Organic electroluminescent material and organic electroluminescent device
By adjusting the molecular structure and electrochemical characteristics of organic electroluminescent materials, the problems of low efficiency and short life in the prior art are solved, and high efficiency and long life organic electroluminescent devices are realized, reducing the driving voltage.
Patent Information
- Application Number
- CN202411014589.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
Existing organic electroluminescent materials have low efficiency and short life in applications, making it difficult to achieve both long life, high efficiency and low driving voltage.
By regulating the structure of LA ligands, increasing electrons and groups, changing the molecular spatial structure, and introducing carbazole groups on the dibenzofuran of the LB ligand, adjusting the electrochemical characteristics of the compound and reducing the starting voltage of the device, Improve luminous efficiency and lifespan.
The driving voltage of the organic electroluminescent device is significantly reduced, the luminescence efficiency and life are improved, exceeding the performance of the comparative example compounds.
Smart Images

Figure BDA0004965337410000011 
Figure BDA0004965337410000021 
Figure BDA0004965337410000022
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optoelectronic devices and relates to an organic electroluminescent material and an organic electroluminescent device. Background Art
[0002] Electroluminescent (EL) devices are self-luminous devices that have the advantages of providing wider, higher contrast ratios and faster response times. Organic EL devices were originally developed by Eastman Kodak by using small aromatic diamine molecules and aluminum complexes as materials for forming a light-emitting layer.
[0003] The most important factor that determines the luminous efficiency of organic EL devices is the luminescent material. So far, fluorescent materials have been widely used as luminescent materials. However, in view of the electroluminescent mechanism, the development of phosphorescent materials is one of the best theoretical methods, which can increase the luminous efficiency by four times compared with fluorescent substances. As a new generation of display technology, organic electroluminescent materials (OLEDs) have the advantages of ultra-thin, self-luminous, wide viewing angle, fast response, high luminous efficiency, good temperature adaptability, simple production process, low driving voltage, and low energy consumption. They have been widely used in industries such as flat panel displays, flexible displays, solid-state lighting, and automotive displays.
[0004] Since the first report of high-efficiency organic light-emitting diodes, the industry has been committed to studying how to improve device efficiency and stability. Phosphorescent materials have strong spin-orbit coupling and can simultaneously utilize singlet and triplet excitons, making the quantum efficiency of phosphorescent electroluminescent devices theoretically reach 100%.
[0005] However, the phosphorescent materials used in the prior art have low efficiency and short life when applied to organic light-emitting devices. Therefore, how to provide an organic electroluminescent material with long life, high efficiency and low driving voltage is an urgent problem to be solved by those skilled in the art. Summary of the invention
[0006] In view of the deficiencies of the prior art, the object of the present invention is to provide an organic electroluminescent material and an organic electroluminescent device. The organic electroluminescent material provided by the present invention adjusts the structure of different LA ligands, adds some electrons and groups, etc., changes the molecular spatial structure, changes the intermolecular force, and introduces a carbazole group on the dibenzofuran on the LB ligand, and adds various electronic groups, so that the compound of the present invention, compared with the comparative example compound, changes the molecular spatial configuration and adjusts the electrochemical properties of the compound, so that the obtained organic compound, after being used in the organic electroluminescent device, reduces the starting voltage of the device and improves the luminous efficiency and life of the device.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In one aspect, the present invention provides an organic electroluminescent material having the following structure: Ir(L A )2(L B );
[0009] Where L A Ligand and L B The ligands are:
[0010]
[0011] in,
[0012] The R1-R 24 Independently selected from any one of -H, -D (deuterium), -T (tritium), -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -SiMe3, -GeMe3, substituted or unsubstituted C2-C18 alkyl, substituted or unsubstituted C3-C18 cycloalkyl, substituted or unsubstituted C6-C18 aryl and substituted or unsubstituted 4-18 membered heterocyclyl;
[0013] The substituents on the aforementioned substituent groups are at least selected from one or a combination of at least two of -H, -D, -T, -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -SiMe3, -GeMe3;
[0014] The heteroatom in the aforementioned heterocyclic group is one or a combination of at least two of N, O, and S;
[0015] R1-R8 cannot form a ring structure with other substituents on the ring;
[0016] R9-R 24 They exist independently of each other or form a ring with adjacent groups;
[0017] R9-R 24 When forming a ring with an adjacent group, the ring is a substituted or unsubstituted C3-C20 aliphatic ring, a substituted or unsubstituted C6-C20 aromatic ring, a substituted or unsubstituted C4-C20 aromatic heterocyclic ring, or a substituted or unsubstituted C10-C20 condensed ring;
[0018] R1-R 24 The hydrogen in may or may not be deuterated.
[0019] In the present invention, the organic electroluminescent material has a structure as shown in the following formula I:
[0020]
[0021] Preferably, the amount of deuterated hydrogen in the organic electroluminescent material is ≤100%.
[0022] Preferably, the amount of deuterated hydrogen in the organic electroluminescent material is selected from the group consisting of: 0%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 95%, 99% and 100%.
[0023] More preferably, R1-R 24 Selected from the following groups: -H, -D, -T, -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -SiMe3, -GeMe3, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, tetrahydrofuran, pyrrolidine, thiolane, tetrahydropyran, phenyl, biphenyl, terphenyl, naphthyl, fluorenyl, phenanthrenyl, anthracenyl, indenyl, triphenylene, pyrenyl, tetraphenylene, perylene, chrysene, fused tetraphenylene, fluoranthenyl, furanyl, thienyl, pyrrolyl, imidazolyl, pyrrolyl The invention also includes but is not limited to: 1-diazoles, 2-dazoles, 3-dazoles, 4-dazoles, 5-dazoles, 6-dazoles, 7-dazoles, 8-dazoles, 9-dazoles, 10-dazoles, 11-dazoles, 12-dazoles, 13-dazoles, 14-dazoles, 15-dazoles, 16-dazoles, 17-dazoles, 18-dazoles, 19-dazoles, 20-dazoles, 21-dazoles, 22-dazoles, 23-dazoles, 24-dazoles, 25-dazoles, 26-dazoles, 27-dazoles, 28-dazoles, 29-dazoles, 30-dazoles, 31-dazoles, 32-dazoles, 33-dazoles, 34-dazoles, 35-dazoles, 36-dazoles, 37-dazoles, 38-dazoles, 39-dazoles, 40-dazoles, 41-dazoles, 42-dazoles, 43-dazoles, 44-dazoles, 45-dazoles, 46-dazoles, 47-dazoles, 48-dazoles, 49-dazoles, 50-dazoles, 51-dazoles, 52-dazoles, 53-dazoles, 54-dazoles, 55-dazoles, 56-dazoles, 57-dazoles, 58-dazoles, 59-dazoles,
[0024] R9-R 24 When it forms a ring with an adjacent group, the formed ring is a benzene ring, a naphthalene ring or a furan ring.
[0025] Furthermore, the organic light-emitting material compound has a specific structure as shown in the following formula, but is not limited thereto:
[0026]
[0027]
[0028]
[0029]
[0030]
[0031]
[0032]
[0033]
[0034]
[0035]
[0036]
[0037]
[0038]
[0039]
[0040]
[0041]
[0042]
[0043]
[0044]
[0045]
[0046]
[0047]
[0048]
[0049]
[0050]
[0051]
[0052]
[0053]
[0054]
[0055]
[0056]
[0057]
[0058]
[0059]
[0060]
[0061]
[0062]
[0063]
[0064]
[0065]
[0066]
[0067]
[0068]
[0069]
[0070]
[0071]
[0072]
[0073]
[0074]
[0075]
[0076]
[0077]
[0078]
[0079]
[0080] In the present invention, the preparation process of the compound of formula I is as follows:
[0081]
[0082] The definitions of the groups in the above formula are consistent with those mentioned above and will not be repeated here.
[0083] The synthesis steps are as follows:
[0084] 1. Under nitrogen protection, the compound of formula LA and IrC13·3H2O are placed in a reaction system, and a mixed solution of ethylene glycol ethyl ether and purified water is added. The mixture is refluxed under nitrogen protection, and then cooled to room temperature. A precipitate is precipitated, and the precipitate is filtered, washed and dried with water, anhydrous ethanol, and petroleum ether in turn. The bridged ligand compound of formula III shown in the figure is obtained.
