Polyvinyl alcohol film waste regenerated particle and production method and application thereof
By mixing polyvinyl alcohol film waste with water, starch, mold release agent and emulsifier, low-temperature screw extrusion, the color and appearance of regenerated particles of polyvinyl alcohol film waste are solved, and semi-transparent and good-looking regenerated particles are achieved Production.
Patent Information
- Application Number
- CN202310541783.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-15
AI Technical Summary
During the melt extrusion and granulation process of polyvinyl alcohol thin film waste, the regenerated particles produced are darker in color and have poor appearance. The reason is that the melting point and decomposition point of polyvinyl alcohol are close, which leads to easy decomposition at high temperatures and destroys its properties.
Mix polyvinyl alcohol film waste with water, starch, mold release agent and emulsifier, extrude and mold the low-temperature screw, and control the temperature between 60℃ and 95℃ to avoid decomposition, starch increases adhesion, and emulsifier ensures uniform composition , the release agent prevents adhesion.
Regenerated particles with translucent appearance are obtained, which avoids the decomposition of polyvinyl alcohol during high-temperature extrusion, maintains the original properties, and improves the color and appearance quality of the regenerated particles.
Smart Images

Figure BSA0000296953960000081 
Figure BSA0000296953960000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer material recycling, and in particular to polyvinyl alcohol film waste recycled particles and a production method and application thereof. Background Art
[0002] With the rapid development of chemical technology, polymer materials have been widely used in various aspects of industrial and civilian products. Polymer materials will generate waste during processing and use. These wastes exist in the form of solid wastes, and some of them will leak additives containing toxic ingredients. If they are not disposed of, they will cause serious pollution to the environment and endanger the health of humans, animals and plants.
[0003] Polyvinyl alcohol film is one of many polymer materials. It will produce scraps during the processing. The same problem also exists in the discarded polyvinyl alcohol film packaging dissolved in high-temperature water. Effectively handling the scraps of polyvinyl alcohol film and the discarded packaging made of polyvinyl alcohol can play a good role in protecting the environment. At the same time, recycling these materials can save resources.
[0004] The method of recycling waste polymer materials is usually to simply classify and clean them before melt extrusion granulation. However, in the process of realizing the present invention, the inventors found that when using polyvinyl alcohol film waste for melt extrusion granulation, the regenerated particles produced have the problem of dark color and poor appearance. Summary of the invention
[0005] In view of this, the present invention provides a polyvinyl alcohol film waste recycled particles and a production method and use thereof, so as to solve the problem that the polyvinyl alcohol film waste recycled particles produced in the related art have darker color and poorer appearance.
[0006] In a first aspect, the present invention provides a method for producing recycled particles from polyvinyl alcohol film waste, the method comprising the following steps:
[0007] Mixing the polyvinyl alcohol film waste fragments with water to obtain an intermediate material;
[0008] The intermediate material is mixed with starch, a release agent and an emulsifier, and dispersed evenly to obtain a material to be extruded;
[0009] The material to be extruded is screw extruded under negative pressure exhaust conditions, and cut after cooling, wherein the temperature of the screw extrusion is 60° C. to 95° C.
[0010] The inventors have found that the reason why the recycled particles of polyvinyl alcohol film waste produced in the related technology are darker in color and have poor appearance is that the melting point and decomposition point of polyvinyl alcohol (PVA) are relatively close, with a difference of about 10°C, which is extremely unfavorable for the plasticization of polyvinyl alcohol (PVA). The heating temperature accuracy of general melt extrusion equipment is low, and it is difficult to ensure that polyvinyl alcohol (PVA) does not decompose during the melting process. The decomposition of polyvinyl alcohol (PVA) will affect its properties, which will cause the color of the recycled particles to become darker on the one hand, and the appearance of the recycled particles to be poor on the other hand.
[0011] In the above-mentioned production method provided by the present invention, by compounding the polyvinyl alcohol film waste fragments with water, starch, a release agent and an emulsifier, the polyvinyl alcohol film waste fragments are subjected to low-temperature screw extrusion molding at 60°C to 95°C. Since the temperature of the screw extrusion molding is lower than 100°C, the problem of polyvinyl alcohol decomposition in the high-temperature screw extrusion process is effectively overcome. The low-temperature screw extrusion molding process will not destroy the original properties of polyvinyl alcohol, thereby obtaining translucent recycled particles with good appearance.
