Etching hollow molecularly imprinted polymer as well as preparation method and application thereof
By preparing the etched hollow molecular imprinted polymer, the reaction of titanate nanotube carrier with tetracycline and other components is solved, and the problem of insufficient adsorption of tetracycline in the prior art is achieved, and efficient and economical pollution control and detection effects are achieved.
Patent Information
- Application Number
- CN202411024127.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The existing molecular blotting technology used for the removal of tetracycline has the problem of limited adsorption amount, making it difficult to effectively deal with tetracycline contamination, and the treatment process is complex, time-consuming and poor selectivity.
Titanate nanotubes are used as carriers, and react with components such as tetracycline, lysozyme and tris(2-carboxyethyl)phosphine hydrochloride after etching treatment to prepare etched hollow molecular imprinted polymers to increase their specific surface area and pore volume to improve adsorption capacity.
It significantly improves the adsorption amount and selectivity of tetracycline, achieves efficient and economical removal effect, and is suitable for the pollution control and selective detection and separation of tetracycline.
Smart Images

Figure CN118955993A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano material preparation and environmental chemical application, and in particular to an etched hollow molecular imprinted polymer, a preparation method and application thereof. Background Art
[0002] Tetracyclines (TCs) are antibacterial substances isolated from the culture fluid of the actinomycete Streptomyces aureofa-ciens. They have a good inhibitory effect on Gram-positive bacteria, Gram-negative bacteria, Rickettsia, filterable viruses, spirochetes and even protozoa, and are a broad-spectrum antibiotic. Preparations obtained by chemically modifying natural tetracyclines (such as pyrimethocycline) and semi-synthetic tetracycline derivatives (such as methadone) have been used in medical practice. At present, there are about 40 natural tetracyclines and more than 3,000 synthetic tetracyclines. Tetracycline (TC) is a yellow crystalline substance that is easily soluble in acid, alkali, methanol, ethylene glycol and pyridine, and slightly soluble in water, chloroform, ethyl acetate and dichloromethane. As a broad-spectrum antibiotic, tetracycline is active against Gram-negative bacteria, Gram-positive bacteria, spirochetes, leptospires, large viruses, protozoa, etc. For a long time, there has been a large-scale abuse of tetracyclines in veterinary medicine for animal and human treatment, which has increased the possibility of such compounds polluting the environment. Tetracyclines may increase bacterial resistance. Therefore, the residues of tetracyclines in the aquatic environment have caused great concern. However, so far, sewage treatment plants have not been able to effectively treat tetracyclines.
[0003] At present, the main sample pretreatment methods for tetracycline include solid-liquid extraction, liquid-liquid extraction, solid phase extraction, etc. However, these methods often have the disadvantages of complex processing, long time consumption, slow analysis speed, poor selectivity, etc. Molecular imprinting technology was first proposed by Wulff in 1972, and has now become a technology that has attracted much attention from researchers. It is used to construct molecularly imprinted polymers (Molecularly Imprinted Polymers, MIP2410496CCDs) with specific sites that are completely complementary to the template molecules in size, shape and chemical function. MIP2410496CCDs can be combined with template molecules through functional monomers with special functional groups, and adjust and form specific spatial conformations according to the needs of the template molecules. Due to the advantages of high selectivity, unique physicochemical stability, simple preparation process and reusability, MIP2410496CCDs has been widely used in chromatography, biosensors, drug delivery, solid phase extraction and other fields.
[0004] However, the existing molecular imprinting technology for the removal of tetracycline still has the problem of limited adsorption capacity, which needs to be solved urgently. Summary of the invention
[0005] In view of the above problems existing in the prior art, the present invention provides an etched hollow molecular imprinted polymer, a preparation method and an application thereof, and proposes the use of titanate nanotubes as carriers to prepare hollow molecular imprinted polymers with high tetracycline adsorption capacity, thereby providing an efficient and economical solution for the molecular imprinting technology to control tetracycline pollution problems, as well as the selective detection and separation of tetracycline in complex matrices.
[0006] The specific content of the invention is as follows:
[0007] In a first aspect, the present invention provides a method for preparing an etched hollow molecularly imprinted polymer, the method comprising:
[0008] Step 1, mixing the hollow titanate nanotubes with a mass volume ratio of 10-20 mg: 5-10 mL with HCl solution, shaking for 0.5-1 h, and filtering to obtain etched hollow titanate nanotubes;
[0009] Step 2, after mixing etched titanate nanotubes, tetracycline, lysozyme, tris(2-carboxyethyl)phosphine hydrochloride and buffer solution in a dosage ratio of 10-50 mg:10-30 mg:10-100 mg:11.4-114 mg:5-30 mL, reacting under stirring conditions for 2-12 hours, and then standing and precipitating for 2-12 hours, washing and vacuum drying the precipitated solid to obtain the etched hollow molecular imprinted polymer precursor;
[0010] Step 3: performing an elution treatment on the etched hollow molecularly imprinted polymer precursor, and then vacuum drying to obtain the etched hollow molecularly imprinted polymer.