[0085] 2. Weigh the intermediate compound of formula III, add silver trifluoromethanesulfonate, then add dichloromethane and methanol to the system, reflux under nitrogen protection, cool to room temperature, and concentrate the filtrate by column chromatography (short column) until solid precipitates to obtain the iridium complex intermediate compound of formula II shown below.
[0086] 3. Weigh the intermediate compound of formula II and add the ligand of formula L B Then, anhydrous ethanol is added to the system, and the mixture is refluxed under nitrogen protection, filtered, washed with alcohol, and dried. Dichloromethane is used as the solvent, and silica gel column chromatography is used. The filtrate is concentrated and solid is precipitated to obtain the final product of the compound formula I shown in the figure.
[0087] On the other hand, the present invention provides an organic electroluminescent device, which includes a first electrode, a second electrode and an organic thin film layer arranged between the first electrode and the second electrode, the organic thin film layer includes a light-emitting layer, the light-emitting layer includes a main material and a doping material, and the doping material includes the organic electroluminescent material as described above.
[0088] Generally speaking, an organic electroluminescent device includes a first electrode, a second electrode, and an organic material layer between the electrodes. The organic material can be divided into multiple regions. For example, the organic material layer can include a hole transport region, a light emitting layer, and an electron transport region.
[0089] In a specific embodiment, a substrate may be used below the first electrode or above the second electrode. The substrate is a glass or polymer material with excellent mechanical strength, thermal stability, water resistance, and transparency. In addition, a thin film transistor (TFT) may also be provided on the substrate used as a display.
[0090] The first electrode can be formed by sputtering or depositing a material used as the first electrode on a substrate. When the first electrode is used as an anode, transparent conductive oxide materials such as indium tin oxide (ITO), indium zinc oxide (IZO), tin dioxide (SnO2), zinc oxide (ZnO) and any combination thereof can be used. In addition, the anode material can also be selected from materials and combinations thereof that facilitate hole injection other than the listed anode materials, including materials known to be suitable for anodes. When the first electrode is used as a cathode, metals or alloys such as magnesium (Mg), silver (Ag), aluminum (Al), aluminum-lithium (Al-Li), calcium (Ca), magnesium-indium (Mg-In), magnesium-silver (Mg-Ag) and any combination thereof can be used. In addition to the cathode materials listed above, the cathode material can also be a material and a combination thereof that facilitates electron injection, including materials known to be suitable for cathodes.
[0091] The hole transport region may include at least one of a hole injection layer, a first hole transport layer, and a light-emitting auxiliary layer (a second hole transport layer, an electron blocking layer), and the electron transport region may include at least one of an electron buffer layer, a hole blocking layer, an electron transport layer, and an electron injection layer.
[0092] The organic material layer can be formed on the electrode by vacuum thermal evaporation, spin coating, printing and the like. The compound used as the organic material layer can be an organic small molecule, an organic macromolecule and a polymer, and a combination thereof. The hole transport region is located between the anode and the light-emitting layer. The hole transport region can be a hole transport layer (HTL) of a single-layer structure, including a single-layer hole transport layer containing only one compound and a single-layer hole transport layer containing multiple compounds. The hole transport region can also be a multilayer structure including at least one layer of a hole injection layer (HIL), a hole transport layer (HTL), and an electron blocking layer (EBL).
[0093] The material of the hole transport layer can be selected from, but not limited to, phthalocyanine derivatives such as CuPc, conductive polymers or polymers containing conductive dopants such as polyphenylene ethylene, polyaniline / dodecylbenzenesulfonic acid (Pani / DBSA), poly(3,4-ethylenedioxythiophene) / poly(4-styrenesulfonate) (PEDOT / PSS), polyaniline / camphorsulfonic acid (Pani / CSA), polyaniline / poly(4-styrenesulfonate) (Pani / PSS), aromatic amine derivatives such as the compounds shown in HT-1 to HT-34 below; or any combination thereof.
[0094]
[0095]
[0096]
[0097] But it is not limited to the above materials.
[0098] The hole injection layer is located between the anode and the hole transport layer. The hole injection layer can be a single compound material or a combination of multiple compounds. For example, the hole injection layer can use one or more compounds of HT-1 to HT-34 above, or one or more compounds of HI1 to HI3 below; or one or more compounds of HT-1 to HT-34 can be doped with one or more compounds of HI-1 to HI-3 below:
[0099]
[0100] But it is not limited to the above materials.
[0101] The OLED organic material layer may further include an electron transport region between the light emitting layer and the cathode.
[0102] The light-emitting layer may include a light-emitting dye (i.e., a dopant) that can emit light of different wavelength spectra, and may also include a host material (Host) at the same time. The light-emitting layer may be a monochrome light-emitting layer that emits a single color such as red, green, or blue. A plurality of monochrome light-emitting layers of different colors may be arranged in a plane according to a pixel pattern, or may be stacked together to form a color light-emitting layer. When light-emitting layers of different colors are stacked together, they may be separated from each other or may be connected to each other. The light-emitting layer may also be a single color light-emitting layer that can simultaneously emit different colors such as red and green.
[0103] According to different technologies, the luminescent layer material can be made of different materials such as phosphorescent electroluminescent materials and thermally activated delayed fluorescent luminescent materials. In an OLED device, a single luminescent technology can be used, or a combination of multiple different luminescent technologies can be used. These different luminescent materials classified by technology can emit light of the same color or different colors.
[0104] The compound of formula I of the present invention is used as a doping material in the light-emitting layer.
[0105] The electron transport region may be a single-layer electron transport layer (ETL), including a single-layer electron transport layer containing only one compound and a single-layer electron transport layer containing multiple compounds. The electron transport region may also be a multi-layer structure including at least one layer of an electron injection layer (EIL), an electron transport layer (ETL), and a hole blocking layer (HBL).
[0106] In one aspect of the present invention, the electron transport layer material can be selected from, but not limited to, one or more combinations of ET-1 to ET-57 listed below.
[0107]
[0108]
[0109]
[0110] But it is not limited to the above materials.
[0111] The device may also include an electron injection layer located between the electron transport layer and the cathode. The electron injection layer material includes but is not limited to one or more combinations of the following: LiF, NaCl, CsF, Li2O, Cs2CO3, BaO, Na, Li, Ca.
[0112] Compared with the prior art, the present invention has the following beneficial effects:
[0113] By adjusting different L A The structure of the ligand, adding some electrons and groups, etc., changes the molecular spatial structure and the intermolecular forces, while at the same time B A carbazole group is introduced into the dibenzofuran on the ligand, and some groups are added at the same time, so that the compound of the present invention is compared with the comparative example compound, by changing the molecular spatial configuration and adjusting the electrochemical properties of the compound, so that the compound of the present invention is used as a doping material for the light-emitting layer, and the organic electroluminescent device prepared by the compound has a significantly lower driving voltage, and the luminous efficiency and life are significantly improved compared with the organic electroluminescent device prepared in the comparative example. DETAILED DESCRIPTION
[0114] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0115] Synthesis example 1
[0116] This synthesis example provides an organometallic compound Ⅰ-151, i.e., a compound numbered Ⅰ-151. The specific synthesis steps are as follows:
[0117]
[0118] Under nitrogen protection system, weigh compound 4,6-dibromodibenzofuran (CAS: 201138-91-2) (400mmol), anhydrous potassium carbonate (1200mmol) are put into the reaction system, 1000ml toluene, 500ml anhydrous ethanol, 500ml purified water are added, Pd(PPh3)4 (8mmol) is added under nitrogen protection, 2-pyridineboric acid (CAS: 197958-29-5) (400mmol) is added, after addition, reflux at 100°C for 24h under nitrogen protection, and then cool to 25°C. After the reaction is cooled, extract with ethyl acetate, wash three times with saturated brine, dry with anhydrous magnesium sulfate, and concentrate under reduced pressure. The crude product is subjected to column chromatography (200-300 mesh, 600g) with developing agent EA:PE=1:15 to remove impurities, and the receiving liquid is vortexed until no liquid flows out, and vacuum dried to obtain the intermediate L of the compound shown. BⅢ -151 (53.17 g, yield 41%), its HPLC purity was greater than 99.5%.
[0119] Mass spectrometry test value: 323.06.