[0012] Specifically, when the temperature is lower than 100°C, polypropylene alcohol is semi-soluble in water due to its water solubility. During the screw extrusion process, when the temperature reaches above 60°C, the starch will gelatinize, increasing the adhesion between water and polypropylene alcohol film waste fragments, neutralizing the plasticizing effect of the original plasticizer in the waste, and reducing the plasticity of the waste, so as to achieve low-temperature screw extrusion of the waste fragments; the release agent can prevent the material from sticking during the extrusion die head, affecting the extrusion continuity and the appearance of the particles; the emulsifier can fully and evenly emulsify the polypropylene alcohol, water and the release agent, so that the composition of the extruded recycled particles is uniform.
[0013] In an optional embodiment, the ratio of the polyvinyl alcohol film waste fragments, the water, the starch, the release agent and the emulsifier is (60-80): (15-30): (5-15): (0.5-3): (1-2) in parts by weight.
[0014] In the above production method provided by the present invention, the weight ratio between various raw materials is suitable, which is more conducive to the low-temperature screw extrusion of polyvinyl alcohol film waste. For example, the amount of starch used is 5 to 15 parts by weight. Within this amount range, it can ensure that the material has sufficient adhesion and completely neutralizes the plasticity generated by the plasticizer in the waste. At the same time, it can ensure that the material has appropriate fluidity, making processing easier; the amount of emulsifier used is 1 to 2 parts by weight. Within this amount range, it can ensure an ideal emulsification effect and avoid the phenomenon of emulsifier seepage during the storage of the regenerated particles.
[0015] In an optional embodiment, the polyvinyl alcohol film waste fragments, the water, the starch, the release agent and the emulsifier are used in a ratio of 75:20:8:1:1.
[0016] In an optional embodiment, in the polyvinyl alcohol film waste fragments, the degree of polymerization of the polyvinyl alcohol is 500-2400, and the degree of alcoholysis is 86%-99%.
[0017] In the above-mentioned production method provided by the present invention, the degree of polymerization of polyvinyl alcohol is preferably 500-2400, and the degree of alcoholysis is 86%-99%. Within this range, the material fluidity is better and it is easier to carry out extrusion processing. At the same time, the regenerated particles produced are of suitable hardness and are not easy to deform. The manufactured products can withstand high humidity environments, do not stick and deform, and have stronger versatility.
[0018] In an optional embodiment, the starch includes at least one of corn starch, sweet potato starch, cassava starch, oxidized starch, cross-linked starch and acid-modified starch;
[0019] Optionally, the starch is corn starch.
[0020] In an optional embodiment, the release agent is a water-soluble release agent, including at least one of dimethyl silicone oil, modified silicone oil, hydrogenated silicone oil, emulsified silicone oil and amino silicone oil;
[0021] Optionally, the release agent is water-soluble dimethyl silicone oil.
[0022] In an optional embodiment, the emulsifier includes at least one of Tween 80, Tween 60, Tween 20, Tween 85, Span 80 and Span 6;
[0023] Optionally, the emulsifier is Tween 80.
[0024] In an optional embodiment, the diameter of the polyvinyl alcohol film waste fragments is 2 mm to 3 mm. Under this condition, the fragments can be fully mixed with other materials and all the fragments can be wetted by water.
[0025] In a second aspect, the present invention further provides recycled particles from waste polyvinyl alcohol film, wherein the recycled particles from waste polyvinyl alcohol film are produced by the production method described above.
[0026] In a third aspect, the present invention also provides the use of the above-mentioned polyvinyl alcohol film waste recycled particles in the preparation of polyvinyl alcohol film.
[0027] In a fourth aspect, the present invention further provides a polyvinyl alcohol film, wherein the polyvinyl alcohol film is prepared using the above-mentioned polyvinyl alcohol film waste recycled particles. DETAILED DESCRIPTION
[0028] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0029] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0030] In order to solve the problems existing in the above-mentioned related art, according to a first aspect of the present invention, a method for producing recycled particles of polyvinyl alcohol film waste is provided, and the production method comprises the following steps:
[0031] Mixing the polyvinyl alcohol film waste fragments with water to obtain an intermediate material;
[0032] The intermediate material is mixed with starch, a release agent and an emulsifier, and dispersed evenly to obtain a material to be extruded;
[0033] The material to be extruded is screw extruded under negative pressure exhaust conditions, and cut after cooling, wherein the temperature of the screw extrusion is 60° C. to 95° C.