[0011] Optionally, in step 2, the stirring conditions include: the stirring method is magnetic stirring, and the stirring speed is 200 to 800 r / min.
[0012] Optionally, in step 2 and step 3, the vacuum drying treatment includes: the vacuum drying temperature is 80-100° C., the pressure is 0.01-0.1 MPa, and the time is 2-5 h.
[0013] Optionally, in step 2, the buffer solution is PBS buffer.
[0014] Optionally, in step 3, the elution treatment includes: using a mixed solution of ethanol and acetic acid in a volume ratio of 92:8 for elution treatment.
[0015] Optionally, the hollow titanate nanotube is obtained by the following preparation method:
[0016] Titanium dioxide, water and sodium hydroxide are mixed according to (1.2-9.6) g: (70-560) mL: (28-224) g, stirred evenly, and then transferred to 40-160° C. for reaction for 60-1380 min. After the reaction is completed, the reaction product is washed until the pH is neutral and vacuum dried for 6-12 h to obtain.
[0017] Optionally, the diameter of the hollow titanate nanotube is no greater than 10 nm, and the length is no greater than 100 nm.
[0018] Optionally, the stirring conditions include: the stirring method is magnetic stirring, the stirring speed is 500-1000 r / min, and the stirring time is 2-8 h.
[0019] In a second aspect, the present invention provides an etched hollow molecular imprinted polymer obtained by the preparation method described in the first aspect.
[0020] In a third aspect, the present invention provides an application of an etched hollow molecular imprinted polymer obtained by the preparation method described in the first aspect, characterized in that the etched hollow molecular imprinted polymer is used for tetracycline pollution control and selective detection and separation of tetracycline in complex matrices.
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] The invention provides a method for preparing an etched hollow molecular imprinted polymer, comprising: mixing a hollow titanate nanotube with an HCl solution, and performing HCl etching to obtain an etched titanate nanotube; mixing the etched titanate nanotube with tetracycline, lysozyme, tris(2-carboxyethyl)phosphine hydrochloride and a buffer solution, and performing polymerization reaction to obtain an etched hollow molecular imprinted polymer precursor; performing elution treatment on the etched hollow molecular imprinted polymer precursor to remove a template molecule (tetracycline) therein, and then vacuum drying to obtain the etched hollow molecular imprinted polymer.
[0023] In the preparation method provided by the present invention, the hollow titanate nanotubes have efficient mass transfer capability. After adjusting the etching conditions, the wall thickness of the pipe is reduced and the pipe diameter is increased after etching, but the morphology of the carbonate nanotubes remains intact, the material weight is reduced, and the surface area of the pipe is increased. This allows the etching of the titanate nanotubes as carriers, and the lysozyme imprinting layer is combined on the surface to form an etched hollow molecular imprinted polymer with increased specific surface area and pore volume, greatly increased imprinting sites, enhanced selective adsorption capacity, and increased adsorption amount, thereby increasing the adsorption amount of TC per unit mass of the titanate nanotube-based molecular imprinted polymer, and greatly improving its practical application ability for TC removal in various fields.
[0024] In addition, the functional monomer lysozyme used in the present invention has multiple functional groups, which can generate multiple interaction forces with the template molecule to enhance the imprinting effect, and the disulfide bonds in the lysozyme can be reduced to cause a configuration change, so that a stable and uniform phase-change lysozyme imprinting layer is formed. Therefore, the etched hollow molecular imprinting polymer prepared by the present invention has a high adsorption and enrichment effect on tetracycline.
[0025] The etched hollow molecular imprinted polymer prepared by the method of the present invention has uniform diameter and length, good structural stability, good reusability, strong selective adsorption capacity for tetracycline, large adsorption amount and high recovery rate, and at the same time, the material cost is low and the preparation is simple. It is a method for highly selectively enriching and removing tetracycline in complex environmental samples, and shows broad application prospects in the selective separation, enrichment and detection of tetracycline.
