according to claim 6, characterized in that: The heating rate of the second step sintering is 3-6°C; the sintering temperature of the second step is 700-950°C, and the sintering time is 2-6h.

8. The method for preparing the ternary material according to claim 7, characterized in that: The second step sintering atmosphere is oxygen atmosphere, the oxygen content is ≥80%, and the furnace pressure is -5-10Pa.

9. The method for preparing the ternary material according to claim 8, characterized in that: In the third step, the coating element is one or more of B, Al, Zr, Mg, Si, P, Ti, Co, Mn, Sr, Y, Nb, Ba, and W.

10. A ternary material, characterized in that: The method is prepared by any one of claims 1 to 9.

Citation Information

Patent Citations

  • High-nickel single-crystal ternary cathode material with low surface residual alkali content and preparation method thereof

    CN110436531A

  • Single-crystal lithium nickel cobalt manganese oxide ternary positive electrode material and low-temperature sintering preparation method thereof

    CN111129448A

  • Low-cost low-cobalt single crystal ternary positive electrode material and preparation method thereof

    CN112342605A

  • Preparation method of ternary positive electrode material, ternary positive electrode material and application

    CN114349077A

  • High-voltage ternary positive electrode material and preparation method thereof

    CN115911300A