[0034] The inventors have found that the reason why the recycled particles of polyvinyl alcohol film waste produced in the related technology are darker in color and have poor appearance is that the melting point and decomposition point of polyvinyl alcohol (PVA) are relatively close, with a difference of about 10°C, which is extremely unfavorable for the plasticization of polyvinyl alcohol (PVA). The heating temperature accuracy of general melt extrusion equipment is low, and it is difficult to ensure that polyvinyl alcohol (PVA) does not decompose during the melting process. The decomposition of polyvinyl alcohol (PVA) will affect its properties, which will cause the color of the recycled particles to become darker on the one hand, and the appearance of the recycled particles to be poor on the other hand.
[0035] In the above-mentioned production method provided by the present invention, by compounding the polyvinyl alcohol film waste fragments with water, starch, a release agent and an emulsifier, the polyvinyl alcohol film waste fragments are subjected to low-temperature screw extrusion molding at 60°C to 95°C. Since the temperature of the screw extrusion molding is lower than 100°C, the problem of polyvinyl alcohol decomposition in the high-temperature screw extrusion process is effectively overcome. The low-temperature screw extrusion molding process will not destroy the original properties of polyvinyl alcohol, thereby obtaining translucent recycled particles with good appearance.
[0036] Specifically, when the temperature is lower than 100°C, polypropylene alcohol is semi-soluble in water due to its water solubility. During the screw extrusion process, when the temperature reaches above 60°C, the starch will gelatinize, increasing the adhesion between water and polypropylene alcohol film waste fragments, neutralizing the plasticizing effect of the original plasticizer in the waste, and reducing the plasticity of the waste, so as to achieve low-temperature screw extrusion of the waste fragments; the release agent can prevent the material from sticking during the extrusion die head, affecting the extrusion continuity and the appearance of the particles; the emulsifier can fully and evenly emulsify the polypropylene alcohol, water and the release agent, so that the composition of the extruded recycled particles is uniform.
[0037] Among them, screw extrusion is carried out under negative pressure exhaust conditions, which can ensure that the water vapor generated during the heating and extrusion process is discharged in time, avoid the formation of high pressure in the heating chamber, and minimize the water content of the regenerated particles. Exemplarily, a venting single screw extruder can be used for the screw extrusion of the present invention, and the aspect ratio of the venting single screw extruder can be 1:22. In a particularly preferred embodiment, the temperature of the screw extrusion is 90°C.
[0038] In an optional embodiment, the ratio of the polyvinyl alcohol film waste fragments, the water, the starch, the release agent and the emulsifier is (60-80): (15-30): (5-15): (0.5-3): (1-2) in parts by weight.
[0039] In the above production method provided by the present invention, the weight ratio between various raw materials is suitable, which is more conducive to the low-temperature screw extrusion of polyvinyl alcohol film waste. For example, the amount of starch used is 5 to 15 parts by weight. Within this amount range, it can ensure that the material has sufficient adhesion and completely neutralizes the plasticity generated by the plasticizer in the waste. At the same time, it can ensure that the material has appropriate fluidity, making processing easier; the amount of emulsifier used is 1 to 2 parts by weight. Within this amount range, it can ensure an ideal emulsification effect and avoid the phenomenon of emulsifier seepage during the storage of the regenerated particles.
[0040] In an optional embodiment, the polyvinyl alcohol film waste fragments, the water, the starch, the release agent and the emulsifier are used in a ratio of 75:20:8:1:1.
[0041] In an optional embodiment, in the polyvinyl alcohol film waste fragments, the degree of polymerization of polyvinyl alcohol is 500-2400, and the degree of alcoholysis is 86%-99%.
[0042] In the above-mentioned production method provided by the present invention, the degree of polymerization of polyvinyl alcohol is preferably 500-2400, and the degree of alcoholysis is 86%-99%. Within this range, the material fluidity is better and it is easier to carry out extrusion processing. At the same time, the regenerated particles produced are of suitable hardness and are not easy to deform. The manufactured products can withstand high humidity environments, do not stick and deform, and have stronger versatility.
[0043] In an optional embodiment, the starch includes at least one of corn starch, sweet potato starch, cassava starch, oxidized starch, cross-linked starch and acid-modified starch;
[0044] Optionally, the starch is corn starch.
[0045] In an optional embodiment, the release agent is a water-soluble release agent, including at least one of dimethyl silicone oil, modified silicone oil, hydrogenated silicone oil, emulsified silicone oil and amino silicone oil;
[0046] Optionally, the release agent is water-soluble dimethyl silicone oil.