[0026] The etched hollow molecular imprinted polymer prepared by the method of the present invention can directly and selectively adsorb tetracycline in complex samples when used, and the samples do not need any pretreatment, thereby reducing the consumption of organic solvents. The obtained etched hollow molecular imprinted polymer shows high binding capacity, fast adsorption rate, good regeneration ability and excellent selectivity for tetracycline. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 The flowchart of the method for preparing the etched hollow molecular imprinted polymer provided by the embodiment of the present invention is shown;
[0029] Figure 2 A transmission electron microscope image of a titanate nanotube provided by an embodiment of the present invention is shown;
[0030] Figure 3 A transmission electron microscope image of etching titanate nanotubes provided by an embodiment of the present invention is shown;
[0031] Figure 4 The adsorption of tetracycline by the molecular imprinting polymers provided in Example 1 of the present invention and Comparative Example 1 is shown. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means a limitation on the present invention and its application or use. Based on the embodiments of the present invention, any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts falls within the scope of protection of the present invention. In addition, all other embodiments obtained by ordinary technicians in this field without carrying out creative work belong to the scope of protection of the present invention.
[0033] In the embodiment, no specific experimental steps or conditions are indicated, and the operation or conditions of the conventional experimental steps described in the prior art in this field can be carried out. The reagents used and other instruments that do not indicate the manufacturer are conventional reagent products that can be obtained commercially. In addition, the accompanying drawings are only schematic diagrams of the embodiments of the present invention and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and thus their repeated description will be omitted. Some block diagrams shown in the accompanying drawings are functional entities and do not necessarily correspond to physically or logically independent entities.
[0034] Technologies, methods, and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the description of the present invention.
[0035] In the description of the present invention, it should be understood that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.
[0036] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0037] Titanate nanotubes (TNTs) have received particular attention due to their high specific surface area and pore volume as well as good ion exchange properties. Titanate nanotubes as small as 10 nm can be prepared by a hydrothermal method, which has a short synthesis time, high yield, and reusable alkaline solution. However, the adsorption of TC by titanate nanotubes is still limited due to the thickness and mass of the wall, which greatly restricts their practical applications.
[0038] Therefore, it is of great scientific significance to reduce the mass of titanate nanotubes and increase the specific surface area of titanate nanotubes to increase the adsorption amount of TC per unit mass of titanate nanotube-based molecular imprinting polymers, thereby enhancing the practical application ability of this type of material for TC removal in various fields.
[0039] In a first aspect, the present invention provides a method for preparing an etched hollow molecularly imprinted polymer. Figure 1 The flowchart of the method for preparing the etched hollow molecular imprinted polymer provided by the embodiment of the present invention is shown as follows: Figure 1 As shown, the method includes:
[0040] S1. Mixing the hollow titanate nanotubes with a mass volume ratio of 10-20 mg: 5-10 mL with HCl solution, shaking for 0.5-1 h, and filtering to obtain etched hollow titanate nanotubes;
[0041] In the specific implementation of this step, hollow titanate nanotubes are used as the carrier of the lysozyme imprinting layer, which has efficient mass transfer capability. After adjusting the etching conditions (the amount of HCl and titanate nanotubes and the control of etching time), the wall thickness of the pipeline is reduced and the diameter is increased after etching, but the morphology of the carbonate nanotubes remains intact, which reduces the material weight, increases the surface area of the pipeline, and creates more adsorption sites.
[0042] S2, mixing etched hollow titanate nanotubes, tetracycline, lysozyme, tris(2-carboxyethyl)phosphine hydrochloride and buffer solution in an amount ratio of 10-50 mg:10-30 mg:10-100 mg:11.4-114 mg:5-30 mL, reacting under stirring conditions for 2-12 hours, and then standing and precipitating for 2-12 hours, washing and vacuum drying the precipitated solid to obtain the etched hollow molecular imprinting polymer precursor;
[0043] When this step is implemented, in a reaction system consisting of etched hollow titanate nanotubes, tetracycline, lysozyme, tris(2-carboxyethyl)phosphine hydrochloride and a buffer solution (PBS buffer), tetracycline is used as a template molecule, and the etched titanate nanotubes are first combined with tetracycline to form a template-carrier complex, and the template-carrier complex further reacts with lysozyme to coat the surface of the template-carrier complex with a lysozyme imprinting layer; this process is carried out under continuous stirring, and the stirring conditions include: the stirring method is magnetic stirring, and the stirring speed is 200-800r / min; after the reaction is completed, the separated precipitate is washed and vacuum dried to obtain an etched hollow molecular imprinting polymer precursor. Wherein, the vacuum drying treatment includes: the vacuum drying temperature is 80-100°C, the pressure is 0.01-0.1MPa, and the time is 2-5h.
[0044] S3, performing an elution treatment on the etched hollow molecularly imprinted polymer precursor, and then vacuum drying to obtain the etched hollow molecularly imprinted polymer.
