Glass fiber and preparation method thereof

By adopting the SiO2-Al2O3-MgO-CaO quadruple system glass fiber formula and adding Li2O and TiO2, the existing glass fiber mechanical properties and corrosion resistance are solved, and high-strength, high-modulus and environmentally friendly glass fibers are achieved. Preparation, suitable for new energy and environmental protection fields.

CN118954958APending Publication Date: 2024-11-15NEIJIANG HUAYUAN ELECTRONICS MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411071004.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing high-strength and high-modulus glass fibers have insufficient mechanical properties, high temperature resistance and corrosion resistance, resulting in poor performance in some applications.

Method used

The SiO2-Al2O3-MgO-CaO quadruple system glass fiber formula is used, and Li2O and TiO2 are added to optimize the formula to improve the modulus, strength and chemical corrosion resistance of the glass, and reduce production costs and environmental pollution through specific preparation methods.

Benefits of technology

It significantly improves the mechanical properties and chemical corrosion resistance of glass fibers, reduces production costs and environmental pollution, and is suitable for applications in new energy and environmental protection fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980869700000111
    Figure BDA0004980869700000111
  • Figure BDA0004980869700000121
    Figure BDA0004980869700000121
Patent Text Reader

Abstract

The invention discloses a glass fiber and a preparation method thereof, and belongs to the technical field of non-metallic materials. The high-strength and high-modulus glass fiber is prepared from the following components in percentage by weight: 57 to 62 percent of SiO2 (silicon dioxide), 17.8 to 21 percent of Al2O3 (aluminum oxide), 5.3 to 11 percent of CaO (calcium oxide), 8.9 to 10.4 percent of MgO (magnesium oxide), 0.46 to 1 percent of TiO2 (titanium dioxide), 0.35 to 0.73 percent of Na2O (sodium oxide) and K2O (potassium oxide), 0.44 to 0.58 percent of Fe2O3 (iron oxide) and 0.4 to 0.61 percent of Li2O (lithium oxide). The glass fiber provided by the invention has excellent mechanical properties, high temperature resistance and corrosion resistance, meanwhile, the spodumene industrial tailing raw material is introduced into the production raw materials to replace part of kaolin, the cost is saved, and the preparation method is simple and convenient, is suitable for large tank furnaces, and has excellent industrial prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of non-metallic materials, and particularly relates to glass fiber and a preparation method thereof. Background Art

[0002] In the context of the rapid development of science and technology and industry, high-strength and high-modulus glass fiber, as an excellent composite material reinforcement, has become increasingly widely used around the world. With its excellent mechanical properties and corrosion resistance, this material plays a pivotal role in many key fields such as aerospace, automobile manufacturing, wind power generation, and building construction. As the global economy gradually recovers from past fluctuations and science and technology continue to advance, the market demand for high-strength and high-modulus glass fiber has shown a steady upward trend.

[0003] It is particularly noteworthy that the application prospects of this material are highly anticipated in emerging industries such as new energy and environmental protection. The rapid development of new energy fields, such as wind energy and solar energy, has provided a huge market space for high-strength and high-modulus glass fibers. In the field of environmental protection, due to its light weight, high strength, and corrosion resistance, this material has also shown great potential in replacing traditional materials and reducing environmental pollution.

[0004] In-depth market analysis and competition research on the high-strength and high-modulus glass fiber industry is undoubtedly the key for enterprises to gain competitive advantages and achieve sustainable development. Through such research, enterprises can not only better grasp the pulse of the market and identify development opportunities, but also timely discover potential threats and challenges, thereby formulating more accurate marketing strategies and product development directions.

