Preparation method of fluorine-containing polymer
By using a combination of fluorinated nanocarbon tubes and boron trifluoride complexes in the preparation process of fluoropolymers, the problem of high impurity content is solved, and the effect of reducing impurities and improving performance is achieved, especially in the performance of electrolytes Improvements in aspects.
Patent Information
- Application Number
- CN202411441201.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There is a high impurity content during the preparation of fluoropolymers, which leads to the inability to effectively resolve crystallization, affecting its performance and application.
Mixed the microemulsion of fluorinated nanocarbon tubes and fluoroether oil in the reaction vessel, and obtain polymer particles less than 50μm by filtration and liquid phase medium crushing method, and add boron trifluoride complex and fluorine-containing monomer. In the reactor, an emulsion polymerization reaction was carried out, and the emulsion polymerization was carried out using a gas-phase comonomer and an initiator to prepare a fluorine-containing polymer.
Effectively reduces the impurity content, improves the stability of the polymer and reduces the tendency of crystallization, and improves its performance. In particular, the combination of fluorinated nanocarbon tubes and boron trifluoride complexes is promoted, which promotes the dissolution of lithium salts and Electrolyte properties.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer compound synthesis, and in particular to a method for preparing a fluorine-containing polymer. Background Art
[0002] Fluoropolymers have excellent mechanical strength, impact resistance, radiation resistance, chemical resistance and weather resistance, and are widely used in many industrial fields. Representative products of fluoropolymers such as polyethylene-chlorotrifluoroethylene (ECTFE) are thermoplastic fluorinated copolymers. Compared with other thermoplastics, they have excellent resistance to chlorine and chlorine derivatives at high temperatures; good toughness, high hardness, excellent impact resistance; excellent electrical properties; and extremely low permeability to water vapor and other gases. As a result, polyethylene-chlorotrifluoroethylene is widely used in the fields of electronic and electrical industry, pharmaceutical industry, chemical equipment corrosion protection, solar energy encapsulation film materials, etc. Emulsion polymerization is one of the important processes for the preparation of fluoropolymers. Polymers such as polytetrafluoroethylene, polyvinylidene fluoride, polyperfluoroethylene propylene, tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer and ethylene-chlorotrifluoroethylene copolymer can all be prepared by emulsion polymerization. The emulsion formed by emulsion polymerization must be condensed, washed and dried before it can be further processed. The coagulation process is a demulsification process. There are two main methods of demulsification: physical demulsification and chemical demulsification. Physical demulsification methods include freezing and stirring, while chemical demulsification methods include salting out.
[0003] Chenguang Chemical Research Institute in China has released a method for preparing surfactants containing ether segments by oxidizing fluorinated olefins with oxygen. As a substitute for PFOA, it is used in the preparation method of fluorinated polymer emulsions. It does not affect the polymerization process and has good results. However, the fluorinated polymer preparation process has a high impurity content and crystallization cannot be effectively solved. A preparation method for fluorinated polymers is needed to solve this problem. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a fluorine-containing polymer to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical scheme: a method for preparing a fluorine-containing polymer, comprising the following steps: S1, first preparing a reaction container, and dispersing fluorinated carbon nanotubes in fluorinated ether oil, then adding water and a surfactant into the reaction container to mix the fluorinated carbon nanotubes and the fluorinated ether oil thoroughly and evenly to obtain a microemulsion; S2, placing the condensed microemulsion into a filter press system for filter pressing to obtain a filter cake, and using a gas phase medium crushing method to pre-crush the filter cake to obtain polymer particles with a maximum particle size of less than 180 mm; S 3. Use a liquid medium crushing method to crush the polymer particles into particles with a maximum particle size of less than 50 μm, and disperse the obtained polymer particles in water to obtain an aqueous dispersion; S4. Then add the aqueous dispersion obtained in step S3 into a reactor containing water, a boron trifluoride complex and a fluorine-containing monomer, and adjust the temperature and pressure of the reactor; S5. Continuously add a gaseous comonomer to the reactor to maintain the pressure fluctuation within a small range, and carry out an emulsion polymerization reaction under the action of an initiator to prepare a fluorinated polymer of fluorinated carbon nanotubes.
[0006] As a preferred technical solution of the present invention, the fluorine-containing polymer surfactant is one of anionic fluorocarbon surfactant, cationic fluorocarbon surfactant and zwitterionic fluorocarbon surfactant.
[0007] As a preferred technical solution of the present invention, the temperature of the reactor mentioned in step S4 is increased to 60-100° C., and the pressure is increased to 1.5-4.0 MPa.
[0008] As a preferred technical solution of the present invention, the fluorine-containing monomer is one of 1H-methacrylate or 1H-perfluorooctyl methacrylate.
[0009] As a preferred technical solution of the present invention, the crosslinking agent is methacryloxypropyl cage-type silsesquioxane.
[0010] As a preferred technical solution of the present invention, the initiator mentioned in step S4 refers to a mixture of one or more of acyl peroxides, ketone peroxides, organic tin salts, persulfates, and azo compounds.