[0045] When this step is implemented, the etched hollow molecular imprinting polymer precursor is eluted and then vacuum dried to remove the template molecule (tetracycline) therein, thereby obtaining a molecular imprinting polymer containing a large number of tetracycline binding sites; wherein the elution treatment comprises: elution treatment with a mixed solution of ethanol and acetic acid in a volume ratio of 92:8; and the vacuum drying treatment comprises: vacuum drying at a temperature of 80-100°C, a pressure of 0.01-0.1MPa, and a time of 2-5h.
[0046] In some embodiments, the hollow titanate nanotubes are obtained by the following preparation method:
[0047] Titanium dioxide, water and sodium hydroxide are mixed according to (1.2-9.6) g: (70-560) mL: (28-224) g, stirred evenly, and then transferred to 40-160° C. for reaction for 60-1380 min. After the reaction is completed, the reaction product is washed until the pH is neutral and vacuum dried for 6-12 h to obtain.
[0048] In specific implementation, the present invention regulates the conditions of the hydrothermal synthesis process, and obtains titanate nanotubes with a diameter of no more than 10 nm and a length of no more than 100 nm through one-step hydrothermal. The preparation method has the advantages of short preparation time, high yield, reusable alkaline solution, and efficient mass transfer capacity of the hollow tube.
[0049] In a second aspect, the present invention provides an etched hollow molecular imprinted polymer obtained by the preparation method described in the first aspect.
[0050] The invention provides a method for preparing an etched hollow molecular imprinted polymer. The obtained etched hollow molecular imprinted polymer has uniform diameter and length, good structural stability, good reusability, strong selective adsorption capacity for tetracycline, large adsorption amount, and high recovery rate. Meanwhile, the material cost is low and the preparation is simple. The invention is a method for highly selectively enriching and removing tetracycline in complex environmental samples, and shows broad application prospects in the selective separation, enrichment, detection, etc. of tetracycline.
[0051] In addition, the etched hollow molecular imprinted polymer prepared by the method of the present invention can directly and selectively adsorb tetracycline in complex samples when used, and the samples do not need any pretreatment, thereby reducing the consumption of organic solvents. The obtained etched hollow molecular imprinted polymer shows high binding capacity, fast adsorption rate, good regeneration ability and excellent selectivity for tetracycline.
[0052] In a third aspect, the present invention provides an application of an etched hollow molecular imprinted polymer obtained by the preparation method described in the first aspect, characterized in that the etched hollow molecular imprinted polymer is used for tetracycline pollution control and selective detection and separation of tetracycline in complex matrices.
[0053] In order to enable those skilled in the art to more clearly understand the present invention, the etched hollow molecular imprinted polymer, preparation method and application of the present invention are now described in detail through the following examples.
[0054] Example 1
[0055] (1) Preparation of Etched Hollow Molecularly Imprinted Polymers
[0056] 1.2 g of titanium dioxide, 70 mL of water, and 28 g of sodium hydroxide were mixed evenly, and magnetically stirred at a speed of 500 r / min for 4 h. The mixture was reacted at 160° C. for 1380 min. After the reaction, the reaction product was washed until the pH was neutral, and vacuum dried at 105° C. and 0.02 MPa for 6 h to obtain hollow titanate nanotubes.
[0057] 10 mg of titanate nanotubes were placed in 5 mL of HCl aqueous solution and shaken for 0.5 h, and then filtered to obtain etched hollow titanate nanotubes.
[0058] 25 mg of etched hollow titanate nanotubes, 15 mg of tetracycline, 100 mg of lysozyme, 114 mg of tris(2-carboxyethyl)phosphine hydrochloride and 30 mL of PBS buffer were mixed, and the mixture was stirred under magnetic stirring at room temperature and a rotation speed of 300 r / min for 10 h, and then allowed to settle for 10 h. The reaction product was washed and vacuum dried at 80° C. and 0.02 MPa for 3 h to obtain a molecularly imprinted polymer precursor.
[0059] The separated molecular imprinting polymer precursor was eluted with a mixed solution of ethanol and acetic acid (volume ratio of 92:8), and vacuum dried at 80°C and 0.02MPa for 3h to obtain an etched hollow molecular imprinting polymer.
[0060] Figure 2 The transmission electron microscope image of the hollow titanate nanotube provided by the embodiment of the present invention is shown. Figure 3 The transmission electron microscope image of the etched hollow titanate nanotube provided by the embodiment of the present invention is shown. Figure 2 , 3 As shown, before etching, the diameter of the hollow titanate nanotube is less than 10nm and the length is about 100nm. After etching, the morphology of the titanate nanotube remains intact, but its wall thickness is reduced, the tube diameter is increased, the tube surface is increased, and it has a high specific surface area and pore volume.