[0005] Research on the high-strength and high-modulus glass fiber industry will also help promote the healthy and orderly development of the entire industry. By gaining a deeper understanding of the competition landscape and market demand within the industry, the government and relevant agencies can formulate more targeted industrial policies and regulatory measures to provide stronger support for the innovation and development of enterprises. Enterprises can also jointly promote the progress and prosperity of the entire industry by strengthening cooperation and sharing resources. Summary of the invention

[0006] In view of the above-mentioned prior art, the present invention provides a glass fiber and a preparation method thereof, which solves the problem that the mechanical properties, high temperature resistance and corrosion resistance of the glass fiber in the prior art are insufficient.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a glass fiber, comprising the following components: SiO 2 57~62wt%Al 2 O 317.8~21wt%, CaO 5.3~11wt%, MgO8.9~10.4wt%, TiO 2 0.46~1wt%Na 2 O+K 2 O 0.35~0.73wt%Fe 2 O 3 0.44~0.58wt%Li 2 O 0.4~0.61wt%.

[0008] The beneficial effects of the present invention are: the present invention is based on the original SiO 2 -Al 2 O 3 -MgO ternary system glass, a certain amount of CaO is introduced to form SiO 2 -Al 2 O 3 -MgO-CaO quaternary system glass is to reduce the melting temperature of glass and the molding temperature of fiber. 2 -Al 2 O 3 -MgO-CaO system glass is added with some other metal oxides (such as Li 2 O、TiO 2 ) in order to improve the processability of glass melting and glass fiber forming, and improve the modulus, strength and chemical corrosion resistance of glass; the composition provided by the present invention does not contain fluoride and boride, which reduces the pollution to the environment. The SiO 2 The content range is 57-62wt%. If SiO 2 When the content exceeds 62wt%, the glass viscosity increases, the glass melting and fiber forming temperature rises significantly, and SiO 2 When the content is lower than 56wt%, the strength and modulus of the glass fiber will decrease, and the crystallization tendency of the glass will increase; the S, T and R glass SiO 2 +Al 2 O 3 The composition of the present invention has a SiO 2 +Al 2 O 3 The content of MgO is between 72 and 80 wt%, and the difficulty of production is greatly reduced; although MgO and CaO are both extra-network components in the glass structure, if the MgO content is too high, the crystallization tendency of the glass will increase significantly, and if the CaO content is too high, the strength and modulus of the glass fiber will be reduced. The MgO content of the optimized formula of the present invention is between 8.9 and 10.4 wt%, and the CaO content is between 5.3 and 11 wt%; TiO 2 Since the single bond strength of Ti-O is the highest among the component ions outside the glass network, TiO2 It can improve the modulus of glass fiber, and TiO 2 It is also very effective in improving the chemical corrosion resistance (especially acid resistance) of glass, but as the added amount increases, the glass gradually becomes light brown and the crystallization tendency increases. The TiO2 content of the optimized formula of the present invention is 0.46-1wt%.

[0009] Based on the above technical solution, the present invention can also be improved as follows.

[0010] Further, the following components are included: SiO 2 58~60wt%Al 2 O 3 19.2~21wt%, CaO6.4~8.1wt%, MgO 9.1~9.7wt%, TiO 2 0.46~1wt%Na 2 O+K 2 O 0.41~0.5wt%Fe 2 O 3 0.44~0.58wt%Li 2 O 0.4~0.61wt%.

[0011] The beneficial effect of adopting the further technical solution is: further optimizing the formula of the composition, and removing the B in the E glass from the glass fiber provided by the present invention. 2 O 3 The composition not only improves the mechanical properties of the glass itself, but also effectively reduces the emission of harmful pollutants, making the production more environmentally friendly. Compared with S glass and traditional R glass, the glass fiber of the present invention has a much higher elastic modulus and a much lower liquidus temperature, which is conducive to reducing the risk of glass crystallization and improving the fiber drawing efficiency; it has a higher crystallization peak temperature, indicating that the formation and growth of the crystal nucleus of the glass during the crystallization process requires more energy, that is, under the same conditions, the crystallization rate of the glass of the present invention is smaller.

[0012] Further, the total content of Y is not more than 5.2wt%. 2 O 3 ,La 2 O 3 , SrO and CeO 2 One or more of .

[0013] The beneficial effect of adopting further technical solutions is: CeO 2 It is a strong oxidant that can help clarify and melt glass and improve glass quality. SrO and Y 2 O 3It can reduce the molding temperature and difficulty of the product, improve the temperature resistance, chemical stability, thermal stability and optical properties of the product, especially the improvement of strength and modulus; La 2 O 3 It can improve physical properties and thermal stability, and optimize the optical properties and production adaptability of glass.

