Low-hardness colored natural rubber material and preparation method thereof
By combining natural rubber with cis-1,4-polybutadiene rubber and diatomaceous earth in low-hardness colored natural rubber, and using a specific vulcanization system, the problem of component balance and bonding performance control is solved. The combination of low hardness and excellent mechanical properties is achieved, reducing material consumption and improving environmental protection.
Patent Information
- Application Number
- CN202411262710.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-15
AI Technical Summary
Low hardness colored natural rubber has problems in the formulation design and production process, which is difficult to control the composition balance and bonding performance, resulting in poor processability, unstable material performance, and high consumption of traditional reinforcement agents, which affects the mechanical strength and service life of the product. .
Use natural rubber and cis-1,4-polybutadiene rubber, combined with diatomaceous earth, light calcium carbonate, cycloane oil and other reinforced plasticization systems, and pass a specific vulcanization system, including sulfur, 4, 4'-dithiodimorpholine, 2,2'-dithiodibenzothiazole and other components control the vulcanization temperature and time to ensure the low hardness and excellent vulcanization characteristics of the rubber.
It achieves the softness and mechanical properties of low-hardness rubber, ensures the stability and service life of the product, and reduces material consumption and meets environmental protection requirements.
Smart Images

Figure BDA0005036221880000091 
Figure BDA0005036221880000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber production, in particular to a low-hardness colored natural rubber material and a preparation method thereof. Background Art
[0002] In today's rapid development of industry and technology, natural rubber, as an elastic solid with excellent performance, has been widely used in many key fields such as home appliances, automobiles, electronics and even national defense technology, showing its irreplaceable and important position. Natural rubber has become an indispensable raw material for many industries due to its extremely strong elasticity, good insulation, plasticity, water and air barrier, tensile and wear resistance.
[0003] Traditionally, in order to further improve the physical properties and mechanical strength of natural rubber, carbon black is widely used as the main reinforcing agent and filler in the production of rubber products. Carbon black is not only consumed in large quantities (accounting for about half of rubber consumption), but also has a significant reinforcing effect on rubber products, especially in tire manufacturing. However, with the changes in market demand and the continuous progress of the rubber industry, colored natural rubber has gradually emerged as an emerging material. Its diverse colors and unique properties provide a broader space for product design and application.
[0004] As a branch of colored rubber, low-hardness colored natural rubber has great application potential in medical devices, household items, toys and other fields due to its softness, easy processing and rich colors. However, the formula design and production process of low-hardness colored natural rubber are more complicated than those of conventional hardness rubber, and there are many technical challenges. Specifically, the proportion of various raw materials needs to be precisely controlled during the formula design of low-hardness rubber to avoid abnormal phenomena such as poor processability, poor material properties and oil injection due to improper matching.
[0005] First of all, the balance and purity of the rubber material itself have a crucial impact on the performance of low-hardness rubber. The presence of any impurities or air may cause the hardness of the rubber to decrease, thereby affecting its performance. Therefore, strict control is required in the selection of raw materials to ensure the quality of the rubber material.
[0006] Secondly, key parameters in the production process such as vulcanization temperature, vulcanization time and rubber ratio are also important factors affecting the performance of low-hardness colored rubber. If the vulcanization temperature is not enough or the vulcanization time is not enough, the rubber product will not be fully cross-linked, thus affecting its physical properties and mechanical strength. At the same time, unreasonable rubber ratio will also directly affect key indicators such as rubber hardness, elasticity and wear resistance.
[0007] In addition, during the production process of low-hardness colored natural rubber, special attention should be paid to its bonding performance with other materials. The bonding strength between rubber and rubber, between rubber and plastic, and between rubber and skeleton materials directly affects the overall performance and service life of rubber products. If the bonding is not strong, the rubber products will fall off and crack during use, which will seriously affect the use effect of the product. Summary of the invention
[0008] In view of the deficiencies in the prior art, the present invention provides a low-hardness colored natural rubber material and a preparation method thereof, which solves the problems raised in the above-mentioned background technology.