[0011] Compared with the prior art, the present invention has the following beneficial effects:
[0012] (1) The present invention is a method for preparing a fluorine-containing polymer. In the method for preparing a fluorine-containing polymer provided by the present invention, a boron trifluoride complex is added as a dissolution promoter to promote the dissolution of a lithium salt additive. The boron trifluoride complex can selectively promote the dissolution of the lithium salt additive, reduce the turbidity of the electrolyte, and help to improve the low-temperature discharge performance and room-temperature cycle performance of the electrolyte.
[0013] (2) The present invention is a method for preparing a fluorine-containing polymer. The method for preparing a fluorine-containing polymer provided by the present invention can effectively reduce the impurity content in the fluorine-containing polymer by treating the fluorine-containing polymer with high crystallinity, thereby improving its stability and reducing the crystallization tendency. In addition, the purity of the epoxy resin is reduced by adding fluorinated nanocarbon tubes, thereby reducing the possibility of crystallization. DETAILED DESCRIPTION
[0014] A method for preparing a fluorine-containing polymer according to an embodiment of the present invention comprises the following steps:
[0015] S1, first prepare a reaction container, and disperse the fluorinated carbon nanotubes in fluorinated ether oil, then add water and a surfactant into the reaction container to mix the fluorinated carbon nanotubes and the fluorinated ether oil thoroughly and evenly to obtain a microemulsion;
[0016] S2, the condensed microemulsion is put into the filter press system for filter pressing to obtain a filter cake, and the filter cake is pre-crushed by a gas phase medium crushing method to obtain polymer particles with a maximum particle size of less than 180 mm;
[0017] S3, crushing the polymer particles into particles with a maximum particle size of less than 50 μm by a liquid medium crushing method, dispersing the obtained polymer particles in water to obtain an aqueous dispersion;
[0018] S4, then adding the aqueous dispersion obtained in step S3 into a reaction kettle containing water, a boron trifluoride complex and a fluorine-containing monomer, and adjusting the temperature and pressure of the reaction kettle;
[0019] S5, continuously adding gas phase comonomer into the reaction kettle to maintain the pressure fluctuation within a small range, and carrying out emulsion polymerization under the action of the initiator to prepare a fluorinated polymer of fluorinated carbon nanotubes;
[0020] In this embodiment, the fluorine-containing polymer surfactant is one of anionic fluorocarbon surfactant, cationic fluorocarbon surfactant and zwitterionic fluorocarbon surfactant, the temperature of the reactor mentioned in step S4 is increased to 60-100°C, the pressure is increased to 1.5-4.0MPa, the fluorine-containing monomer is one of 1H or 1H-perfluorooctyl methacrylate, the cross-linking agent is methacryloyloxypropyl cage-type silsesquioxane, and the initiator mentioned in step S4 refers to a mixture of one or more of acyl peroxides, ketone peroxides, organic tin salts, persulfates, and azo compounds.
[0021] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a fluorine-containing polymer, characterized in that: The following steps are involved: S1. First, prepare a reaction container, and disperse the fluorinated carbon nanotubes in fluoroether oil, then add water and surfactant into the reaction container to mix the fluorinated carbon nanotubes and fluoroether oil thoroughly and evenly to obtain a microemulsion; S2. Put the condensed microemulsion into a filter press system for filter pressing to obtain a filter cake, and use a gas phase medium crushing method to pre-crush the filter cake to obtain polymer particles with a maximum particle size of less than 180 mm; S3. Use a liquid phase medium crushing method to crush the polymer particles into particles with a maximum particle size of less than 50 μm, and disperse the obtained polymer particles in water to obtain an aqueous dispersion; S4, then adding the aqueous dispersion obtained in step S3 into a reactor containing water, a boron trifluoride complex and a fluorine-containing monomer, and adjusting the temperature and pressure of the reactor; S5, continuously adding a gas phase copolymer monomer into the reactor to maintain the pressure fluctuation within a small range, and carrying out an emulsion polymerization reaction under the action of an initiator to prepare a fluorinated carbon nanotube containing polymer.
2. The method for preparing a fluorine-containing polymer according to claim 1, characterized in that: The fluorine-containing polymer surfactant is one of anionic fluorocarbon surfactant, cationic fluorocarbon surfactant and zwitterionic fluorocarbon surfactant.
3. The method for preparing a fluorine-containing polymer according to claim 1, characterized in that: The temperature of the reactor mentioned in step S4 is raised to 60-100° C., and the pressure is raised to 1.5-4.0 MPa.
4. The method for preparing a fluorine-containing polymer according to claim 1, characterized in that: The fluorine-containing monomer is one of 1H-methacrylate or 1H-perfluorooctyl methacrylate.
5. The method for preparing a fluorine-containing polymer according to claim 1, characterized in that: The crosslinking agent is methacryloxypropyl cage-type silsesquioxane.
6. The method for preparing a fluorine-containing polymer according to claim 1, characterized in that: The initiator mentioned in step S4 refers to one or more mixtures of acyl peroxides, ketone peroxides, organic tin salts, persulfates, and azo compounds.
Citation Information
Patent Citations
Method for reducing impurity content in fluorine-containing polymer
CN101624432A
Composite ultraviolet-curing coating containing vinyl-terminated fluorinated alkyl ester polymer, its preparation and application
CN102898932A
Method for improving solubility of lithium salt additive and electrolyte containing lithium salt additive
CN115133125A
Synthetic method of fluorine-containing polymer, fluorine-containing rubber and preparation method of fluorine-containing rubber
CN115716895A