[0014] Furthermore, SiO 2 and Al 2 O 3 The mass ratio is 3 to 3.4:1.

[0015] Furthermore, the mass ratio of CaO to MgO is 0.6 to 1.2:1.

[0016] The present invention also discloses a method for preparing glass fiber, comprising the following steps:

[0017] S1: Mix the mineral raw materials uniformly according to the mass percentage of the glass fiber components to obtain a mixture;

[0018] S2: clarifying and homogenizing the mixture at 1550-1650°C to obtain glass liquid;

[0019] S3: Cooling the glass liquid to 1300-1370°C, flowing out through a platinum bushing, and drawing a crude product;

[0020] S4: coating the crude product with a sizing agent, and then drawing the resulting glass fiber;

[0021] The mineral raw materials are quartz sand, pyrophyllite, limestone, dolomite, spodumene and kaolin; the particle size of the quartz sand is 50-200 μm, the particle size of the pyrophyllite is 40-50 μm, the particle size of the limestone is 150-200 μm, the particle size of the dolomite is 150-200 μm, the particle size of the spodumene is 50-100 μm, and the particle size of the kaolin is 40-50 μm.

[0022] Furthermore, the mass ratio of spodumene to kaolin is 2 to 6:3.

[0023] Furthermore, the wetting agent is paraffin emulsion.

[0024] The beneficial effects of the present invention are as follows: in order to reduce the production cost, the Al 2 O 3 The introduction of spodumene industrial tailings raw materials, including Li 2 The O content is about 0.5%, Al 2 O 3 The content is about 23%. The primary value of spodumene is to replace kaolin to introduce Al 2 O 3, and the proportion of kaolin replacement shall not be less than 40%, which can greatly reduce the cost of glass; secondly, the main purpose of roasting spodumene is to effectively adjust the COD and gas rate of the mixture; thirdly, the crystal structure of roasted spodumene belongs to the monoclinic system, with a symmetry of 2 / m, and its crystal structure is similar to that of diopside, but the difference is that Li at the M2 position is coordinated six times. Compared with kaolin, spodumene has a lower melting point, only about 1350°C, which is very beneficial to reducing the energy consumption of batch melting and saving glass production costs; and the present invention ensures the melting quality of the glass liquid of the glass system through reasonable raw material selection and particle size control, while reducing the melting temperature and energy consumption of the kiln, and reducing the erosion of the refractory materials in the kiln by the glass liquid at high temperature. At the same time, the present invention adopts raw materials with different particle size gradings, on the one hand, to ensure the uniformity of raw material mixing; on the other hand, to reduce the introduction of ultrafine powder, which is conducive to the discharge of bubbles in the glass liquid. The preparation method of the present invention is suitable for large-scale pool kilns, which is conducive to improving production efficiency. DETAILED DESCRIPTION

[0025] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.

[0026] In the embodiments of the present invention, for ease of operation, the total content of the glass fiber component is taken as 100%, wherein the total content of the components in the embodiments is slightly less than 100%, and it can be understood that the residual amount is a trace amount of impurities.

[0027] Example 1

[0028] A glass fiber composition is: SiO2 58.2wt%, Al 2 O 3 19.2wt%, CaO 8.1wt%, MgO9.4wt%, TiO 2 0.75wt%Na 2 O+K 2 O 0.45wt%,Fe 2 O 3 0.44wt%Li 2 O 0.4wt%, SrO 0.7wt%, La 2 O 3 2.0wt%, the remainder is impurities;

[0029] According to the components of the glass fiber, ore raw materials are taken, the ore raw materials include quartz sand with a particle size of 100 μm, pyrophyllite with a particle size of 45 μm, limestone with a particle size of 160 μm, dolomite with a particle size of 160 μm, spodumene with a particle size of 75 μm and kaolin with a particle size of 45 μm, wherein the mass ratio of spodumene to kaolin is 1:1; the ore raw materials are subjected to the following steps:

[0030] S1: The mineral raw materials are transported to the mixing tank for mixing, and after being evenly mixed, they are transported to the kiln head silo to obtain a mixed material;

[0031] S2: The mixed material is put into a tank kiln, clarified and homogenized at 1600°C to obtain glass liquid;

[0032] S3: placing the glass liquid in a wire drawing operation channel and cooling it to 1320°C, flowing out through a platinum bushing, and drawing a crude product;

[0033] S4: The crude product is coated with paraffin emulsion and then drawn to obtain high-strength and high-modulus glass fiber.