[0120]
[0121] Under nitrogen protection system, weigh the intermediate compound L BⅢ -151 (160 mmol), 2-nitrobenzeneboronic acid (CAS: 5570-19-4) (176 mmol), anhydrous potassium carbonate (480 mmol) were put into the reaction system, 900 ml toluene, 450 mL anhydrous ethanol, 450 mL pure water were added, Pd (PPh3) 4 (3.2 mmol) was added under nitrogen protection, and refluxed at 100 ° C for 20 h under nitrogen protection. Then cooled to 25 ° C, after the reaction was cooled, extracted with ethyl acetate, washed three times with saturated brine, dried over anhydrous magnesium sulfate, concentrated under reduced pressure, and the crude product was column chromatographed (200-300 mesh, 600 g) with a developing agent of EA: PE = 1: 12 to remove impurities, and the receiving liquid was vortexed until no liquid flowed out, and vacuum dried to obtain the intermediate L of the compound shown. BⅡ -151 (50.41 g, yield 86%), its HPLC purity was greater than 99.5%.
[0122] Mass spectrometry test value: 366.51.
[0123]
[0124] Under nitrogen protection system, weigh the intermediate compound L BⅡ-151 (130 mmol), triethyl phosphite [P(OEt)3] (260 mL) were placed in the reaction system, 1,2-dichlorobenzene (1,2-DCB) (500 mL) was added, and the reaction was refluxed for 13 h under nitrogen protection. After 13 hours, the solvent was distilled, and the solid was dissolved in dichloromethane and separated by silica gel column chromatography to obtain compound intermediate L BⅠ -151 (22.60 g, yield 52%), its HPLC purity was greater than 99.5%.
[0125] Mass spectrometry test value: 334.45.
[0126]
[0127] Under nitrogen protection system, weigh compound L BⅠ -151 (60.5 mmol), bromobenzene (CAS: 108-86-1) (55 mmol), Cu powder (27.5 mmol), K2CO3 (110 mmol) were placed in the reaction system, 1,2-DCB (600 mL) was added, and the reaction was refluxed for 24 h under nitrogen protection. After 24 hours, the solvent was distilled, and the obtained solid was dissolved in dichloromethane, and separated by silica gel column chromatography to obtain compound L B -151 (14.22 g, yield 63%), its HPLC purity was greater than 99.5%.
[0128] Mass spectrometry test value: 410.45.
[0129]
[0130] Under nitrogen protection system, weigh compound 2-bromopyridine (CAS: 109-04-6) (75mmol), 3,4-dimethylphenylboronic acid (CAS: 55499-43-9) (82.5mmol), anhydrous potassium carbonate (225mmol) and put into the reaction system, add 600ml toluene, 300ml anhydrous ethanol, 300ml purified water, add Pd(PPh3)4 (1.5mmol) under nitrogen protection, reflux at 100℃ for 26h under nitrogen protection, and then cool to 25℃. After the reaction is cooled, extract with ethyl acetate, wash three times with saturated brine, dry with anhydrous magnesium sulfate, and concentrate under reduced pressure. The crude product is chromatographed on a column (200-300 mesh, 500g), and the developing agent EA:PE=1:18 is used to remove impurities. The receiving liquid is vortexed until no liquid flows out, and vacuum dried to obtain the intermediate L of the compound shown. AⅠ -151 (11.68 g, yield 85%), its HPLC purity was greater than 99.5%.
[0131] Mass spectrometry test value: 183.41.
[0132]
[0133] Under nitrogen protection system, add intermediate L AⅠ -151 (60 mmol), DMSO-d6 (1620 mmol), NaOH (66 mmol), N2 replacement three times and N2 protection, heating reaction at 100 ° C for 14 h. After the reaction is completed, ethyl acetate is extracted, saturated brine is washed three times, and concentrated under reduced pressure. The crude product is purified by column chromatography with a gradient elution of PE:EA = 15:1 to 5:1 (v / v) to obtain intermediate L A -151 (10.68 g, yield 94%), its HPLC purity was greater than 99.5%.
[0134] The test value is 189.46.
[0135]
[0136] Under nitrogen protection system, weigh the ligand L A -151 (50mmol), IrC13·3H20 (22mmol) were placed in the reaction system, and a mixed solution of 360ml ethylene glycol ethyl ether and 120ml pure water was added. The mixture was refluxed for 28 hours under nitrogen protection, and then cooled to room temperature. A precipitate was precipitated, and the precipitate was filtered, washed with water, anhydrous ethanol, and petroleum ether in turn, and dried. The bridged ligand III-151 (7.05g, yield 53%) was obtained.
[0137]
[0138] Weigh the intermediate formula III-151 (5 mmol), add silver trifluoromethanesulfonate (11 mmol), then add 450 ml of dichloromethane and 150 ml of methanol to the system, reflux for 26 hours under nitrogen protection, cool to room temperature, and concentrate the filtrate by column chromatography (short column) until solid precipitates. The iridium complex intermediate formula II-151 shown is obtained (7.41 g, yield 95%).
[0139]
[0140] Weigh the intermediate II-151 (9 mmol) and add the ligand L B -151 (22.5mmol), then add 200ml of anhydrous ethanol to the system, reflux for 36 hours under nitrogen protection, filter, wash with alcohol, and dry. Use dichloromethane as solvent, use silica gel column chromatography, concentrate the filtrate and precipitate solid to obtain the final compound shown in formula I-151 (2.38g, yield 27%), and its HPLC purity is greater than 99%.
[0141] The organometallic compound I-151 was subjected to the following analytical tests:
[0142] HPLC purity: greater than 99.5%;
[0143] The mass spectrometry test value was 978.46.
[0144] Elemental analysis: Calculated values are C, 67.53; H, 5.46; N, 5.73; O, 1.64. Found values are C, 67.54; H, 5.45; N, 5.75; O, 1.63.
[0145] 1 H NMR (400 MHz, deuterated chloroform) δ 8.71–8.64 (m, 2H), 8.64 (t, 1H), 7.95 (dd, 1H), 7.77 (dd, 2H), 7.73 (s, 2H), 7.74–7.64 (m, 5H), 7.61–7.47 (m, 5H), 7.47–7.42 (m, 2H), 7.42–7.34 (m, 2H), 7.34–7.27 (m, 1H), 7.30 (s, 2H), 7.27–7.19 (m, 4H).
[0146] Synthesis example 2
[0147] This synthesis example provides an organometallic compound I-387, i.e., a compound numbered I-387. The specific synthesis steps are as follows:
[0148]
[0149] Under nitrogen protection system, 2-bromo-4-isopropylpyridine (CAS: 1086381-43-2) (600mmol), biboric acid pinacol ester (900mmol), X-Phos (72mmol), palladium acetate (12mmol), potassium acetate (1800mmol) and dioxane (1500mL) were added to the reaction system in sequence, N2 was replaced three times and N2 was protected, and heated and stirred at 100°C overnight. After the reaction was completed, diatomaceous earth and anhydrous magnesium sulfate were filtered, ethyl acetate was washed twice, and the organic phase was collected and concentrated under reduced pressure to obtain a crude product intermediate of formula L BⅤ -387 was used directly in the next step.
[0150]
[0151] Under nitrogen protection, weigh the compound 4,6-dibromodibenzofuran (CAS: 201138-91-2) (500 mmol), anhydrous potassium carbonate (1500 mmol) and put it into the reaction system, add 1200 ml of toluene, 600 ml of anhydrous ethanol, 600 ml of purified water, add Pd(PPh3)4 (10 mmol) under nitrogen protection, add L BⅤ -387 (600mmol), after addition, reflux at 100℃ for 23h under nitrogen protection, then cool to 25℃, after cooling, extract with ethyl acetate, wash three times with saturated brine, dry with anhydrous magnesium sulfate, concentrate under reduced pressure, and column chromatography (200-300 mesh, 650g) of the crude product with developing agent EA:PE=1:16 to remove impurities, vortex the receiving solution until no liquid flows out, and vacuum dry to obtain the intermediate L shown in the figure BⅣ -387 (82.41 g, 45% yield) with HPLC purity greater than 99.5%.
[0152] Mass spectrometry test value: 365.26.
