Online aging method of wire rod for large-specification high-strength steel strand

Through the online aging method, including slow cooling of cast billet stacking and Steyrmo air-cooled line cooling technology, the problems of natural long ageing and brittle fracture of the coil strips for high-strength steel strands are solved, and high strength and high stability are achieved The production of steel strands meets the needs of continuous production.

CN118957225AActive Publication Date: 2024-11-15PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP +1

Patent Information

Application Number
CN202411171033.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The strips for large-scale high-strength steel strands have brittle fracture problems during natural aging treatment, resulting in low production efficiency and unstable product quality. The strips without aging treatment have low cross-sectional shrinkage rate, which is prone to surface defects.

Method used

The online aging method is adopted, including slow cooling of cast billet stacking, Steyrmo air-cooled line cooling technology after rolling, waste heat insulation on the PF transport chain, and slow cooling pits. Through phased cooling process and insulation control, the Plastic stability of the strip.

Benefits of technology

The plastic stabilization of the high-strength steel stranded coils without natural aging has been achieved. The tensile strength is between 1280 and 1320MPa, and the cross-sectional surface shrinkage rate is 30% to 40%, which meets the demand for continuous production, reduces the wire breakage rate and improves the The strength and stability of finished steel strands.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of steel rolling, and discloses an online aging method for a wire rod for a large-specification high-strength steel strand. The technological process comprises the steps of tundish hydrogen determination, casting blank stacking and slow cooling, casting blank heating, high-wire rolling, spinning, heat preservation after stelmor wire phase change, coil collection, PF conveying chain heat preservation, finishing, packaging and weighing, and heat preservation in a slow cooling pit to obtain a wire rod, in the heat preservation process after stelmor wire phase change, the initial speed of a roller bed is 0.56 m / s and is increased by 0.01 m / s section by section, and the initial speed of the roller bed is increased by 0.01 m / s section by section. The heat preservation process is carried out in stages, and the first stage is that the temperature ranges from 890 + / -10 DEG C to 650 + / -10 DEG C, the second stage is that the temperature ranges from 650 + / -10 DEG C to 590 + / -10 DEG C, the third stage is that the temperature ranges from 590 + / -10 DEG C to 500 + / -10 DEG C, the fourth stage is that the temperature ranges from 450 + / -10 DEG C to 300 + / -10 DEG C, and the fifth stage is that the temperature ranges from 200 + / -10 DEG C to the room temperature. According to the method, the technical problems that the natural aging period of the wire rod for the large-specification high-strength steel strand is long, brittle fracture is likely to happen in the using process, and continuous production cannot be met are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel rolling, and in particular to an online aging method for wire rods for large-size high-strength steel strands. Background Art

[0002] For high-strength steel strands, the production process without vacuum treatment is often adopted, so as to achieve cost reduction and efficiency improvement for steel enterprises. However, when the hydrogen content in molten steel is tested by the intermediate hydrogen determination equipment, [H] is often 3-5ppm. On the one hand, it is easy to cause hydrogen-induced cracks in steel. In addition, due to the high sensitivity of crack defects in high-carbon steel wire rods, users often experience a sudden increase in wire breakage rate during use, which seriously affects the quality and production efficiency of steel strand products. On the other hand, the cross-sectional shrinkage rate of wire rods that have not been aged is extremely low. The gas in the steel gathers near the non-metallic inclusions or crack defects in the wire rods, embrittles the wire rods, and is more likely to form surface defects during transportation, which introduces more defects before the wire rods are used. The general practice is to place the wire rods in a natural environment for a period of time (the natural environment temperature is low and the time is longer), and the gas and residual stress in the wire rods are continuously released, so that the plasticity of the wire rods can be stabilized at ≥30%. The duration varies with the fluctuation of the gas content in different furnaces, resulting in problems such as difficulty in determining shipment, product backlog, and difficulty in capital circulation.

[0003] Therefore, there is a need in the prior art for an online aging method for wire rods for large-size high-strength steel strands. Summary of the invention

[0004] In view of this, the purpose of an embodiment of the present invention is to propose an online aging method for wire rods for large-size high-strength steel strands, by means of slow cooling of wire rod ingots for steel strands, Stelmor air-cooling line controlled cooling process after rolling, waste heat insulation on PF transport chain and slow cooling in slow cooling pit, a wire rod for high-strength steel strands with plasticity stabilized without natural aging treatment is obtained, which solves the technical problems that the natural aging period of wire rods for large-size high-strength steel strands is long, brittle fracture is prone to occur during use and cannot meet the requirements of continuous production.