[0009] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0010] In a first aspect, the present invention provides a low-hardness colored natural rubber material, comprising the following components by weight:
[0011] The matrix glue composition is 46% to 52%, the reinforcing plasticizing composition is 37% to 43%, the vulcanizing composition is 2.1% to 2.7%, the zinc oxide is 2% to 3%, the octadecanoic acid is 0.6% to 0.9%, the polyethylene glycol is 0.8% to 1%, the 935P is 0.8% to 1%, the (Z)-9-octadecenoic acid amide is 0.4% to 0.6%, the vinyl tris (b-methoxyethoxy) silane is 0.8% to 1%, the titanium dioxide is 0.2% to 0.3%, and the color masterbatch is 0.4% to 0.6%.
[0012] Furthermore, the matrix rubber composition uses natural rubber and cis-1,4-polybutadiene rubber in combination, with the weight ratio of natural rubber being 33% to 36% and the weight ratio of cis-1,4-polybutadiene rubber being 13% to 16%, thereby eliminating vulcanization reversion to a certain extent and improving the heat generation and wear resistance of the material.
[0013] Furthermore, the reinforcing plasticizing composition uses diatomaceous earth, light calcium carbonate and cyclohexane oil in combination, with the weight ratio of diatomaceous earth being 9% to 11%, the weight ratio of light calcium carbonate being 14% to 16%, and the weight ratio of cyclohexane oil being 14% to 16%, so that oil spraying will not occur while ensuring low hardness.
[0014] Furthermore, the vulcanization composition uses sulfur, 4,4'-dithiodimorpholine and 2,2'-dithiodibenzothiazole in combination, and the weight ratio of sulfur is 0.7% to 0.9%, the weight ratio of 4,4'-dithiodimorpholine is 0.7% to 0.9%, and the weight ratio of 2,2'-dithiodibenzothiazole is 0.7% to 0.9%, ensuring that the material has excellent scorch time and positive vulcanization time.
[0015] In a second aspect, the present invention further provides a method for preparing a low-hardness colored natural rubber material, comprising the following steps:
[0016] S1. Weigh the materials according to the weight ratio;
[0017] S2. Put the natural rubber into an internal mixer, mix it to 140℃, and leave it for more than 24 hours;
[0018] S3, put the natural rubber and cis-1,4-polybutadiene rubber after internal mixing into an internal mixer and internal mix for 1 minute, then lift the top bolt of the internal mixer, and add diatomaceous earth, light calcium carbonate, cyclohexane oil, zinc oxide, octadecanoic acid, polyethylene glycol, 935P, (Z)-9-octadecenoic acid amide, vinyl tri(b-methoxyethoxy) silane, titanium dioxide and masterbatch, internal mix to 120°C for rubber discharge, cool to room temperature, collect the rubber, and leave it for more than 16 hours to obtain a premixed rubber;
[0019] S4, putting the premixed rubber into an internal mixer and mixing it to 95°C, then lifting the top bolt of the internal mixer again, adding sulfur, 4,4′-dimorpholine disulfide, and 2,2′-dibenzothiazole disulfide, mixing it to 105°C and discharging the rubber to obtain a vulcanized rubber;
[0020] S5. Put the vulcanized rubber into the open mill, pass the open mill 4-6 times with a thickness of 2 mm, make 2 triangle packs, adjust the roller distance to 6-8 mm and cool the sheet;
[0021] S6. Take samples for inspection and test hardness, strength, elongation, T10 and T90 for monitoring;
[0022] S7, the rubber that has passed the test is subjected to an open mixing mill for refining and molding, and the molded rubber is then placed into a mold in a vulcanization device for vulcanization molding treatment;
[0023] S8. Trim the vulcanized product and inspect its size and appearance to obtain qualified finished products.