[0153]
[0154] Under nitrogen protection system, weigh the intermediate compound L BⅣ -387 (200 mmol), 2-nitrobenzeneboronic acid (CAS: 5570-19-4) (220 mmol), anhydrous potassium carbonate (600 mmol) were placed in the reaction system, 1100 ml toluene, 550 mL anhydrous ethanol, 550 mL pure water were added, Pd (PPh3) 4 (4 mmol) was added under nitrogen protection, and refluxed at 100 ° C for 21 hours under nitrogen protection. Then cooled to 25 ° C, after the reaction was cooled, extracted with ethyl acetate, washed three times with saturated brine, dried over anhydrous magnesium sulfate, concentrated under reduced pressure, and the crude product was column chromatographed (200-300 mesh, 550 g) with a developing agent of EA: PE = 1: 14 to remove impurities, and the receiving liquid was vortexed until no liquid flowed out, and vacuum dried to obtain the intermediate L of the compound shown. BⅢ -387 (71.89 g, yield 88%) with HPLC purity greater than 99.5%.
[0155] Mass spectrometry test value: 408.49.
[0156]
[0157] Under nitrogen protection system, weigh the intermediate compound L BⅢ-387 (170 mmol), triethyl phosphite [P(OEt)3] (340 mL) were placed in the reaction system, 1,2-dichlorobenzene (1,2-DCB) (700 mL) was added, and the reaction was refluxed for 15 h under nitrogen protection. After 15 hours, the solvent was distilled, and the solid was dissolved in dichloromethane and separated by silica gel column chromatography to obtain compound intermediate L BⅡ -387 (32.64 g, yield 51%) with HPLC purity greater than 99.5%.
[0158] Mass spectrometry test value: 376.48.
[0159]
[0160] Under nitrogen protection system, weigh compound L BⅡ -387 (82.5 mmol), bromobenzene (CAS: 108-86-1) (75 mmol), Cu powder (37.5 mmol), K2CO3 (150 mmol) were placed in the reaction system, 1,2-DCB (900 mL) was added, and the reaction was refluxed for 24 h under nitrogen protection. After 24 hours, the solvent was distilled, and the obtained solid was dissolved in dichloromethane, and separated by silica gel column chromatography to obtain compound L BⅠ -387 (22.40 g, yield 66%) with HPLC purity greater than 99.5%.
[0161] Mass spectrometry test value: 452.38.
[0162]
[0163] Under nitrogen protection system, add intermediate L BⅠ -387 (45 mmol), DMSO-d6 (1800 mmol), NaOH (49.5 mmol), N2 replacement three times and N2 protection, heating reaction at 100 ° C for 20 h. After the reaction is completed, ethyl acetate is extracted, saturated brine is washed three times, and concentrated under reduced pressure. The crude product is purified by column chromatography with a gradient elution of PE:EA = 15:1 to 5:1 (v / v) to obtain intermediate L B -387 (14.70 g, yield 72%) with HPLC purity greater than 99.5%.
[0164] Mass spectrometry test value: 453.38.
[0165]
[0166] Under nitrogen protection system, weigh the compound 5-methyl-2-phenylpyridine (CAS: 27012-22-2) (120mmol) and put it into the reaction system, add 800mL THF, cool to -78°C, start to drop n-BuLi (2.5M, 72mL), keep the internal temperature at 78±5°C, after the drop, keep the temperature for 4h, start to drop TMSCl (180mmol), keep the internal temperature at 78±5°C, after the drop, keep the temperature for 4h, then slowly return to room temperature for 10h, extract with ethyl acetate, wash three times with saturated brine, dry with anhydrous magnesium sulfate, concentrate under reduced pressure, and remove impurities by column chromatography (200-300 mesh, 600g) of the crude product, with the developing agent EA:PE=1:15, vortex the receiving solution until no liquid flows out, and dry under vacuum to obtain the intermediate L of the compound shown. A -387 (14.19 g, yield 52%) with HPLC purity greater than 99.5%.
[0167] Mass spectrometry test value: 227.42.
[0168]
[0169] Under nitrogen protection system, weigh the ligand L A -387 (66mmol), IrC13·3H2O (22mmol) were placed in the reaction system, and a mixed solution of 380ml of ethylene glycol ethyl ether and 127ml of pure water was added. The mixture was refluxed for 28 hours under nitrogen protection, and then cooled to room temperature. A precipitate was precipitated, and the precipitate was filtered, washed and dried with water, anhydrous ethanol, and petroleum ether in turn. The bridged ligand III-387 (7.63g, yield 51%) was obtained.
[0170]
[0171] Weigh the intermediate formula III-387 (5mmol), add silver trifluoromethanesulfonate (12.5mmol), then add 420ml of dichloromethane to the system, add 140ml of methanol, reflux for 26 hours under nitrogen protection, cool to room temperature, and concentrate the filtrate by column chromatography (short column) until solid precipitates. The iridium complex intermediate formula II-387 (7.96g, yield 93%) is obtained.
[0172]
[0173] Weigh the intermediate II-387 (9 mmol) and add the ligand L B-387 (19.8 mmol), then add 250 mL of anhydrous ethanol to the system, reflux for 36 hours under nitrogen protection, filter, wash with alcohol, and dry. Use dichloromethane as solvent, use silica gel column chromatography, concentrate the filtrate and precipitate solid to obtain the final compound shown in formula I-387 (3.56 g, yield 36%), and its HPLC purity is greater than 99%.
[0174] The organometallic compound I-387 was subjected to the following analytical tests:
[0175] HPLC purity: greater than 99.5%;
[0176] The mass spectrometry test value was 1097.49.
[0177] Elemental analysis: calculated values are C, 65.66; H, 5.14; N, 5.10; O, 1.46; Si, 5.12. Measured values are C, 65.68; H, 5.12; N, 5.13; O, 1.45; Si, 5.10.
[0178] 1H NMR (400 MHz, deuterated chloroform) δ8.84 (d, 2H), 8.61 (d, 1H), 8.11 (dd, 2H), 7.96 (s, 1H), 7.90 (dd, 2H), 7.84 (dd, 2H), 7.77 (d, 1H), 7.71–7.62 (m, 3H), 7.60–7.52 (m, 2H), 7.54–7.47 (m, 3H), 7.47–7.21 (m, 8H), 7.19–7.09 (m, 3H), 1.28 (s, 6H), 0.46 (s, 18H).
[0179] Synthesis example 3
[0180] This synthesis example provides an organometallic compound I-527, i.e., a compound numbered I-527. The specific synthesis steps are as follows:
[0181]
[0182] Under nitrogen protection system, 2-bromo-4-neopentylpyridine (CAS: 2387538-18-1) (600mmol), biboric acid pinacol ester (900mmol), X-Phos (72mmol), palladium acetate (12mmol), potassium acetate (1800mmol) and dioxane (2000mL) were added to the reaction system in sequence, N2 was replaced three times and N2 was protected, and heated and stirred at 100°C overnight. After the reaction was completed, diatomaceous earth and anhydrous magnesium sulfate were filtered, ethyl acetate was washed twice, and the organic phase was collected and concentrated under reduced pressure to obtain a crude product intermediate formula L BⅤ -527 is used directly in the next step.
[0183]
[0184] Under nitrogen protection, weigh the compound 4,6-dibromodibenzofuran (CAS: 201138-91-2) (500 mmol), anhydrous potassium carbonate (1500 mmol) and put it into the reaction system, add 1300 ml of toluene, 650 mL of anhydrous ethanol, 650 mL of purified water, add Pd(PPh3)4 (10 mmol) under nitrogen protection, add L BⅤ -527 (600mmol), after addition, reflux at 100℃ for 23h under nitrogen protection, then cool to 25℃, after cooling, extract with ethyl acetate, wash three times with saturated brine, dry with anhydrous magnesium sulfate, concentrate under reduced pressure, and column chromatography (200-300 mesh, 630g) of the crude product with developing agent EA:PE=1:16 to remove impurities, vortex the receiving solution until no liquid flows out, and vacuum dry to obtain the intermediate L shown in the figure BⅣ -527 (82.81 g, 42% yield) with HPLC purity greater than 99.5%.
[0185] Mass spectrometry test value: 393.43.