[0005] Based on the above purpose, the embodiment of the present invention provides an online aging method for wire rods for large-size high-strength steel strands, and the process flow includes: hydrogen determination in the tundish → slow cooling of the ingot stacking → heating of the ingot → high-speed wire rolling → spinning → insulation after the Stelmor line phase change → coiling → PF transport chain insulation → finishing, packaging, weighing → entering the slow cooling pit for insulation to obtain the wire rod. During the insulation process after the Stelmor line phase change, the initial speed of the roller is 0.56m / s, and increases by 0.01m / s step by step. The insulation process is carried out in stages, including: The first stage: the temperature is 890±10℃~650±10℃, the fan is turned on, the cooling speed is controlled to 8~10℃ / s, and the heat preservation cover is opened; The second stage: the temperature is 650±10℃~590±10℃, the cooling speed is controlled at 3~5℃ / s, and the heat preservation cover is opened; The third stage: the temperature is 590±10℃~500±10℃, the fan is turned off, the insulation cover is closed, the cooling speed is controlled to 0.5~1.5℃ / s, and the residence time in the insulation cover is ≥90s.

[0006] In some embodiments, the chemical composition of the wire rod includes, by mass fraction: C: 0.84% ​​to 0.87%, Si: 0.50% to 0.60%, Mn: 0.60% to 0.80%, P≤0.015%, S≤0.010%, Cr: 0.25% to 0.35%, Cu≤0.20%, Ni≤0.10%, N≤40ppm, O≤12ppm, H≤1.0ppm, and the rest is Fe and unavoidable impurities.

[0007] In some embodiments, in the slow cooling process of the ingot stacking, the temperature is controlled at 350-450° C., and the stacking time is controlled at 32-48 hours.

[0008] In some embodiments, during the tundish hydrogen determination process, the hydrogen content in the molten steel is monitored in real time, and the hydrogen content does not exceed 5.0 ppm.

[0009] In some embodiments, in the billet heating process, the uniform heating temperature of the billet is 1080-1150° C., and the heating time t=(0.7-1.2)H, wherein H is the billet thickness in mm, and the heating time t is in min.

[0010] In some embodiments, the cast strand is heated using a walking beam furnace.

[0011] In some embodiments, after the high-speed wire rolling process, water cooling control is performed in a post-rolling water tank so that the wire drawing temperature of the wire rod is controlled to be 890±10°C.

[0012] In some embodiments, the maximum flow rate of the fan in the first stage is 200,000 m 3 / h, the maximum flow rate of the fan in the second stage is 155,000m 3 / h.

[0013] In some embodiments, the temperature of the wire rod entering the PF chain insulation corridor after double-core rod coiling is controlled at 450°C±10°C, the residence time in the PF chain insulation corridor is ≥600s, and the temperature of the wire rod in the finishing process is controlled at 300°C±10°C.

[0014] In some embodiments, the temperature of the wire rod entering the slow cooling pit is 200°C ± 10°C, and the slow cooling time is 22 to 24 hours.

[0015] The present invention has at least the following beneficial technical effects: The present invention aims at the common technical problem of long aging period of wire rod for large-size high-strength steel strand and provides an online aging method for wire rod for large-size high-strength steel strand. Through slow cooling of wire rod ingots stacking for steel strand, Stelmor air-cooling line controlled cooling process after rolling, waste heat insulation on PF transport chain and slow cooling in wire rod slow cooling pit, a wire rod for high-strength steel strand with plasticity stabilized without natural aging treatment is obtained, which solves the technical problem that wire rod for large-size high-strength steel strand has long natural aging period and is prone to brittle fracture during use and cannot meet the requirements of continuous production. The wire rod is cooled to below 50°C and then subjected to mechanical property test. The tensile strength of the wire rod is in the range of 1280~1320MPa, and the cross-sectional area reduction is 30%~40%. It does not change with time, reaching the level of artificial aging test and realizing online aging plastic recovery of the wire rod. The grades of network cementite and martensite in the organization are both ≤1.0. After being sent to users, it can be directly dephosphorized and drawn. The wire breakage rate per 100 tons is ≤1.0 times, and the strength of the finished steel strand is in the range of 1990~2050MPa. DETAILED DESCRIPTION

[0016] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in conjunction with specific embodiments.