[0024] Furthermore, in S3, the kneaded natural rubber and cis-1,4-polybutadiene rubber are fed into an internal mixer, and in S4, the premixed rubber is fed into an internal mixer, and the feeding temperature is not higher than 65°C.
[0025] Furthermore, in S7, the mixing temperature of the mixing mill is 55-65°C.
[0026] Furthermore, the pressure of the mold in the vulcanization equipment is 180-200 Kgf / cm 2 , the temperature is 160-170℃, and the vulcanization time is 240-260 seconds.
[0027] The present invention provides a low-hardness colored natural rubber material and a preparation method thereof. Compared with the prior art, it has the following beneficial effects:
[0028] 1. Low hardness property: The present invention uses natural rubber and cis-1,4-polybutadiene rubber together, and through a specific reinforcement plasticizing system and vulcanization system, the rubber presents low hardness. This property makes the rubber product softer and more comfortable during use, and is suitable for fields with special requirements on hardness, such as seals, shock absorbing materials, etc.
[0029] 2. Excellent vulcanization characteristics: The vulcanization system in the formula uses ingredients such as 4,4'-dithiodimorpholine, which makes the rubber have good vulcanization characteristics. Specifically, the scorch time is moderate, which ensures the safety of the production process; the positive vulcanization time is reasonable, which improves the production efficiency; the maximum torque and minimum torque values are relatively ideal, indicating that the cross-linking degree of the rubber during the vulcanization process is moderate, thus ensuring the stable performance of the rubber.
[0030] 3. Good physical and mechanical properties: By using diatomaceous earth, light calcium carbonate and naphthenic oil and other reinforcing and plasticizing systems, the physical and mechanical properties of rubber such as tensile strength, elongation at break, and tear strength are significantly improved, which can meet the use requirements under various complex working conditions. For example, when subjected to external forces such as stretching and tearing, it has higher reliability and durability.
[0031] 4. Environmental protection and sustainability: The materials used in the present invention are mostly common industrial raw materials, which are widely available and relatively environmentally friendly. Compared with traditional rubber formulas, it reduces pollution to the environment and meets the requirements of sustainable development. At the same time, by optimizing the formula, the performance of the rubber is improved, the consumption of materials is reduced, and it also helps to save resources. DETAILED DESCRIPTION
[0032] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.
[0033] Example 1
[0034] A low-hardness colored natural rubber material, comprising the following components by weight:
[0035] Natural rubber 35.5%, cis-1,4-polybutadiene rubber 16%, diatomaceous earth 9%, light calcium carbonate 15%, cyclohexane oil 15%, sulfur 0.8%, 4,4'-dithiodimorpholine 0.8%, 2,2'-dithiodibenzothiazole 0.8%, zinc oxide 2.5%, octadecanoic acid 0.8%, polyethylene glycol 0.9%, 935P 0.9%, (Z)-9-octadecenoic acid amide 0.5%, vinyl tri(b-methoxyethoxy) silane 0.8%, titanium dioxide 0.2%, masterbatch 0.5%.