[0186]
[0187] Under nitrogen protection system, weigh the intermediate compound L BⅣ -527 (200 mmol), 2-nitrobenzeneboronic acid (CAS: 5570-19-4) (220 mmol), anhydrous potassium carbonate (600 mmol) were placed in the reaction system, 1300 ml toluene, 650 mL anhydrous ethanol, 650 mL pure water were added, Pd (PPh3) 4 (4 mmol) was added under nitrogen protection, and refluxed at 100 ° C for 21 hours under nitrogen protection. Then cooled to 25 ° C, after the reaction was cooled, extracted with ethyl acetate, washed three times with saturated brine, dried over anhydrous magnesium sulfate, concentrated under reduced pressure, and the crude product was column chromatographed (200-300 mesh, 550 g) with a developing agent of EA: PE = 1: 10 to remove impurities, and the receiving liquid was vortexed until no liquid flowed out, and vacuum dried to obtain the intermediate L of the compound shown. BⅢ -527 (78.57 g, yield 90%), with HPLC purity greater than 99.5%.
[0188] Mass spectrometry test value: 436.35.
[0189]
[0190] Under nitrogen protection system, weigh the intermediate compound L BⅢ-527 (170 mmol), triethyl phosphite [P(OEt)3] (340 mL) were placed in the reaction system, 1,2-dichlorobenzene (1,2-DCB) (700 mL) was added, and the reaction was refluxed for 15 h under nitrogen protection. After 15 hours, the solvent was distilled, and the solid was dissolved in dichloromethane and separated by silica gel column chromatography to obtain compound intermediate L BⅡ -527 (38.51 g, yield 56%), with HPLC purity greater than 99.5%.
[0191] Mass spectrometry test value: 404.34.
[0192]
[0193] Under nitrogen protection system, weigh compound L BⅡ -527 (82.5 mmol), bromobenzene (CAS: 108-86-1) (75 mmol), Cu powder (37.5 mmol), K2CO3 (150 mmol) were placed in the reaction system, 1,2-DCB (900 mL) was added, and the reaction was refluxed for 24 h under nitrogen protection. After 24 hours, the solvent was distilled, and the obtained solid was dissolved in dichloromethane, and separated by silica gel column chromatography to obtain compound L BⅠ -527 (24.87 g, yield 69%), with HPLC purity greater than 99.5%.
[0194] Mass spectrometry test value: 480.41.
[0195]
[0196] Under nitrogen protection system, add intermediate L BⅠ -527 (45mmol), DMSO-d6 (1800mmol), NaOH (49.5mmol), N2 replacement three times and N2 protection, heating reaction at 100℃ for 20h. After the reaction is completed, extraction with ethyl acetate, washing with saturated brine three times, and concentration under reduced pressure. The crude product is purified by column chromatography with a gradient elution of PE:EA=15:1 to 5:1 (v / v) to obtain intermediate L B -527 (17.37 g, yield 80%), with HPLC purity greater than 99.5%.
[0197] Mass spectrometry test value: 482.44.
[0198] 1H NMR (400 MHz, deuterated chloroform) δ8.57 (d, 1H), 8.04 (dd, 1H), 7.99 (dd, 1H), 7.95 (dd, 1H), 7.87 (d, 1H), 7.66 (d, 1H), 7.59 (dd, 1H), 7.57–7.51 (m, 2H), 7.51 (d, 2H), 7.46–7.40 (m, 2H), 7.40–7.30 (m, 2H), 7.23 (td, 1H), 7.10 (dd, 1H), 1.12 (s, 9H).
[0199]
[0200] Under nitrogen protection system, weigh the ligand L A -527 (CAS: 1008-89-5) (55mmol), IrC13·3H20 (22mmol) were placed in the reaction system, and a mixed solution of 400ml of ethylene glycol ethyl ether and 133ml of pure water was added. The mixture was refluxed for 28 hours under nitrogen protection, and then cooled to room temperature. A precipitate was precipitated, and the precipitate was filtered, washed with water, anhydrous ethanol, and petroleum ether in turn, and dried. The bridged ligand III-527 (7.08g, yield 60%) was obtained.
[0201]
[0202] Weigh the intermediate formula III-527 (5mmol), add silver trifluoromethanesulfonate (12.5mmol), then add 450mL of dichloromethane to the system, add 150ml of methanol, reflux for 26 hours under nitrogen protection, cool to room temperature, and concentrate the filtrate by column chromatography (short column) until solid precipitates. The iridium complex intermediate formula II-527 (6.97g, yield 98%) is obtained.
[0203]
[0204] Weigh the intermediate II-527 (9 mmol) and add the ligand L B -527 (18 mmol), then add 300 ml of anhydrous ethanol to the system, reflux for 36 hours under nitrogen protection, filter, wash with alcohol, and dry. Use dichloromethane as solvent, use silica gel column chromatography, concentrate the filtrate and precipitate solid to obtain the final compound shown in formula I-527 (3.62 g, yield 41%), and its HPLC purity is greater than 99%.
[0205] The organometallic compound I-527 was subjected to the following analytical tests:
[0206] HPLC purity: greater than 99.5%;
[0207] The mass spectrometry test value was 982.45.
[0208] Elemental analysis: Calculated values are C, 68.48; H, 4.62; N, 5.70; O, 1.63. Found values are C, 68.49; H, 4.61; N, 5.72; O, 1.61.
[0209] 1H NMR (400 MHz, deuterated chloroform) δ8.64 (dd, 3H), 8.09 (dd, 2H), 7.95 (dd, 1H), 7.77 (d, 1H), 7.75–7.64 (m, 5H), 7.61–7.54 (m, 2H), 7.54–7.48 (m, 3H), 7.47–7.41 (m, 5H), 7.37 (td, 1H), 7.31–7.26 (m, 3H), 7.26–7.20 (m, 3H), 7.16–7.07 (m, 3H), 1.06 (s, 9H).
[0210] Synthesis example 4
[0211] This synthesis example provides an organometallic compound Ⅰ-638, i.e., a compound numbered Ⅰ-638. The specific synthesis steps are as follows:
[0212]
[0213] Under nitrogen protection system, weigh compound 4,6-dibromodibenzofuran (CAS: 201138-91-2) (400mmol), anhydrous potassium carbonate (1200mmol) are put into the reaction system, add 1300ml toluene, 650ml anhydrous ethanol, 650ml purified water, add Pd(PPh3)4 (8mmol) under nitrogen protection, add 4-phenylpyridine-2-boric acid (CAS: 1257879-78-9) (400mmol), reflux at 100°C for 24h under nitrogen protection, and then cool to 25°C. After the reaction is cooled, extract with ethyl acetate, wash three times with saturated brine, dry with anhydrous magnesium sulfate, and concentrate under reduced pressure. The crude product is subjected to column chromatography (200-300 mesh, 700g) with developing agent EA:PE=1:14 to remove impurities, and the receiving liquid is vortexed until no liquid flows out, and vacuum dried to obtain the intermediate L of the compound shown. BⅢ -638 (75.25 g, 47% yield) with HPLC purity greater than 99.5%.
[0214] Mass spectrometry test value: 399.15.
[0215]
[0216] Under nitrogen protection system, weigh the intermediate compound L BⅢ-638 (160 mmol), 2-nitrobenzeneboronic acid (CAS: 5570-19-4) (176 mmol), anhydrous potassium carbonate (480 mmol) were put into the reaction system, 1100 ml toluene, 550 mL anhydrous ethanol, 550 mL pure water were added, Pd (PPh3) 4 (3.2 mmol) was added under nitrogen protection, and refluxed at 100 ° C for 22 h under nitrogen protection. Then cooled to 25 ° C, after the reaction was cooled, extracted with ethyl acetate, washed three times with saturated brine, dried over anhydrous magnesium sulfate, concentrated under reduced pressure, and the crude product was column chromatographed (200-300 mesh, 600 g) with a developing agent of EA: PE = 1: 12 to remove impurities, and the receiving liquid was vortexed until no liquid flowed out, and vacuum dried to obtain the intermediate L of the compound shown. BⅡ -638 (63.71 g, yield 90%), with HPLC purity greater than 99.5%.
[0217] Mass spectrometry test value: 442.36.
[0218]
[0219] Under nitrogen protection system, weigh the intermediate compound L BⅡ -638 (130 mmol), triethyl phosphite [P(OEt)3] (260 mL) were placed in the reaction system, 1,2-dichlorobenzene (1,2-DCB) (500 mL) was added, and the reaction was refluxed for 15 h under nitrogen protection. After 15 hours, the solvent was distilled, and the solid was dissolved in dichloromethane and separated by silica gel column chromatography to obtain compound intermediate L BⅠ -638 (29.88 g, yield 56%), with HPLC purity greater than 99.5%.
[0220] Mass spectrometry test value: 410.38.