[0017] The terms "including" and "having" and any variations thereof in the specification and claims of the present invention are intended to cover non-exclusive inclusions; the terms "first", "second", etc. in the specification and claims of the present invention are used to distinguish different objects rather than to describe a specific order. "Multiple" means two or more, unless otherwise clearly and specifically defined.

[0018] In addition, reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0019] The present invention provides an online aging method for wire rods for large-size high-strength steel strands, and the process flow includes: hydrogen determination in tundish → slow cooling of billet stacking → heating of billet → high-speed wire rolling → spinning → heat preservation after Stelmor line phase change → coiling → heat preservation of PF transport chain → finishing, packaging, weighing → heat preservation in slow cooling pit to obtain wire rods. During the heat preservation process after the Stelmor line phase change, the initial speed of the roller is 0.56 m / s, and increases by 0.01 m / s step by step. The heat preservation process is carried out in stages, including: The first stage: the temperature is 890±10℃~650±10℃, the fan is turned on, the cooling speed is controlled to 8~10℃ / s, and the heat preservation cover is opened; The second stage: the temperature is 650±10℃~590±10℃, the cooling speed is controlled at 3~5℃ / s, and the heat preservation cover is opened; The third stage: the temperature is 590±10℃~500±10℃, the fan is turned off, the insulation cover is closed, the cooling speed is controlled to 0.5~1.5℃ / s, and the residence time in the insulation cover is ≥90s.

[0020] Furthermore, the chemical composition (mass fraction) of the wire rod for large-size steel strands is: C 0.84%-0.87%, Si 0.50%-0.60%, Mn 0.60%-0.80%, P≤0.015%, S≤0.010%, Cr 0.25%-0.35%, Cu≤0.20%, Ni≤0.10%, N≤40ppm, O≤12ppm, H≤1.0ppm; the rest is Fe and unavoidable impurities; The specification of high-strength wire rod is Φ14.0mm, which is used to prepare steel strands of 1960MPa and above.

[0021] The control of N and O in the chemical composition is achieved through the quality control of raw and auxiliary materials in the converter smelting + refining process and the control of the deoxidation process, ensuring a high degree of cleanliness of the molten steel.

[0022] The H content in the chemical composition cannot exceed 5.0ppm, otherwise hydrogen-induced cracks are easily formed in the ingot, and the plasticity of the wire rod cannot be improved by reducing the gas content in the steel through online aging methods.

[0023] Furthermore, hydrogen is determined in the tundish: during the continuous casting process, the hydrogen content in the molten steel is monitored to control the hydrogen release in the subsequent slow cooling process of the ingot.

[0024] Furthermore, the ingots are stacked and slowly cooled: the continuous casting square billets are cut to a fixed length, and then stacked and slowly cooled. The stacking slow cooling temperature is controlled at 350-450°C, and the stacking time is controlled at 32-48 hours.

[0025] Furthermore, the wire rod before the phase transformation of the Stelmore air-cooled line is obtained by heating the ingot in a walking-beam heating furnace, high-speed wire rolling and spinning by a spinning machine. The ingot is heated at an average temperature of 1080-1150°C, and the heating time t= (0.7-1.2)H, where H is the ingot thickness in mm and the heating time t is in min. The spinning temperature of the wire rod is controlled at 890±10°C by water cooling in a water tank after rolling.

[0026] Furthermore, the temperature of the wire rod entering the PF chain insulation corridor after double-core rod coiling is controlled at 450℃±10℃, the residence time in the PF chain insulation corridor is ≥600s, and the temperature of the wire rod in the finishing process is controlled at 300℃±10℃.

[0027] Furthermore, the wire rod finishing, packaging and weighing processes are carried out in a closed environment, and wind blowing and cooling the wire rod is strictly prohibited, which further prolongs the release time of residual stress, nitrogen, hydrogen, etc. during high temperature to increase the cross-sectional shrinkage rate and achieve online aging of the wire rod residual heat.