[0036] The method for preparing the above-mentioned low-hardness colored natural rubber material comprises the following steps:
[0037] S1. Weigh the materials according to the weight ratio;
[0038] S2. Put the natural rubber into an internal mixer, mix it to 140℃, and leave it for more than 24 hours;
[0039] S3, put the natural rubber and cis-1,4-polybutadiene rubber after internal mixing into an internal mixer (the feeding temperature is not higher than 65°C), after internal mixing for 1 minute, lift the top bolt of the internal mixer, and add diatomaceous earth, light calcium carbonate, cyclohexane oil, zinc oxide, octadecanoic acid, polyethylene glycol, 935P, (Z)-9-octadecenoic acid amide, vinyl tri(b-methoxyethoxy) silane, titanium dioxide and masterbatch, internal mixing to 120°C for rubber discharge, cool to room temperature, collect the rubber, and leave it for more than 16 hours to obtain a premixed rubber;
[0040] S4, the premixed rubber is put into an internal mixer (the feeding temperature is not higher than 65°C), and after internal mixing to 95°C, the top bolt of the internal mixer is lifted again, and sulfur, 4,4'-dithiodimorpholine, and 2,2'-dithiodibenzothiazole are added, and the mixture is internally mixed to 105°C and the rubber is discharged to obtain a vulcanized rubber;
[0041] S5. Put the vulcanized rubber into the open mill, pass the open mill 4-6 times with a thickness of 2 mm, make 2 triangle packs, adjust the roller distance to 6-8 mm and cool the sheet;
[0042] S6. Take samples for inspection and test hardness, strength, elongation, T10 and T90 for monitoring;
[0043] S7, the qualified rubber is put into the mold of the vulcanizing equipment (pressure is 180Kgf / cm 2 , temperature is 160°C, vulcanization time is 240 seconds), and vulcanization molding treatment is performed;
[0044] S8. Trim the vulcanized product and inspect its size and appearance to obtain qualified finished products.
[0045] Example 2
[0046] A low-hardness colored natural rubber material, comprising the following components by weight:
[0047] Natural rubber 35%, cis-1,4-polybutadiene rubber 15.9%, diatomaceous earth 9.3%, light calcium carbonate 16%, cyclohexane oil 14.5%, sulfur 0.7%, 4,4'-dithiodimorpholine 0.9%, 2,2'-dithiodibenzothiazole 0.7%, zinc oxide 2%, octadecanoic acid 0.9%, polyethylene glycol 0.8%, 935P 1%, (Z)-9-octadecenoic acid amide 0.4%, vinyl tri(b-methoxyethoxy) silane 1%, titanium dioxide 0.3%, masterbatch 0.6%.
[0048] The method for preparing the above-mentioned low-hardness colored natural rubber material comprises the following steps:
[0049] S1. Weigh the materials according to the weight ratio;
[0050] S2. Put the natural rubber into an internal mixer, mix it to 140℃, and leave it for more than 24 hours;
[0051] S3, put the natural rubber and cis-1,4-polybutadiene rubber after internal mixing into an internal mixer (the feeding temperature is not higher than 65°C), after internal mixing for 1 minute, lift the top bolt of the internal mixer, and add diatomaceous earth, light calcium carbonate, cyclohexane oil, zinc oxide, octadecanoic acid, polyethylene glycol, 935P, (Z)-9-octadecenoic acid amide, vinyl tri(b-methoxyethoxy) silane, titanium dioxide and masterbatch, internal mixing to 120°C for rubber discharge, cool to room temperature, collect the rubber, and leave it for more than 16 hours to obtain a premixed rubber;
[0052] S4, the premixed rubber is put into an internal mixer (the feeding temperature is not higher than 65°C), and after internal mixing to 95°C, the top bolt of the internal mixer is lifted again, and sulfur, 4,4'-dithiodimorpholine, and 2,2'-dithiodibenzothiazole are added, and the mixture is internally mixed to 105°C and the rubber is discharged to obtain a vulcanized rubber;
[0053] S5. Put the vulcanized rubber into the open mill, pass the open mill 4-6 times with a thickness of 2 mm, make 2 triangle packs, adjust the roller distance to 6-8 mm and cool the sheet;
[0054] S6. Take samples for inspection and test hardness, strength, elongation, T10 and T90 for monitoring;
[0055] S7, the qualified rubber is put into the mold of the vulcanizing equipment (pressure is 190Kgf / cm 2, temperature is 165°C, vulcanization time is 250 seconds), and vulcanization molding treatment is performed;
[0056] S8. Trim the vulcanized product and inspect its size and appearance to obtain qualified finished products.