[0221]
[0222] Under nitrogen protection system, weigh compound L BⅠ -638 (60.5 mmol), bromobenzene (CAS: 108-86-1) (55 mmol), Cu powder (27.5 mmol), K2CO3 (110 mmol) were placed in the reaction system, 1,2-DCB (600 mL) was added, and the reaction was refluxed for 20 h under nitrogen protection. After 20 hours, the solvent was distilled, and the obtained solid was dissolved in dichloromethane, and separated by silica gel column chromatography to obtain compound L B -638 (18.47 g, 69% yield) with HPLC purity greater than 99.5%.
[0223] Mass spectrometry test value: 486.36.
[0224]
[0225] Under nitrogen protection system, compound 5-methyl-2-phenylpyridine (CAS: 27012-22-2) (70mmol), DMSO-d6 (1890mmol), NaOH (77mmol) were added in sequence, N2 was replaced three times and N2 was protected, and the reaction was heated at 100°C for 18h. After the reaction was completed, ethyl acetate was extracted, saturated brine was washed three times, and the reaction was concentrated under reduced pressure. The crude product was purified by column chromatography with a gradient elution of PE:EA = 15:1 to 5:1 (v / v) to obtain intermediate L A -638 (10.61 g, yield 88%), with HPLC purity greater than 99.5%.
[0226] The mass spectrometry test value was 172.38.
[0227]
[0228] Under nitrogen protection system, weigh the ligand L A -638 (66mmol), IrCl3·3H2O (22mmol) were placed in the reaction system, and a mixed solution of 330mL ethylene glycol ethyl ether and 110mL pure water was added. The mixture was refluxed for 30 hours under nitrogen protection, and then cooled to room temperature. A precipitate was precipitated, and the precipitate was filtered, washed with water, anhydrous ethanol, and petroleum ether in turn, and dried. The bridged ligand III-638 (7.15g, yield 57%) was obtained.
[0229]
[0230] Weigh the intermediate formula III-638 (5 mmol), add silver trifluoromethanesulfonate (11 mmol), then add 460 mL of dichloromethane to the system, add 153 mL of methanol, reflux for 29 hours under nitrogen protection, cool to room temperature, and concentrate the filtrate by column chromatography (short column) until solid precipitates. The iridium complex intermediate formula II-638 (6.94 g, yield 93%) is obtained.
[0231]
[0232] Weigh the intermediate II-638 (9 mmol) and add the ligand L B -151 (22.5mmol), then add 230ml of anhydrous ethanol to the system, reflux for 38 hours under nitrogen protection, filter, wash with alcohol, and dry. Use dichloromethane as solvent, use silica gel column chromatography, concentrate the filtrate and precipitate solid to obtain the final compound shown in formula I-638 (2.75g, yield 30%), and its HPLC purity is greater than 99%.
[0233] The organometallic compound I-638 was subjected to the following analytical tests:
[0234] HPLC purity: greater than 99.5%;
[0235] The mass spectrometry test value is 1020.38.
[0236] Elemental analysis: Calculated values are C, 69.46; H, 4.64; N, 5.49; O, 1.57. Measured values are C, 69.44; H, 4.66; N, 5.48; O, 1.58.
[0237] 1H NMR (400 MHz, deuterated chloroform) δ9.27 (d, 1H), 8.46 (d, 1H), 8.33 (d, 2H), 8.11 (dd, 2H), 7.95 (dd, 1H), 7.77 (d, 1H), 7.69 (dt, 3H), 7.64 (d, 2H), 7.60–7.21 (m, 20H), 7.13 (td, 2H).
[0238] Synthesis example 5
[0239] This synthesis example provides an organometallic compound Ⅰ-793, i.e., a compound numbered Ⅰ-793. The specific synthesis steps are as follows:
[0240]
[0241] Under nitrogen protection system, weigh compound 5-bromo-2-chlorotoluene (CAS: 54932-72-8) (3750mmol), anhydrous potassium carbonate (11250mmol) are put into the reaction system, 6000ml toluene, 3000mL anhydrous ethanol, 3000mL purified water are added, Pd(PPh3)4 (37.5mmol) is added under nitrogen protection, neopentylboric acid (CAS: 701261-35-0) (3750mmol) is added, and after the addition, reflux at 100°C for 28h under nitrogen protection, and then cool to 25°C. After the reaction is cooled, extract with ethyl acetate, wash three times with saturated brine, dry with anhydrous magnesium sulfate, and concentrate under reduced pressure. The crude product is subjected to column chromatography (200-300 mesh, 3000g) with developing agent EA:PE=1:14 to remove impurities, and the receiving liquid is vortexed until no liquid flows out, and vacuum dried to obtain the intermediate L of the compound shown. BⅧ -793 (317.21 g, 43% yield) with HPLC purity greater than 99.5%.
[0242] Mass spectrometry test value: 196.21.
[0243]
[0244] Under nitrogen protection system, compound L was added in sequence BⅧ -793 (1500mmol), biboric acid pinacol ester (2250mmol), X-Phos (120mmol), palladium acetate (60mmol), potassium acetate (3000mmol) and dioxane (3000mL) were added to the reaction system, replaced with N2 three times and protected with N2, and heated and stirred at 100°C overnight. After the reaction was completed, the mixture was filtered with diatomaceous earth and anhydrous magnesium sulfate, washed twice with ethyl acetate, and the organic phase was collected and concentrated under reduced pressure to obtain a crude product intermediate of formula L BⅦ -793 is used directly in the next step.
[0245]
[0246] Under nitrogen protection, weigh the compound 4-bromo-2-chloropyridine (CAS: 73583-37-6) (1500mmol), anhydrous potassium carbonate (4500mmol) and put it into the reaction system, add 4000ml toluene, 2000mL anhydrous ethanol, 2000mL purified water, add Pd(PPh3)4 (15mmol) under nitrogen protection, add L BⅦ -793 (1500mmol), after addition, reflux at 100℃ for 30h under nitrogen protection, then cool to 25℃, after cooling, extract with ethyl acetate, wash three times with saturated brine, dry with anhydrous magnesium sulfate, concentrate under reduced pressure, and column chromatograph the crude product (200-300 mesh, 2000g) with developing agent EA:PE=1:14 to remove impurities, vortex the receiving solution until no liquid flows out, and dry under vacuum to obtain the intermediate L shown in the figure BⅥ -793 (193.05 g, yield 47%), with HPLC purity greater than 99.5%.
[0247] Mass spectrometry test value: 273.36.
[0248]
[0249] Under nitrogen protection system, compound L was added in sequence BⅥ -793 (600 mmol), biboric acid pinacol ester (900 mmol), X-Phos (48 mmol), palladium acetate (24 mmol), potassium acetate (1800 mmol) and dioxane (2500 mL) were added to the reaction system, replaced with N2 three times and protected with N2, and heated and stirred at 100°C overnight. After the reaction was completed, the mixture was filtered with diatomaceous earth and anhydrous magnesium sulfate, washed twice with ethyl acetate, and the organic phase was collected and concentrated under reduced pressure to obtain a crude product intermediate of formula L BⅤ -793 is used directly in the next step.
[0250]
[0251] Under nitrogen protection, weigh the compound 4,6-dibromodibenzofuran (CAS: 201138-91-2) (500mmol), anhydrous potassium carbonate (1500mmol) and put it into the reaction system, add 1300ml toluene, 650mL anhydrous ethanol, 650mL pure water, add Pd(PPh3)4 (10mmol) under nitrogen protection, add L BⅤ -793 (600mmol), after addition, reflux at 100℃ for 20h under nitrogen protection, then cool to 25℃, after cooling, extract with ethyl acetate, wash three times with saturated brine, dry with anhydrous magnesium sulfate, concentrate under reduced pressure, and perform column chromatography (200-300 mesh, 1000g) of the crude product with a developing agent of EA:PE=1:12 to remove impurities, vortex the receiving solution until no liquid flows out, and dry under vacuum to obtain the intermediate L shown in the figure BⅣ -793 (116.27 g, yield 48%), with HPLC purity greater than 99.5%.
[0252] Mass spectrometry test value: 483.44.