[0061] (2) Testing the adsorption performance of etched hollow molecular imprinted polymers
[0062] 10 mg of the etched hollow molecularly imprinted polymer was added to 10 mL of an aqueous solution of tetracycline with a concentration of 800 μg / mL, and after shaking at room temperature for 30 min, the supernatant was separated by applying an external magnetic field;
[0063] The concentration of tetracycline in the obtained supernatant was measured by HPLC, and the concentration of tetracycline in the supernatant was 689 μg / mL; and the adsorption amount of tetracycline by the etched hollow molecular imprinting polymer was calculated;
[0064] The calculation formula for the adsorption amount of tetracycline by the etched hollow molecular imprinted polymer is:
[0065]
[0066] Where C e is the concentration of tetracycline in the above supernatant;
[0067] Through calculation, the adsorption capacity of tetracycline by the etched hollow molecular imprinting polymer is 111 mg / g.
[0068] Example 2
[0069] (1) Preparation of Etched Hollow Molecularly Imprinted Polymers
[0070] 2.4g titanium dioxide, 140mL water, and 56g sodium hydroxide were mixed evenly, magnetically stirred at a speed of 600r / min for 5h, reacted at 140℃ for 1320min, and after the reaction, the reaction product was washed to a neutral pH, and vacuum dried at 90℃ and 0.03MPa for 4h. Hollow titanate nanotubes with a diameter as small as 10nm and a length of 100nm were obtained.
[0071] 12 mg of hollow titanate nanotubes were placed in 6 mL of HCl aqueous solution and shaken for 0.6 h, and then filtered to obtain etched titanate nanotubes.
[0072] 15 mg of hollow etched titanate nanotubes, 10 mg of tetracycline, 80 mg of lysozyme, 91.2 mg of tris(2-carboxyethyl)phosphine hydrochloride and 25 mL of PBS buffer were mixed, and then magnetically stirred at room temperature at a speed of 400 r / min for 8 h, and then allowed to settle for 8 h. The reaction product was washed and vacuum dried at 70°C and 0.03 MPa for 4 h to obtain a molecularly imprinted polymer precursor.
[0073] The separated molecular imprinting polymer precursor was eluted with a mixed solution of ethanol:acetic acid (volume ratio 93:7) and vacuum dried at 70°C and 0.03MPa for 4h to obtain an etched hollow molecular imprinting polymer.
[0074] (2) Testing the adsorption performance of etched hollow molecular imprinted polymers
[0075] 10 mg of the etched hollow molecularly imprinted polymer was added to 10 mL of an aqueous solution of tetracycline with a concentration of 800 μg / mL, and after shaking at room temperature for 30 min, the supernatant was separated by applying an external magnetic field;
[0076] The concentration of tetracycline in the supernatant obtained in (1) was measured by HPLC, and the concentration of tetracycline in the supernatant was 686.5 μg / mL; and the adsorption amount of tetracycline by the etched hollow molecular imprinting polymer was calculated;
[0077] The calculation formula for the adsorption amount of tetracycline by the etched hollow molecular imprinted polymer is:
[0078]
[0079] Where C e is the concentration of tetracycline in the above supernatant;
[0080] Through calculation, the adsorption capacity of tetracycline by the etched hollow molecular imprinting polymer is 113.5 mg / g.
[0081] Example 3
[0082] (1) Preparation of Etched Hollow Molecularly Imprinted Polymers
[0083] 3.6g titanium dioxide, 210mL water, and 84g sodium hydroxide were mixed evenly, stirred magnetically at a speed of 700r / min for 6h, reacted at 120℃ for 1260min, and after the reaction, the reaction product was washed to a neutral pH, and vacuum dried at 80℃ and 0.04MPa for 7h. Hollow titanate nanotubes with a diameter as small as 10nm and a length of 100nm were obtained.
[0084] 17 mg of hollow titanate nanotubes were placed in 7 mL of HCl aqueous solution and shaken for 0.7 h, and then filtered to obtain etched hollow titanate nanotubes.
[0085] 10 mg of etched hollow titanate nanotubes, 10 mg of tetracycline, 70 mg of lysozyme, 79.8 mg of tri(2-carboxyethyl)phosphine hydrochloride and 20 mL of PBS buffer were mixed, and then magnetically stirred at room temperature at a speed of 300 r / min for 9 h, and then allowed to settle for 9 h. The reaction product was washed and vacuum dried at 60° C. and 0.04 MPa for 4 h to obtain a molecularly imprinted polymer.
[0086] The separated molecular imprinted polymer was eluted with a mixed solution of ethanol:acetic acid 94:6 and vacuum dried at 60°C and 0.04MPa for 4h to obtain an etched hollow molecular imprinted polymer.