[0057] Example 3
[0058] A low-hardness colored natural rubber material, comprising the following components by weight:
[0059] Natural rubber 36%, cis-1,4-polybutadiene rubber 13%, diatomaceous earth 11%, light calcium carbonate 14%, cyclohexane oil 15.9%, sulfur 0.9%, 4,4'-dithiodimorpholine 0.7%, 2,2'-dithiodibenzothiazole 0.9%, zinc oxide 3%, octadecanoic acid 0.6%, polyethylene glycol 1%, 935P 0.8%, (Z)-9-octadecenoic acid amide 0.6%, vinyl tri(b-methoxyethoxy) silane 0.8%, titanium dioxide 0.3%, masterbatch 0.5%.
[0060] The method for preparing the above-mentioned low-hardness colored natural rubber material comprises the following steps:
[0061] S1. Weigh the materials according to the weight ratio;
[0062] S2. Put the natural rubber into an internal mixer, mix it to 140℃, and leave it for more than 24 hours;
[0063] S3, put the natural rubber and cis-1,4-polybutadiene rubber after internal mixing into an internal mixer (the feeding temperature is not higher than 65°C), after internal mixing for 1 minute, lift the top bolt of the internal mixer, and add diatomaceous earth, light calcium carbonate, cyclohexane oil, zinc oxide, octadecanoic acid, polyethylene glycol, 935P, (Z)-9-octadecenoic acid amide, vinyl tri(b-methoxyethoxy) silane, titanium dioxide and masterbatch, internal mixing to 120°C for rubber discharge, cool to room temperature, collect the rubber, and leave it for more than 16 hours to obtain a premixed rubber;
[0064] S4, the premixed rubber is put into an internal mixer (the feeding temperature is not higher than 65°C), and after internal mixing to 95°C, the top bolt of the internal mixer is lifted again, and sulfur, 4,4'-dithiodimorpholine, and 2,2'-dithiodibenzothiazole are added, and the mixture is internally mixed to 105°C and the rubber is discharged to obtain a vulcanized rubber;
[0065] S5. Put the vulcanized rubber into the open mill, pass the open mill 4-6 times with a thickness of 2 mm, make 2 triangle packs, adjust the roller distance to 6-8 mm and cool the sheet;
[0066] S6. Take samples for inspection and test hardness, strength, elongation, T10 and T90 for monitoring;
[0067] S7, the qualified rubber is molded through an open mill (the open mill temperature is 65°C), and then the molded rubber is placed in the mold of the vulcanization equipment (pressure is 200Kgf / cm 2 , temperature is 170°C, vulcanization time is 260 seconds), and vulcanization molding treatment is performed;
[0068] S8. Trim the vulcanized product and inspect its size and appearance to obtain qualified finished products.
[0069] Experimental Section
[0070] 1. Purpose of the experiment
[0071] This experiment aims to study the use of natural rubber and cis-1,4-polybutadiene rubber, using different reinforcement and plasticization systems and vulcanization systems to obtain a rubber material with low hardness, excellent vulcanization characteristics and good physical and mechanical properties;
[0072] 2. Experimental Materials
[0073] 1. Main rubber materials: natural rubber, cis-1,4-polybutadiene rubber.
[0074] 2. Reinforcement and plasticization system: diatomaceous earth, light calcium carbonate, and cyclohexane oil.