[0034] Example 2

[0035] A glass fiber component is: SiO 2 58.2wt%Al 2 O 3 19.2wt%, CaO 7.8wt%, MgO9.7wt%, TiO 2 0.49wt%Na 2 O+K 2 O 0.41wt%,Fe 2 O 3 0.44wt%Li 2 O 0.5wt%, SrO 0.7wt%, Y 2 O 3 2.0wt%CeO 2 0.2wt%, the remainder is impurities;

[0036] According to the components of the above glass fiber, ore raw materials are taken, the ore raw materials include quartz sand with a particle size of 50 μm, pyrophyllite with a particle size of 40 μm, limestone with a particle size of 150 μm, dolomite with a particle size of 150 μm, spodumene with a particle size of 50 μm and kaolin with a particle size of 40 μm, wherein the mass ratio of spodumene to kaolin is 2:3; the ore raw materials are subjected to the following steps:

[0037] S1: The mineral raw materials are transported to the mixing tank for mixing, and after being evenly mixed, they are transported to the kiln head silo to obtain a mixed material;

[0038] S2: The mixed material is put into a tank kiln, clarified and homogenized at 1550°C to obtain glass liquid;

[0039] S3: placing the glass liquid in a wire drawing operation channel and cooling it to 1300°C, flowing out through a platinum bushing, and drawing a crude product;

[0040] S4: The crude product is coated with paraffin emulsion and then drawn to obtain high-strength and high-modulus glass fiber.

[0041] Example 3

[0042] A glass fiber formula is: SiO 2 58wt%Al 2 O 3 21wt%, CaO 5.3wt%, MgO9.1wt%, TiO 2 0.46wt%Na 2 O+K 2 O 0.44wt%,Fe 2 O 3 0.44wt%Li 2 O 0.5wt%, SrO 0.7wt%, Y 2 O 3 3.5wt%, the remainder is impurities;

[0043] According to the components of the above glass fiber, ore raw materials are taken, the ore raw materials include quartz sand with a particle size of 50 μm, pyrophyllite with a particle size of 40 μm, limestone with a particle size of 150 μm, dolomite with a particle size of 150 μm, spodumene with a particle size of 50 μm and kaolin with a particle size of 40 μm, wherein the mass ratio of spodumene to kaolin is 2:1; the ore raw materials are subjected to the following steps:

[0044] S1: The mineral raw materials are transported to the mixing tank for mixing, and after being evenly mixed, they are transported to the kiln head silo to obtain a mixed material;

[0045] S2: The mixed material is put into a tank kiln, clarified and homogenized at 1650°C to obtain glass liquid;

[0046] S3: placing the glass liquid in a wire drawing operation channel and cooling it to 1370°C, flowing out through a platinum bushing, and drawing a crude product;

[0047] S4: The crude product is coated with paraffin emulsion and then drawn to obtain high-strength and high-modulus glass fiber.

[0048] Example 4

[0049] A glass fiber formula is: SiO 2 57wt%Al 2 O 3 21wt%, CaO 5.3wt%, MgO10.4wt%, TiO 2 0.74wt%Na 2 O+K 2 O 0.35wt%,Fe 2 O 3 0.44wt%Li 2 O 0.61wt%, La 2O 3 0.5wt%, Y 2 O 3 3.5wt%, the remainder is impurities;

[0050] According to the components of the glass fiber, ore raw materials are taken, the ore raw materials include quartz sand with a particle size of 100 μm, pyrophyllite with a particle size of 45 μm, limestone with a particle size of 160 μm, dolomite with a particle size of 160 μm, spodumene with a particle size of 75 μm and kaolin with a particle size of 45 μm, wherein the mass ratio of spodumene to kaolin is 1:1; the ore raw materials are subjected to the following steps:

[0051] S1: The mineral raw materials are transported to the mixing tank for mixing, and after being evenly mixed, they are transported to the kiln head silo to obtain a mixed material;

[0052] S2: The mixed material is put into a tank kiln, clarified and homogenized at 1600°C to obtain glass liquid;

[0053] S3: placing the glass liquid in a wire drawing operation channel and cooling it to 1320°C, flowing out through a platinum bushing, and drawing a crude product;

[0054] S4: The crude product is coated with paraffin emulsion and then drawn to obtain high-strength and high-modulus glass fiber.

[0055] Example 5

[0056] A glass fiber formula is: SiO 2 58.1wt%Al 2 O 3 19.2wt%, CaO 6.7wt%, MgO9.3wt%, TiO 2 0.41wt%Na 2 O+K 2 O 0.44wt%,Fe 2 O 3 0.44wt%Li 2 O 0.51wt%, La 2 O 3 2.0wt%, Y 2 O 3 1.6wt%, SrO 1.1wt%, the remainder is impurities;

[0057] According to the components of the glass fiber, ore raw materials are taken, the ore raw materials include quartz sand with a particle size of 100 μm, pyrophyllite with a particle size of 45 μm, limestone with a particle size of 160 μm, dolomite with a particle size of 160 μm, spodumene with a particle size of 75 μm and kaolin with a particle size of 45 μm, wherein the mass ratio of spodumene to kaolin is 1:1; the ore raw materials are subjected to the following steps:

[0058] S1: The mineral raw materials are transported to the mixing tank for mixing, and after being evenly mixed, they are transported to the kiln head silo to obtain a mixed material;

[0059] S2: The mixed material is put into a tank kiln, clarified and homogenized at 1600°C to obtain glass liquid;

[0060] S3: placing the glass liquid in a wire drawing operation channel and cooling it to 1320°C, flowing out through a platinum bushing, and drawing a crude product;

[0061] S4: The crude product is coated with paraffin emulsion and then drawn to obtain high-strength and high-modulus glass fiber.

[0062] Example 6

[0063] A glass fiber formula is: SiO 2 58.1wt%Al 2 O 3 19.2wt%, CaO 7.3wt%, MgO9.3wt%, TiO 2 0.95wt%Na 2 O+K 2 O 0.39wt%,Fe 2 O 3 0.44wt%Li 2 O 0.51wt%, La 2 O 3 1.6wt%, Y 2 O 3 2.0wt%, the remainder is impurities;

[0064] According to the components of the glass fiber, ore raw materials are taken, the ore raw materials include quartz sand with a particle size of 100 μm, pyrophyllite with a particle size of 45 μm, limestone with a particle size of 160 μm, dolomite with a particle size of 160 μm, spodumene with a particle size of 75 μm and kaolin with a particle size of 45 μm, wherein the mass ratio of spodumene to kaolin is 1:1; the ore raw materials are subjected to the following steps:

[0065] S1: The mineral raw materials are transported to the mixing tank for mixing, and after being evenly mixed, they are transported to the kiln head silo to obtain a mixed material;

[0066] S2: The mixed material is put into a tank kiln, clarified and homogenized at 1600°C to obtain glass liquid;

[0067] S3: placing the glass liquid in a wire drawing operation channel and cooling it to 1320°C, flowing out through a platinum bushing, and drawing a crude product;

[0068] S4: The crude product is coated with paraffin emulsion and then drawn to obtain high-strength and high-modulus glass fiber.