[0087] (2) Testing the adsorption performance of etched hollow molecular imprinted polymers
[0088] 10 mg of the etched hollow molecularly imprinted polymer was added to 10 mL of an aqueous solution of tetracycline with a concentration of 800 μg / mL, and after shaking at room temperature for 30 min, the supernatant was separated by applying an external magnetic field;
[0089] The concentration of tetracycline in the supernatant obtained in (1) was determined by HPLC; the concentration of tetracycline in the supernatant was 683 μg / mL; and the adsorption amount of tetracycline by the etched hollow molecular imprinting polymer was calculated;
[0090] The calculation formula for the adsorption amount of tetracycline by the etched hollow molecular imprinted polymer is:
[0091]
[0092] Where C e is the concentration of tetracycline in the above supernatant;
[0093] Through calculation, the adsorption capacity of tetracycline by the etched hollow molecular imprinting polymer is 117 mg / g.
[0094] Example 4
[0095] (1) Preparation of Etched Hollow Molecularly Imprinted Polymers
[0096] 4.8g titanium dioxide, 280mL water, and 112g sodium hydroxide were mixed evenly, stirred magnetically at a speed of 800r / min for 5h, reacted at 160°C for 1200min, and after the reaction, the reaction product was washed until the pH was neutral, and vacuum dried at 65°C and 0.05MPa for 8h. Hollow titanate nanotubes with a diameter as small as 10nm and a length of 100nm were obtained.
[0097] 18 mg of hollow titanate nanotubes were placed in 8 mL of HCl aqueous solution and shaken for 0.8 h, and then filtered to obtain etched titanate nanotubes.
[0098] 50 mg of etched hollow titanate nanotubes, 30 mg of tetracycline, 50 mg of lysozyme, 57 mg of tris(2-carboxyethyl)phosphine hydrochloride and 30 mL of PBS buffer were mixed, and then magnetically stirred at room temperature at a speed of 500 r / min for 8 h, and then allowed to settle for 8 h. The reaction product was washed and vacuum dried at 65° C. and 0.05 MPa for 8 h to obtain a molecularly imprinted polymer.
[0099] The separated molecular imprinted polymer was eluted with a mixed solution of ethanol:acetic acid 94:6 and vacuum dried at 65°C and 0.05MPa for 8h to obtain an etched hollow molecular imprinted polymer.
[0100] (2) Testing the adsorption performance of etched hollow molecular imprinted polymers
[0101] 10 mg of the etched hollow molecularly imprinted polymer was added to 10 mL of an aqueous solution of tetracycline with a concentration of 800 μg / mL, and after shaking at room temperature for 30 min, the supernatant was separated by applying an external magnetic field;
[0102] The concentration of tetracycline in the supernatant obtained in (1) was determined by HPLC, and the concentration of tetracycline in the supernatant was 671 μg / mL. The adsorption amount of tetracycline by the etched hollow molecular imprinting polymer was then calculated.
[0103] The calculation formula for the adsorption amount of tetracycline by the etched hollow molecular imprinted polymer is:
[0104]
[0105] Where C e is the concentration of tetracycline in the above supernatant;
[0106] Through calculation, the adsorption capacity of tetracycline by the etched hollow molecular imprinting polymer is 129 mg / g.
[0107] Example 5
[0108] (1) Preparation of Etched Hollow Molecularly Imprinted Polymers
[0109] 6.0g titanium dioxide, 350mL water, and 140g sodium hydroxide were mixed evenly, stirred magnetically at a speed of 900r / min for 2h, and reacted at 80°C for 1380min. After the reaction, the reaction product was washed until the pH was neutral, and vacuum dried at 70°C and 0.06MPa for 8h. Hollow titanate nanotubes with a diameter as small as 10nm and a length of 100nm were obtained. Support carrier
[0110] 19 mg of hollow titanate nanotubes were placed in 9 mL of HCl aqueous solution and shaken for 0.9 h, and then filtered to obtain etched titanate nanotubes.
[0111] 40 mg of etched hollow titanate nanotubes, 30 mg of tetracycline, 40 mg of lysozyme, 45.6 mg of tris(2-carboxyethyl)phosphine hydrochloride and 30 mL of PBS buffer were mixed, and then reacted under magnetic stirring at room temperature and a rotation speed of 600 r / min for 4 h, and then allowed to settle for 8 h. The reaction product was washed and vacuum dried at 70°C and 0.06 MPa for 8 h to obtain a molecularly imprinted polymer.
[0112] The separated molecular imprinted polymer was eluted with a mixed solution of ethanol:acetic acid 95:5 and vacuum dried at 70°C and 0.06MPa for 8h to obtain an etched hollow molecular imprinted polymer.