[0075] 3. Vulcanization system: sulfur, 4,4'-dithiodimorpholine, 2,2'-dithiodibenzothiazole, zinc oxide, octadecanoic acid, polyethylene glycol, 935P, (Z)-9-octadecenoic acid amide, vinyl tris(b-methoxyethoxy)silane, titanium dioxide, masterbatch;
[0076] 3. Experimental Design
[0077] 1. Three embodiments and one control group were set up, and the specific formula is as follows:
[0078] Example 1: 35.5% natural rubber, 16% cis-1,4-polybutadiene rubber, 9% diatomaceous earth, 15% light calcium carbonate, 15% naphthenic oil, 0.8% sulfur, 0.8% 4,4'-dithiodimorpholine, 0.8% 2,2'-dithiodibenzothiazole, 2.5% zinc oxide, 0.8% octadecanoic acid, 0.9% polyethylene glycol, 0.9% 935P, 0.5% (Z)-9-octadecenoic acid amide, 0.8% vinyl tris (b-methoxyethoxy) silane, 0.2% titanium dioxide, 0.5 color masterbatch;
[0079] Example 2: 35% natural rubber, 15.9% cis-1,4-polybutadiene rubber, 9.3% diatomaceous earth, 16% light calcium carbonate, 14.5% naphthenic oil, 0.7% sulfur, 0.9% 4,4'-dithiodimorpholine, 0.7% 2,2'-dithiodibenzothiazole, 2% zinc oxide, 0.9% octadecanoic acid, 0.8% polyethylene glycol, 1% 935P, 0.4% (Z)-9-octadecenoic acid amide, 1% vinyl tris (b-methoxyethoxy) silane, 0.3% titanium dioxide, 0.6% masterbatch;
[0080] Example 3: 36% natural rubber, 13% cis-1,4-polybutadiene rubber, 11% diatomaceous earth, 14% light calcium carbonate, 15.9% naphthenic oil, 0.9% sulfur, 0.7% 4,4′-dithiodimorpholine, 0.9% 2,2′-dithiodibenzothiazole, 3% zinc oxide, 0.6% octadecanoic acid, 1% polyethylene glycol, 0.8% 935P, 0.6% (Z)-9-octadecenoic acid amide, 0.8% vinyl tris(b-methoxyethoxy)silane, 0.3% titanium dioxide, 0.5% masterbatch;
[0081] Control group: natural rubber 40%, cis-1,4-polybutadiene rubber 10%, carbon black 20%, aromatic oil 10%, sulfur 1.5%, accelerator M 1%, zinc oxide 3%, stearic acid 1%, antioxidant 1%;
[0082] 2. Mix various materials evenly according to the formula, vulcanize them at a certain temperature and pressure, and prepare rubber samples;
[0083] 4. Experimental Test
[0084] 1. Hardness test: Use a Shore durometer to measure the hardness of the rubber sample.
[0085] 2. Vulcanization characteristics test: Use a rotorless vulcanizer to test the vulcanization characteristics of rubber, including scorch time (T10), positive vulcanization time (T90), maximum torque (Mh), and minimum torque (M l).
[0086] 3. Physical and mechanical properties test:
[0087] Tensile properties: Use a universal testing machine to test the tensile strength, elongation at break and tensile stress of rubber.
[0088] Tear performance: The tear strength of rubber is tested by right-angle tear test.
[0089] Compression set: The rubber sample is compressed to a certain ratio, kept at a certain temperature for a certain period of time, and then its compression set is measured.
[0090] V. Experimental Results
[0091]
[0092]
[0093] 6. Experimental Conclusion
[0094] 1. Natural rubber and cis-1,4-polybutadiene rubber are used together, diatomaceous earth, light calcium carbonate and cyclohexane oil are used in the reinforcement and plasticization system, and 4,4'-dithiodimorpholine is used in the vulcanization system, which can give the rubber a low hardness while taking into account excellent vulcanization characteristics and good physical and mechanical properties.
[0095] 2. Compared with the control group, the rubber hardness in the embodiment is significantly reduced, while the physical and mechanical properties such as tensile strength, elongation at break, and tear strength are improved, and the vulcanization characteristics are also improved.