[0253]
[0254] Under nitrogen protection system, weigh the intermediate compound L BⅣ -793 (200 mmol), 2-nitrobenzeneboronic acid (CAS: 5570-19-4) (220 mmol), anhydrous potassium carbonate (600 mmol) were placed in the reaction system, 1400 ml toluene, 700 mL anhydrous ethanol, 700 mL pure water were added, Pd (PPh3) 4 (4 mmol) was added under nitrogen protection, and refluxed at 100 ° C for 21 hours under nitrogen protection. Then cooled to 25 ° C, after the reaction was cooled, extracted with ethyl acetate, washed three times with saturated brine, dried over anhydrous magnesium sulfate, concentrated under reduced pressure, and the crude product was column chromatographed (200-300 mesh, 550 g) with a developing agent of EA: PE = 1: 13 to remove impurities, and the receiving liquid was vortexed until no liquid flowed out, and vacuum dried to obtain the intermediate L of the compound shown. BⅢ -793 (92.69 g, yield 88%) with HPLC purity greater than 99.5%.
[0255] Mass spectrometry test value: 526.40.
[0256]
[0257] Under nitrogen protection system, weigh the intermediate compound L BⅢ-793 (170 mmol), triethyl phosphite [P(OEt)3] (340 mL) were placed in the reaction system, 1,2-dichlorobenzene (1,2-DCB) (700 mL) was added, and the reaction was refluxed for 15 h under nitrogen protection. After 15 hours, the solvent was distilled, and the solid was dissolved in dichloromethane and separated by silica gel column chromatography to obtain compound intermediate L BⅡ -793 (51.29 g, 61% yield) with HPLC purity greater than 99.5%.
[0258] Mass spectrometry test value: 494.38.
[0259]
[0260] Under nitrogen protection system, weigh compound L BⅡ -793 (82.5 mmol), bromobenzene (CAS: 108-86-1) (75 mmol), Cu powder (37.5 mmol), K2CO3 (150 mmol) were placed in the reaction system, 1,2-DCB (900 mL) was added, and the reaction was refluxed for 24 h under nitrogen protection. After 24 hours, the solvent was distilled, and the obtained solid was dissolved in dichloromethane, and separated by silica gel column chromatography to obtain compound L BⅠ -793 (28.25 g, yield 66%), with HPLC purity greater than 99.5%.
[0261] Mass spectrometry test value: 570.42.
[0262]
[0263] Under nitrogen protection system, add intermediate L BⅠ -793 (45mmol), DMSO-d6 (1800mmol), NaOH (49.5mmol), N2 replacement three times and N2 protection, heating at 100℃ for 20h. After the reaction is completed, ethyl acetate is extracted, saturated brine is washed three times, and concentrated under reduced pressure. The crude product is purified by column chromatography with a gradient elution of PE:EA=15:1 to 5:1 (v / v) to obtain intermediate L B -793 (18.65 g, yield 72%), with HPLC purity greater than 99.5%.
[0264] Mass spectrometry test value: 575.48.
[0265]
[0266] Under nitrogen protection system, compound trimethyl bipyridine (CAS: 2218457-00-0) (70mmol), DMSO-d6 (1890mmol), NaOH (77mmol) were added in sequence, N2 was replaced three times and N2 was protected, and the reaction was heated at 100°C for 18h. After the reaction was completed, ethyl acetate was extracted, saturated brine was washed three times, and the reaction was concentrated under reduced pressure. The crude product was purified by column chromatography with a gradient elution of PE:EA = 15:1 to 5:1 (v / v) to obtain intermediate L A -793 (18.19 g, yield 92%) with HPLC purity greater than 99.5%.
[0267] The mass spectrometry test value was 282.43.
[0268]
[0269] Under nitrogen protection system, weigh the ligand L A -793 (55mmol), IrC13·3H20 (22mmol) were placed in the reaction system, and a mixed solution of 380ml of ethylene glycol ethyl ether and 127ml of pure water was added. The mixture was refluxed for 28 hours under nitrogen protection, and then cooled to room temperature. A precipitate was precipitated, and the precipitate was filtered, washed with water, anhydrous ethanol, and petroleum ether in turn, and dried. The bridged ligand III-793 (10.61g, yield 61%) was obtained.
[0270]
[0271] Weigh the intermediate formula III-793 (5mmol), add silver trifluoromethanesulfonate (11mmol), then add 490ml of dichloromethane and 163ml of methanol to the system, reflux for 31 hours under nitrogen protection, cool to room temperature, and concentrate the filtrate by column chromatography (short column) until solid precipitates. The iridium complex intermediate formula II-793 (9.08g, yield 94%) is obtained.
[0272]
[0273] Weigh the intermediate II-793 (9 mmol) and add the ligand L B -793 (27 mmol), then add 300 ml of anhydrous ethanol to the system, reflux for 48 hours under nitrogen protection, filter, wash with alcohol, and dry. Use dichloromethane as solvent, use silica gel column chromatography, concentrate the filtrate and precipitate solid to obtain the final compound shown in formula I-793 (3.83 g, yield 32%), and its HPLC purity is greater than 99%.
[0274] The organometallic compound I-793 was subjected to the following analytical tests:
[0275] HPLC purity: greater than 99.5%;
[0276] The mass spectrometry test value was 1329.96.
[0277] Elemental analysis: Calculated values are C, 73.16; H, 6.97; N, 4.21; O, 1.20. Found values are C, 73.18; H, 6.95; N, 4.20; O, 1.21.
[0278] 1H NMR (400 MHz, deuterated chloroform) δ9.16 (d, 1H), 8.29 (d, 3H), 7.95 (dd, 1H), 7.77 (d, 1H), 7.57 (d, 4H), 7.53 (d, 1H), 7.52–7.48 (m, 6H), 7.46–7.15 (m, 20H), 1.07 (s, 9H).
[0279] The synthesis methods of other compounds are the same as above, and will not be described one by one here. The mass spectra or molecular formulas of other synthesis examples are shown in Table 1 below:
[0280] Table 1
[0281] Compound Molecular formula Mass spectrometry test value Yield Formula Ⅰ-1 <![CDATA[C 53 H 37 IrN4O]]> 938.51 25% Formula I-21 <![CDATA[C 59 H 31 D 18 IrN4O]]> 1040.59 19% Formula I-293 <![CDATA[C 60 H 53 GeIrN4O]]> 1112.42 21% Formula I-400 <![CDATA[C 93 H 77 IrN4O]]> 1458.84 31% Formula I-452 <![CDATA[C 64 H 55 D8Ge2IrN4O]]> 1252.48 28% Formula I-574 <![CDATA[C 64 H 42 IrN5O]]> 1089.55 18% Formula I-657 <![CDATA[C 65 H 45 D8IrN4O]]> 1106.56 21% Formula I-747 <![CDATA[C 63 H 30 D 27 IrN4O]]> 1105.78 25% Formula I-825 <![CDATA[C 71 H 33 D 24 IrN4O]]> 1198.83 34% Formula I-844 <![CDATA[C 81 H 34 D 27 IrN4O]]> 1325.91 30%
[0282] Example 1
[0283] The organic electroluminescent device is prepared using the organic phosphorus luminescent material of formula Ⅰ-1, which is more specifically:
[0284] As the anode, the ITO patterned glass substrate was cut into a size of 50 mm × 50 mm × 0.5 mm, ultrasonically treated with isopropyl alcohol and deionized water for 5 minutes each, and then cleaned by exposure to ultraviolet light and ozone for 30 minutes. The resulting glass substrate was loaded onto a vacuum deposition device. First, the ITO (anode) was evaporated with a thickness of The hole injection layer of HI-1 is then deposited on the hole injection layer with a thickness of The hole transport layer of HT-4 was then evaporated to a thickness of The light-emitting layer is composed of a main material 4,4'-N,N'-biphenyldicarbazole ("CBP") and a dopant compound of formula I-1 (90:10 weight ratio), and then a layer with a thickness of The electron transport layer of ET-4 is then evaporated to a thickness of Finally, a LiQ electron injection layer with a thickness of The cathode material Al is added to obtain an organic electroluminescent device. The performance and luminescence characteristics of the obtained device are tested by using a KEITHLEY 2400 source measurement unit and a CS-2000 spectroradiometer to evaluate the driving voltage, lifespan, and luminous efficiency.
[0285] Comparative Example 1
[0286] An organic electroluminescent device was prepared in the same manner as in Example 1, and the structure of the green light-emitting doping compound in the luminescent layer was as follows:
[0287]
[0288] The prepared organic electroluminescent device was tested in the same manner as in Example 1. The results are shown in Table 2.