[0113] (2) Testing the adsorption performance of etched hollow molecular imprinted polymers
[0114] 10 mg of the etched hollow molecularly imprinted polymer was added to 10 mL of an aqueous solution of tetracycline with a concentration of 800 μg / mL, and after shaking at room temperature for 30 min, the supernatant was separated by applying an external magnetic field;
[0115] The concentration of tetracycline in the supernatant obtained in (1) was measured by HPLC, and the concentration of tetracycline in the supernatant was 673 μg / mL. The adsorption amount of tetracycline by the etched hollow molecular imprinting polymer was then calculated;
[0116] The calculation formula for the adsorption amount of tetracycline by the etched hollow molecular imprinted polymer is:
[0117]
[0118] Where C e is the concentration of tetracycline in the above supernatant;
[0119] Through calculation, the adsorption capacity of tetracycline by the etched hollow molecular imprinting polymer is 127 mg / g.
[0120] Example 6
[0121] (1) Preparation of Etched Hollow Molecularly Imprinted Polymers
[0122] 7.2g titanium dioxide, 420mL water, and 168g sodium hydroxide were mixed evenly, magnetically stirred at a speed of 1000r / min for 3h, reacted at 100℃ for 1200min, and after the reaction, the reaction product was washed to a neutral pH, and vacuum dried at 75℃ and 0.06MPa for 8h. Hollow titanate nanotubes with a diameter as small as 10nm and a length of 100nm were obtained.
[0123] 20 mg of hollow titanate nanotubes were placed in 10 mL of HCl aqueous solution and shaken for 1 h, and then filtered to obtain etched hollow titanate nanotubes.
[0124] 25 mg of etched hollow titanate nanotubes, 30 mg of tetracycline, 60 mg of lysozyme, 68.4 mg of tris(2-carboxyethyl)phosphine hydrochloride and 30 mL of PBS buffer were mixed, and then reacted for 2 h at room temperature and at a speed of 700 r / min under magnetic stirring, and then allowed to settle for 2 h. The reaction product was washed and vacuum dried at 75°C and 0.07 MPa for 8 h to obtain a molecularly imprinted polymer.
[0125] The separated molecular imprinted polymer was eluted with a mixed solution of ethanol:acetic acid 96:4 and vacuum dried at 75°C and 0.07MPa for 8h to obtain an etched hollow molecular imprinted polymer.
[0126] (2) Testing the adsorption performance of etched hollow molecular imprinted polymers
[0127] 10 mg of the etched hollow molecularly imprinted polymer was added to 10 mL of an aqueous solution of tetracycline with a concentration of 800 μg / mL, and after shaking at room temperature for 30 min, the supernatant was separated by applying an external magnetic field;
[0128] The concentration of tetracycline in the supernatant obtained in (1) was measured by HPLC, and the concentration of tetracycline in the supernatant was 683 μg / mL; and the adsorption amount of tetracycline by the etched hollow molecular imprinting polymer was calculated;
[0129] The calculation formula for the adsorption amount of tetracycline by the etched hollow molecular imprinted polymer is:
[0130]
[0131] Where C e is the concentration of tetracycline in the above supernatant;
[0132] Through calculation, the adsorption capacity of tetracycline by the etched hollow molecular imprinting polymer is 117 mg / g.
[0133] Comparative Example 1
[0134] (The difference from Example 1 is that no HCl etching treatment is performed)
[0135] (1) Preparation of Etched Hollow Molecularly Imprinted Polymers
[0136] 1.2 g of titanium dioxide, 70 mL of water, and 28 g of sodium hydroxide were mixed evenly, and magnetically stirred at a speed of 500 r / min for 4 h. The mixture was reacted at 160° C. for 1380 min. After the reaction, the reaction product was washed until the pH was neutral, and vacuum dried at 105° C. and 0.02 MPa for 6 h to obtain hollow titanate nanotubes.
[0137] 25 mg of hollow titanate nanotubes, 15 mg of tetracycline, 100 mg of lysozyme, 114 mg of tris(2-carboxyethyl)phosphine hydrochloride and 30 mL of PBS buffer were mixed, and the mixture was reacted under magnetic stirring at room temperature and a rotation speed of 300 r / min for 10 h, and then allowed to settle for 10 h. The reaction product was washed and vacuum dried at 80° C. and 0.02 MPa for 3 h to obtain a molecularly imprinted polymer precursor.
[0138] The separated molecular imprinting polymer precursor was eluted with a mixed solution of ethanol and acetic acid (volume ratio of 92:8), and vacuum dried at 80°C and 0.02MPa for 3h to obtain an etched hollow molecular imprinting polymer.