[0069] Example 7

[0070] A glass fiber formula is: SiO 2 59.7wt%Al 2 O 3 17.8wt%, CaO 10.9wt%, MgO8.9wt%, TiO 2 0.82wt%Na 2 O+K 2 O 0.73wt%,Fe 2 O 3 0.58wt%Li 2 O 0.48wt%, the remainder is impurities;

[0071] According to the components of the glass fiber, ore raw materials are taken, the ore raw materials include quartz sand with a particle size of 100 μm, pyrophyllite with a particle size of 45 μm, limestone with a particle size of 160 μm, dolomite with a particle size of 160 μm, spodumene with a particle size of 75 μm and kaolin with a particle size of 45 μm, wherein the mass ratio of spodumene to kaolin is 1:1; the ore raw materials are subjected to the following steps:

[0072] S1: The mineral raw materials are transported to the mixing tank for mixing, and after being evenly mixed, they are transported to the kiln head silo to obtain a mixed material;

[0073] S2: The mixed material is put into a tank kiln, clarified and homogenized at 1600°C to obtain glass liquid;

[0074] S3: placing the glass liquid in a wire drawing operation channel and cooling it to 1300°C, flowing out through a platinum bushing, and drawing a crude product;

[0075] S4: The crude product is coated with paraffin emulsion and then drawn to obtain high-strength and high-modulus glass fiber.

[0076] Comparative Example 1

[0077] The components of S glass fiber are: SiO 2 65wt%Al 2 O 3 25wt%, MgO 10wt%.

[0078] According to the components of the above-mentioned S glass fiber, ore raw materials are taken, and the ore raw materials include quartz sand with a particle size of 100 μm, pyrophyllite with a particle size of 45 μm, limestone with a particle size of 160 μm, dolomite with a particle size of 160 μm and kaolin with a particle size of 45 μm; the ore raw materials are subjected to the following steps:

[0079] S1: The mineral raw materials are transported to the mixing tank for mixing, and after being evenly mixed, they are transported to the kiln head silo to obtain a mixed material;

[0080] S2: The mixed material is put into a tank kiln, clarified and homogenized at 1650°C to obtain glass liquid;

[0081] S3: placing the glass liquid in a wire drawing operation channel and cooling it to 1300°C, flowing out through a platinum bushing, and drawing a crude product;

[0082] S4: The crude product is coated with paraffin emulsion and then drawn to obtain S glass fiber.

[0083] Comparative Example 2

[0084] The components of traditional R glass fiber are: SiO 2 60wt%Al 2 O 3 25wt%, CaO 9wt%, MgO6wt%.

[0085] According to the components of the above-mentioned conventional R glass fiber, ore raw materials are taken, the ore raw materials include quartz sand with a particle size of 100 μm, pyrophyllite with a particle size of 45 μm, limestone with a particle size of 160 μm, dolomite with a particle size of 160 μm and kaolin with a particle size of 45 μm; the ore raw materials are subjected to the following steps:

[0086] S1: The mineral raw materials are transported to the mixing tank for mixing, and after being evenly mixed, they are transported to the kiln head silo to obtain a mixed material;

[0087] S2: The mixed material is put into a tank kiln, clarified and homogenized at 1650°C to obtain glass liquid;

[0088] S3: placing the glass liquid in a wire drawing operation channel and cooling it to 1450°C, flowing out through a platinum bushing, and drawing a crude product;

[0089] S4: The crude product is coated with paraffin emulsion and then drawn to obtain conventional R glass fiber.

[0090] Comparative Example 3

[0091] The components of E glass fiber are: SiO 2 54wt%Al 2 O 3 14wt%, CaO 22.5wt%, MgO 2wt%, Na 2 O+K 2 O 0.85wt%,Fe 2 O 3 0.35wt%TiO 2 0.45wt%,F 20.5wt%B 2 O 3 5.5wt%.

[0092] According to the components of the above-mentioned E glass fiber, ore raw materials are taken, and the ore raw materials include quartz sand with a particle size of 100 μm, pyrophyllite with a particle size of 45 μm, limestone with a particle size of 160 μm, dolomite with a particle size of 160 μm and kaolin with a particle size of 45 μm; the ore raw materials are subjected to the following steps:

[0093] S1: The mineral raw materials are transported to the mixing tank for mixing, and after being evenly mixed, they are transported to the kiln head silo to obtain a mixed material;

[0094] S2: The mixed material is put into a tank kiln, clarified and homogenized at 1600°C to obtain glass liquid;

[0095] S3: placing the glass liquid in a wire drawing operation channel to cool to 1200°C, flowing out through a platinum bushing, and drawing a crude product;

[0096] S4: The crude product is coated with paraffin emulsion and then drawn to obtain E glass fiber.