[0047] In an optional embodiment, the emulsifier includes at least one of Tween 80, Tween 60, Tween 20, Tween 85, Span 80 and Span 6;
[0048] Optionally, the emulsifier is Tween 80.
[0049] In an optional embodiment, the diameter of the polyvinyl alcohol film waste fragments is 2 mm to 3 mm. Under this condition, the fragments can be fully mixed with other materials and all the fragments can be wetted by water.
[0050] In a second aspect, the present invention further provides recycled particles from waste polyvinyl alcohol film, wherein the recycled particles from waste polyvinyl alcohol film are produced by the production method described above.
[0051] In a third aspect, the present invention also provides the use of the above-mentioned polyvinyl alcohol film waste recycled particles in the preparation of polyvinyl alcohol film.
[0052] In a fourth aspect, the present invention further provides a polyvinyl alcohol film, wherein the polyvinyl alcohol film is prepared using the above-mentioned polyvinyl alcohol film waste recycled particles.
[0053] The present invention is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed by the present invention.
[0054] Example 1
[0055] Polyvinyl alcohol film waste recycled particles are produced according to the following raw material formula and production method:
[0056] Raw material formula: 70kg polyvinyl alcohol film waste, 20kg water, 8kg corn starch, 1kg dimethyl silicone oil, 1kg Tween 80.
[0057] Production method:
[0058] (1) crushing a polyvinyl alcohol film of formula 1799 (polyvinyl alcohol degree of polymerization: 1700, degree of alcoholysis: 99%) into pieces with an average diameter of 2-3 mm, putting the pieces into a stirring kettle, adding a formula amount of water, and stirring until all the pieces are wetted by water to obtain an intermediate material;
[0059] (2) Add corn starch, dimethyl silicone oil and Tween 80 in the formula amount to the stirring tank loaded with the intermediate material, and continue stirring until all the ingredients are evenly dispersed to obtain the material to be extruded;
[0060] (3) The material to be extruded is fed into a vented single screw extruder through a screw feeding system, extruded at 90° C., and cut into particles after air cooling. During the extrusion process, negative pressure exhaust is turned on to discharge water vapor.
[0061] Example 2
[0062] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that the raw material formula used in this example was: 70 kg of polyvinyl alcohol film waste, 30 kg of water, 5 kg of corn starch, 1 kg of dimethyl silicone oil, and 1 kg of Tween 80.
[0063] Example 3
[0064] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that the raw material formula used in this example was: 75 kg of polyvinyl alcohol film waste, 20 kg of water, 8 kg of corn starch, 1 kg of dimethyl silicone oil, and 1 kg of Tween 80.
[0065] Example 4
[0066] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that the raw material formula used in this example was: 60 kg of polyvinyl alcohol film waste, 30 kg of water, 5 kg of corn starch, 3 kg of dimethyl silicone oil, and 1 kg of Tween 80.
[0067] Example 5
[0068] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that the raw material formula used in this example was: 80 kg of polyvinyl alcohol film waste, 15 kg of water, 15 kg of corn starch, 0.5 kg of dimethyl silicone oil, and 2 kg of Tween 80.
[0069] Example 6
[0070] Polyvinyl alcohol film waste recycled particles are produced according to the method of Example 1, except that in the production method of this example, the temperature of the screw extrusion in step (3) is 60°C.
[0071] Example 7
[0072] Polyvinyl alcohol film waste recycled particles are produced according to the method of Example 1, except that in the production method of this example, the temperature of the screw extrusion in step (3) is 70°C.
[0073] Example 8
[0074] Polyvinyl alcohol film waste recycled particles are produced according to the method of Example 1, except that in the production method of this example, the temperature of the screw extrusion in step (3) is 80°C.
[0075] Example 9
[0076] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that in the production method of this example, the temperature of the screw extrusion in step (3) was 95°C.
[0077] Example 10
[0078] The polyvinyl alcohol film waste recycled particles are produced according to the method of Example 1, except that in this example, the model of the polyvinyl alcohol film waste is 1788, the degree of polymerization of polyvinyl alcohol is 1700, and the degree of alcoholysis is 88%.
[0079] Comparative Example 1
[0080] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that the raw material formula used in this comparative example did not contain dimethyl silicone oil, that is, the raw material formula used in this comparative example was: 70 kg of polyvinyl alcohol film waste, 20 kg of water, 8 kg of corn starch, and 1 kg of Tween 80.