Claims
1. A low-hardness colored natural rubber material, characterized in that: Contains the following components by weight: The matrix glue composition is 46% to 52%, the reinforcing plasticizing composition is 37% to 43%, the vulcanizing composition is 2.1% to 2.7%, the zinc oxide is 2% to 3%, the octadecanoic acid is 0.6% to 0.9%, the polyethylene glycol is 0.8% to 1%, the 935P is 0.8% to 1%, the (Z)-9-octadecenoic acid amide is 0.4% to 0.6%, the vinyl tris (b-methoxyethoxy) silane is 0.8% to 1%, the titanium dioxide is 0.2% to 0.3%, and the color masterbatch is 0.4% to 0.6%.
2. The low-hardness colored natural rubber material according to claim 1, characterized in that: The matrix rubber composition uses natural rubber and cis-1,4-polybutadiene rubber in combination, with the weight ratio of the natural rubber being 33% to 36% and the weight ratio of the cis-1,4-polybutadiene rubber being 13% to 16%.
3. The low-hardness colored natural rubber material according to claim 1, characterized in that: The reinforcing plasticizing composition uses diatomaceous earth, light calcium carbonate and naphthenic oil in combination, wherein the weight ratio of diatomaceous earth is 9% to 11%, the weight ratio of light calcium carbonate is 14% to 16%, and the weight ratio of naphthenic oil is 14% to 16%.
4. The low-hardness colored natural rubber material according to claim 1, characterized in that: The vulcanization composition uses sulfur, 4,4'-dithiodimorpholine and 2,2'-dithiodibenzothiazole in combination, and the weight ratio of sulfur is 0.7% to 0.9%, the weight ratio of 4,4'-dithiodimorpholine is 0.7% to 0.9%, and the weight ratio of 2,2'-dithiodibenzothiazole is 0.7% to 0.9%.
5. A low-hardness colored natural rubber material according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: S1. Weigh the materials according to the weight ratio; S2. Put the natural rubber into an internal mixer, mix it to 140℃, and leave it for more than 24 hours; S3, put the natural rubber and cis-1,4-polybutadiene rubber after internal mixing into an internal mixer and internal mix for 1 minute, then lift the top bolt of the internal mixer, and add diatomaceous earth, light calcium carbonate, cyclohexane oil, zinc oxide, octadecanoic acid, polyethylene glycol, 935P, (Z)-9-octadecenoic acid amide, vinyl tri(b-methoxyethoxy) silane, titanium dioxide and masterbatch, internal mix to 120°C for rubber discharge, cool to room temperature, collect the rubber, and leave it for more than 16 hours to obtain a premixed rubber; S4, putting the premixed rubber into an internal mixer and mixing it to 95°C, then lifting the top bolt of the internal mixer again, adding sulfur, 4,4′-dimorpholine disulfide, and 2,2′-dibenzothiazole disulfide, mixing it to 105°C and discharging the rubber to obtain a vulcanized rubber; S5. Put the vulcanized rubber into the open mill, pass the open mill 4-6 times with a thickness of 2 mm, make 2 triangle packs, adjust the roller distance to 6-8 mm and cool the sheet; S6. Take samples for inspection and test hardness, strength, elongation, T10 and T90 for monitoring; S7, the rubber that has passed the test is subjected to an open mixing mill for refining and molding, and the molded rubber is then placed into a mold in a vulcanization device for vulcanization molding treatment; S8. Trim the vulcanized product and inspect its size and appearance to obtain qualified finished products.
6. The method for preparing a low-hardness colored natural rubber material according to claim 5, characterized in that: In the S3, the kneaded natural rubber and cis-1,4-polybutadiene rubber are put into an internal mixer, and in the S4, the premixed rubber is put into an internal mixer, and the feeding temperature is not higher than 65°C.
7. The method for preparing a low-hardness colored natural rubber material according to claim 5, characterized in that: In S7, the mixing temperature of the mixing mill is 55-65°C.
8. The method for preparing a low-hardness colored natural rubber material according to claim 5, characterized in that: The pressure of the mold in the vulcanization equipment is 180-200 Kgf / cm 2 , the temperature is 160-170℃, and the vulcanization time is 240-260 seconds.