[0139] (2) Detection of adsorption performance of hollow molecular imprinted polymers
[0140] 10 mg of the hollow molecularly imprinted polymer was added to 10 mL of an aqueous solution of tetracycline at a concentration of 800 μg / mL, and after shaking at room temperature for 30 min, the supernatant was separated by applying an external magnetic field;
[0141] The concentration of tetracycline in the obtained supernatant was measured by HPLC, and the concentration of tetracycline in the supernatant was 689 μg / mL; and the adsorption amount of tetracycline by the hollow molecular imprinting polymer was calculated;
[0142] The calculation formula of the adsorption amount of tetracycline by the hollow molecular imprinted polymer is:
[0143]
[0144] Where C e is the concentration of tetracycline in the above supernatant;
[0145] Through calculation, the adsorption capacity of tetracycline by hollow molecular imprinting polymer is: 68mg / g, Figure 4The adsorption of tetracycline by the molecular imprinting polymer provided in Example 1 of the present invention and Comparative Example 1 is shown. Figure 4 As shown in the figure, compared with the unetched hollow molecular imprinting polymer, the adsorption of tetracycline is very different. The etched hollow molecular imprinting polymer has a larger adsorption amount of tetracycline.
[0146] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification.
[0147] For the method embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the order of the actions described, because according to the present invention, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and components involved are not necessarily required by the present invention.
[0148] The above is a detailed introduction to an etched hollow molecular imprinted polymer, a preparation method and an application thereof provided by the present invention. Specific examples are used herein to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method and core idea of the present invention. At the same time, for a person skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for preparing an etched hollow molecularly imprinted polymer, characterized in that: The method comprises: Step 1, mixing the hollow titanate nanotubes with a mass volume ratio of 10-20 mg: 5-10 mL with HCl solution, shaking for 0.5-1 h, and filtering to obtain etched hollow titanate nanotubes; Step 2, after mixing etched titanate nanotubes, tetracycline, lysozyme, tris(2-carboxyethyl)phosphine hydrochloride and buffer solution in a dosage ratio of 10-50 mg:10-30 mg:10-100 mg:11.4-114 mg:5-30 mL, reacting under stirring conditions for 2-12 hours, and then standing and precipitating for 2-12 hours, washing and vacuum drying the precipitated solid to obtain the etched hollow molecular imprinted polymer precursor; Step 3: performing an elution treatment on the etched hollow molecularly imprinted polymer precursor, and then vacuum drying to obtain the etched hollow molecularly imprinted polymer.
2. The method for preparing the etched hollow molecularly imprinted polymer according to claim 1, characterized in that: In step 2, the stirring conditions include: the stirring method is magnetic stirring, and the stirring speed is 200 to 800 r / min.
3. The method for preparing the etched hollow molecularly imprinted polymer according to claim 1, characterized in that: In step 2 and step 3, the vacuum drying treatment includes: the vacuum drying temperature is 80-100° C., the pressure is 0.01-0.1 MPa, and the time is 2-5 hours.
4. The method for preparing the etched hollow molecularly imprinted polymer according to claim 1, characterized in that: In step 2, the buffer solution is PBS buffer.
5. The method for preparing the etched hollow molecularly imprinted polymer according to claim 1, characterized in that: In step 3, the elution treatment includes: using a mixed solution of ethanol and acetic acid in a volume ratio of 92:8 for elution treatment.
6. The method for preparing the etched hollow molecularly imprinted polymer according to claim 1, characterized in that: The hollow titanate nanotubes are obtained by the following preparation method: Titanium dioxide, water and sodium hydroxide are mixed according to (1.2-9.6) g: (70-560) mL: (28-224) g, stirred evenly, and then transferred to 40-160° C. for reaction for 60-1380 min. After the reaction is completed, the reaction product is washed until the pH is neutral and vacuum dried for 6-12 h to obtain.
7. The method for preparing an etched hollow molecularly imprinted polymer according to claim 6, characterized in that: The diameter of the hollow titanate nanotube is no greater than 10 nm, and the length is no greater than 100 nm.
8. The method for preparing an etched hollow molecularly imprinted polymer according to claim 6, characterized in that: The stirring conditions include: the stirring method is magnetic stirring, the stirring speed is 500-1000 r / min, and the stirring time is 2-8 hours.
9. An etched hollow molecularly imprinted polymer obtained by the preparation method according to any one of claims 1 to 8.
10. An application of an etched hollow molecularly imprinted polymer obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The etched hollow molecular imprinting polymer is used for tetracycline pollution control and selective detection and separation of tetracycline in complex matrices.