[0081] Comparative Example 2
[0082] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that the raw material formula used in this comparative example did not contain Tween 80, that is, the raw material formula used in this comparative example was: 70 kg of polyvinyl alcohol film waste, 20 kg of water, 8 kg of corn starch, and 1 kg of dimethyl silicone oil.
[0083] Comparative Example 3
[0084] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that the raw material formula used in this comparative example did not contain corn starch, that is, the raw material formula used in this comparative example was: 70 kg of polyvinyl alcohol film waste, 20 kg of water, 1 kg of dimethyl silicone oil, and 1 kg of Tween 80.
[0085] Comparative Example 4
[0086] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that the raw material formula used in this comparative example did not contain water, that is, the raw material formula used in this comparative example was: 70 kg of polyvinyl alcohol film waste, 8 kg of corn starch, 1 kg of dimethyl silicone oil, and 1 kg of Tween 80.
[0087] Comparative Example 5
[0088] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that in the raw material formula used in this comparative example, an equal amount of propylene glycol was used to replace the water in Example 1, that is, the raw material formula used in this comparative example was: 70 kg of polyvinyl alcohol film waste, 20 kg of propylene glycol, 8 kg of corn starch, 1 kg of dimethyl silicone oil, and 1 kg of Tween 80.
[0089] Comparative Example 6
[0090] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that in the production method of this comparative example, the temperature of the screw extrusion in step (3) was 50°C.
[0091] Comparative Example 7
[0092] Polyvinyl alcohol film waste recycled particles were produced according to the method of Example 1, except that in the production method of this comparative example, the temperature of the screw extrusion in step (3) was 105°C.
[0093] Experimental example
[0094] The regenerated particles prepared in Examples 1-10 and Comparative Examples 1-7 were respectively taken, and the average diameter, appearance, shape and color of each regenerated particle were respectively detected. The results are shown in Table 1.
[0095] Table 1 The average diameter, appearance, shape and color test results of each regenerated particle
[0096]
[0097]
[0098] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for producing recycled particles from polyvinyl alcohol film waste, characterized in that: The production method comprises the following steps: Mixing the polyvinyl alcohol film waste fragments with water to obtain an intermediate material; The intermediate material is mixed with starch, a release agent and an emulsifier, and dispersed evenly to obtain a material to be extruded; The material to be extruded is screw extruded under negative pressure exhaust conditions, and cut after cooling, wherein the temperature of the screw extrusion is 60° C. to 95° C.
2. The production method according to claim 1, characterized in that In parts by weight, the waste polyvinyl alcohol film fragments, the water, the starch, the release agent and the emulsifier are used in a ratio of (60-80): (15-30): (5-15): (0.5-3): (1-2); Optionally, the waste polyvinyl alcohol film fragments, the water, the starch, the release agent and the emulsifier are used in a ratio of 75:20:8:1:
1.
3. The production method according to claim 1 or 2, characterized in that: In the polyvinyl alcohol film waste fragments, the polymerization degree of polyvinyl alcohol is 500-2400, and the alcoholysis degree is 86%-99%.
4. The production method according to any one of claims 1 to 3, characterized in that The starch comprises at least one of corn starch, sweet potato starch, cassava starch, oxidized starch, cross-linked starch and acid-modified starch; Optionally, the starch is corn starch.
5. The production method according to any one of claims 1 to 4, characterized in that The release agent is a water-soluble release agent, including at least one of dimethyl silicone oil, modified silicone oil, hydrogenated silicone oil, emulsified silicone oil and amino silicone oil; Optionally, the release agent is water-soluble dimethyl silicone oil.
6. The production method according to any one of claims 1 to 5, characterized in that The emulsifier comprises at least one of Tween 80, Tween 60, Tween 20, Tween 85, Span 80 and Span 6; Optionally, the emulsifier is Tween 80.
7. The production method according to any one of claims 1 to 6, characterized in that The diameter of the polyvinyl alcohol film waste fragments is 2 mm to 3 mm.
8. A polyvinyl alcohol film waste recycled particles, characterized in that: The polyvinyl alcohol film waste recycled particles are produced by the production method described in any one of claims 1 to 7.
9. Use of the recycled particles from polyvinyl alcohol film waste according to claim 8 in the preparation of polyvinyl alcohol film.
10. A polyvinyl alcohol film, characterized in that: The polyvinyl alcohol film is prepared using the polyvinyl alcohol film waste recycled particles described in claim 8.