[0289] Comparative Example 2
[0290] An organic electroluminescent device was prepared in the same manner as in Example 1, and the structure of the green light-emitting doping compound in the luminescent layer was as follows:
[0291]
[0292] The prepared organic electroluminescent device was tested in the same manner as in Example 1. The results are shown in Table 2.
[0293] Comparative Example 3
[0294] An organic electroluminescent device was prepared in the same manner as in Example 1, and the structure of the green light-emitting doping compound in the luminescent layer was as follows:
[0295]
[0296] The prepared organic electroluminescent device was tested in the same manner as in Example 1. The results are shown in Table 2.
[0297] Comparative Example 4
[0298] An organic electroluminescent device was prepared in the same manner as in Example 1, and the structure of the green light-emitting doping compound in the luminescent layer was as follows:
[0299]
[0300] Comparative Example 5
[0301] An organic electroluminescent device was prepared in the same manner as in Example 1, and the structure of the green light-emitting doping compound in the luminescent layer was as follows:
[0302]
[0303] Comparative Example 6
[0304] An organic electroluminescent device was prepared in the same manner as in Example 1, and the structure of the green light-emitting doping compound in the luminescent layer was as follows:
[0305]
[0306] The prepared organic electroluminescent device was tested in the same manner as in Example 1. The results are shown in Table 2.
[0307] Example 2
[0308] The method of the above-mentioned embodiment 1 is referred to, with the only difference being that the doping material I-1 is replaced by I-21.
[0309] Example 3
[0310] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-151.
[0311] Example 4
[0312] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material Ⅰ-1 is replaced by Ⅰ-293.
[0313] Example 5
[0314] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-387.
[0315] Example 6
[0316] The method of the above-mentioned embodiment 1 is referred to, the only difference being that the doping material I-1 is replaced by I-400.
[0317] Example 7
[0318] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-452.
[0319] Example 8
[0320] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-527.
[0321] Example 9
[0322] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-574.
[0323] Example 10
[0324] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-638.
[0325] Embodiment 11
[0326] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-657.
[0327] Example 12
[0328] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-747.
[0329] Embodiment 13
[0330] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-793.
[0331] Embodiment 14
[0332] The method of the above-mentioned embodiment 1 is referred to, with the only difference being that the doping material Ⅰ-1 is replaced by Ⅰ-825.
[0333] Embodiment 15
[0334] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-844.
[0335] The driving voltage, luminous efficiency and life of the organic electroluminescent devices obtained in the above device embodiments and device comparative examples were characterized at a brightness of 8000 (nits). The test results are shown in Table 2 below:
[0336] Table 2
[0337]
[0338] By comparing the comparative examples 1-5 with the organometallic compound of the present invention, it can be seen that L B The ligand introduces a carbazole group on dibenzofuran and adds some electron-withdrawing groups, so that the molecular spatial configuration of the compound of the present invention is changed compared with the comparative example compound, and the electrochemical properties of the compound are adjusted, so that the compound of the present invention is used as a doping material for the light-emitting layer. Compared with the organic electroluminescent device prepared in the comparative example, the driving voltage of the prepared organic electroluminescent device is significantly reduced, and the luminous efficiency and life are significantly improved.
[0339] By comparing the comparative examples 1-5 with the organometallic compound of the present invention, it can be seen that by adjusting different L AThe structure of the ligand, adding some electrons and groups, etc., changing the molecular spatial structure, changing the intermolecular force, so that the organic electroluminescent device prepared by the compound of the present invention as the doping material of the light-emitting layer has a significantly lower driving voltage, and the luminous efficiency and life are significantly improved compared with the organic electroluminescent device prepared in the comparative example, and these numbers are all beyond any value attributable to experimental errors.
[0340] The applicant declares that the present invention uses the above embodiments to illustrate the organic electroluminescent material and the organic electroluminescent device of the present invention, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. An organic electroluminescent material, characterized in that: The organic electroluminescent material has the following structure: Ir(L A )2(L B ); Where L A Ligand and L B The ligands are: in, The R1-R 24 Independently selected from -H, -D (deuterium), -T (tritium), -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -SiMe3, -GeMe3, substituted or unsubstituted C2-C18 alkyl, substituted or unsubstituted C3-C18 cycloalkyl, substituted or unsubstituted C6-C18 aryl and substituted or unsubstituted 4-18 membered heterocyclyl; The substituents on the aforementioned substituent groups are at least selected from one or a combination of at least two of -H, -D, -T, -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -SiMe3, -GeMe3; The heteroatom in the aforementioned heterocyclic group is one or a combination of at least two of N, O, and S; R1-R8 cannot form a ring structure with other substituents on the ring; R9-R 24 They exist independently of each other or form a ring with adjacent groups; R9-R 24 When forming a ring with an adjacent group, the ring is a substituted or unsubstituted C3-C20 aliphatic ring, a substituted or unsubstituted C6-C20 aromatic ring, a substituted or unsubstituted C4-C20 aromatic heterocyclic ring, or a substituted or unsubstituted C10-C20 condensed ring; R1-R 24 The hydrogen in is either undeuterated or deuterated.
2. The organic electroluminescent material according to claim 1, characterized in that: The organic electroluminescent material has a structure as shown in the following formula I:
3. The organic electroluminescent material according to claim 1 or 2, characterized in that: The amount of deuterated hydrogen in the organic electroluminescent material is ≤100%.
4. The organic electroluminescent material according to claim 3, characterized in that: The amount of deuterated hydrogen in the organic electroluminescent material is 0%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 95%, 99% or 100%.
5. The organic electroluminescent material according to any one of claims 1 to 4, characterized in that: R1-R 24 Selected from the following groups: -H, -D, -T, -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -SiMe3, -GeMe3, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, tetrahydrofuran, pyrrolidine, thiolane, tetrahydropyran, phenyl, biphenyl, terphenyl, naphthyl, fluorenyl, phenanthrenyl, anthracenyl, indenyl, triphenylene, pyrenyl, tetraphenylene, perylene, chrysene, fused tetraphenylene, fluoranthenyl, furanyl, thienyl, pyrrolyl, imidazolyl, pyrazolyl, thiazolyl, thiadiazolyl, isothiazolyl, isoxazolyl, oxazolyl, oxadiazolyl, triazinyl, tetrazinyl, triazolyl, tetrazolyl, furazolyl, pyridinyl, pyrazinyl, pyrimidinyl, pyridazinyl, benzofuranyl, benzothiophenyl, isobenzofuranyl, dibenzofuranyl, dibenzothiophenyl, benzimidazolyl, benzothiazolyl, benzisothiazolyl, benzisoxazolyl, benzoxazolyl, isoindolyl, indolyl, indazolyl, benzothiadiazolyl, quinolyl, isoquinolyl, cinnolinyl, quinazolinyl, quinoxalinyl, carbazolyl, phenoxazinyl, phenanthridinyl or benzodioxolyl.
6. The organic electroluminescent material according to any one of claims 1 to 5, characterized in that: R9-R 24 When forming a ring with an adjacent group, the formed ring is a benzene ring, a naphthalene ring or a furan ring.
7. The organic electroluminescent material according to any one of claims 1 to 6, characterized in that: The organic light-emitting material is any one of the following compounds:
8. An organic electroluminescent device, characterized in that: The organic electroluminescent device comprises a first electrode, a second electrode and an organic thin film layer arranged between the first electrode and the second electrode, the organic thin film layer comprises a light-emitting layer, the light-emitting layer comprises a main material and a doping material, and the doping material comprises the organic electroluminescent material as described in any one of claims 1-7.
9. The organic electroluminescent device according to claim 8, characterized in that: The organic thin film layer further includes a hole transport region and an electron transport region.
10. The organic electroluminescent device according to claim 9, characterized in that: The hole transport region includes at least one of a hole injection layer, a first hole transport layer, a second hole transport layer or an electron blocking layer; The electron transport region includes at least one of an electron buffer layer, a hole blocking layer, an electron transport layer, and an electron injection layer.
Citation Information
Cited By
Organic electroluminescent doping material and organic electroluminescent device
CN120441623A
Organometallic compound, organic light emitting diode and organic light emitting device including the same
JP2025093286A
Organometallic compounds, organic light-emitting diodes containing the same, and organic light-emitting devices.
JP7844566B2