[0097] Table 1 lists 7 embodiments of the present invention and 3 comparative examples, and statistically analyzes their performance data.

[0098] Table 1 Performance data statistics

[0099]

[0100]

[0101] From the specific values ​​in the above table, it can be seen that compared with S glass fiber and traditional R glass fiber, the glass fiber of the present invention has a higher elastic modulus; a lower liquidus temperature, which is conducive to reducing the risk of glass crystallization and improving the fiber drawing efficiency; and a higher crystallization peak temperature, which indicates that the formation and growth of the crystal nucleus of the glass during the crystallization process requires more energy, that is, under the same conditions, the crystallization rate of the glass of the present invention is smaller; the glass fiber of the present invention not only has a sufficiently low liquidus temperature and a smaller crystallization rate, and can be produced in a pool kiln, but also achieves a significant increase in the glass modulus. Compared with E glass fiber, the glass fiber of the present invention does not use F 2 and B 2 O 3, effectively reducing the emission of harmful pollutants, making production more environmentally friendly, and having a higher elastic modulus. The production process of the glass fiber of the present invention is similar to the production process of E glass. Although the molding temperature is about 80°C higher than that of E glass fiber, due to the successful application of a large number of new equipment and new processes, such as full oxygen combustion, electric melting, platinum leak plate dispersion strengthening technology, etc., modern pool kilns can fully meet the large-scale production of high-strength and high-modulus glass fibers.

[0102] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A glass fiber, characterized in that: The invention comprises the following components: SiO2 57-62wt%, Al2O3 17.8-21wt%, CaO 5.3-11wt%, MgO 8.9-10.4wt%, TiO2 0.46-1wt%, Na2O+K2O 0.35-0.73wt%, Fe2O3 0.44-0.58wt%, and Li2O 0.4-0.61wt%.

2. The glass fiber according to claim 1 is characterized in that The invention comprises the following components: SiO2 58-60wt%, Al2O3 19.2-21wt%, CaO 6.4-8.1wt%, MgO 9.1-9.7wt%, TiO2 0.46-1wt%, Na2O+K2O 0.41-0.5wt%, Fe2O3 0.44-0.58wt%, and Li2O 0.4-0.61wt%.

3. The glass fiber according to claim 1, characterized in that: It also includes one or more of Y2O3, La2O3, SrO and CeO2 with a total content not exceeding 5.2wt%.

4. The glass fiber according to claim 1, characterized in that: The mass ratio of SiO2 to Al2O3 is 3 to 3.4:

1.

5. The glass fiber according to claim 1, characterized in that: The mass ratio of CaO to MgO is 0.6-1.2:

1.

6. The method for preparing glass fiber according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: Take the corresponding mineral raw materials according to the mass percentage of the glass fiber component and mix them evenly to obtain a mixture; S2: clarifying and homogenizing the mixture at 1550-1650°C to obtain glass liquid; S3: Cooling the glass liquid to 1300-1370°C, flowing out through a platinum bushing, and drawing a crude product; S4: coating the crude product with a sizing agent, and then drawing the resulting glass fiber; The mineral raw materials are quartz sand, pyrophyllite, limestone, dolomite, spodumene and kaolin; the particle size of the quartz sand is 50-200 μm, the particle size of the pyrophyllite is 40-50 μm, the particle size of the limestone is 150-200 μm, the particle size of the dolomite is 150-200 μm, the particle size of the spodumene is 50-100 μm, and the particle size of the kaolin is 40-50 μm.

7. The method for preparing glass fiber according to claim 6, characterized in that: The mass ratio of spodumene to kaolin is 2 to 6:

3.

8. The method for preparing glass fiber according to claim 6, characterized in that: The infiltrant is paraffin emulsion.

Citation Information

Patent Citations

  • High-modulus glass fiber composition as well as glass fiber and composite material thereof

    CN105731814A

  • Glass fiber composition with ultrahigh specific modulus and glass fiber

    CN115432932A