[0028] Furthermore, the wire rod is kept warm in a slow cooling pit: the wire rod temperature entering the slow cooling pit is 200°C ± 10°C, and the slow cooling time is 24h.

[0029] After the wire rod is cooled to room temperature, the mechanical properties are tested. The tensile strength of the wire rod ranges from 1280 to 1320 MPa, and the cross-sectional area reduction is 30% to 40%. It does not change with time, reaching the level of artificial aging inspection and realizing online aging plastic recovery of the wire rod. The grades of network cementite and martensite in the organization are both ≤1.0. After being sent to users, it can be directly dephosphorized and drawn. The wire breakage rate per 100 tons is ≤1.0 times, and the strength of the finished steel strand is between 1990 and 2050 MPa.

[0030] The present invention will be further explained below in conjunction with specific embodiments.

[0031] Example 1 A metal products company adopts the technology of the present invention to prepare Φ14.0mm specification 1960MPa grade wire rod for steel strand, and its production process is as follows: hydrogenation in the tundish → slow cooling of the ingot stacking → heating of the ingot walking beam heating furnace → rolling by the high-speed wire unit → wire laying machine → insulation after phase change of the Stelmor wire → coiling → long-term insulation of the PF transport chain → finishing, packaging, weighing → insulation of the wire rod in the slow cooling pit.

[0032] The chemical composition (mass fraction) of the wire rod is: C: 0.86%, Si: 0.52%, Mn: 0.75%, P: 0.011%, S: 0.009%, Cr 0.30%, Cu: 0.04%, Ni: 0.03%, N: 36ppm, O 10ppm, H 0.8ppm, and the rest are Fe and unavoidable impurities.

[0033] The H content of molten steel in the tundish is set to 4.5ppm.

[0034] Ingot stacking and slow cooling: The continuous casting square billets are cut to a fixed length and then stacked and slowly cooled. The stacking slow cooling temperature is controlled at 350~450℃ and the stacking time is controlled at 40h.

[0035] The wire rod of the Stelmore air-cooled wire before phase transformation is obtained by heating the ingot in a walking beam heating furnace, high-speed wire rolling and spinning on a spinning machine. The ingot specification is 200mm×200mm, the uniform heating temperature during ingot heating is 1080~1150℃, the heating time is 210min, and the spinning temperature of the wire rod is controlled at 890±10℃ through water cooling control in a water tank after rolling.

[0036] The air cooling control parameters of the phase change process are: the initial roller speed is 0.56m / s, and increases by 0.01m / s step by step. (1) 890±10℃ to 650±10℃, with a maximum flow rate of 200,000m 3 / h fan, control the cooling rate to 8℃ / s to avoid the precipitation of pro-eutectoid cementite, and open the heat preservation cover at this time; (2) 650±10℃ to 590±10℃, use the maximum flow rate of 155,000m 3 / h fan, control the cooling rate to 4℃ / s, so that the high-temperature wire rod is supercooled to the sorbitization temperature range, fully sorbitized, and the transformation time is extended. At this time, the insulation cover is opened; (3) 590±10℃ to 500±10℃, turn off the fan, close the insulation cover, control the cooling rate to 1.0℃ / s, and the residence time in the insulation cover is 96s.

[0037] After coiling, the temperature of the wire rod entering the PF chain insulation corridor is controlled at 450℃±10℃, the residence time in the PF chain insulation corridor is 600s, and the temperature of the wire rod in the finishing process is controlled at 300℃±10℃.

[0038] The wire rod finishing, packaging and weighing processes are carried out in a closed environment. It is strictly forbidden to cool the wire rod by wind. This will further extend the release time of residual stress, nitrogen, hydrogen, etc. during high temperature, increase the cross-sectional shrinkage rate, and achieve online aging of residual heat of the wire rod.

[0039] Insulation in the slow cooling pit: The wire rod temperature entering the slow cooling pit is 200℃±10℃, and the slow cooling time is 24h.

[0040] After the wire rod is cooled to room temperature, the mechanical properties are tested. The tensile strength of the wire rod is in the range of 1280MPa, and the cross-sectional area reduction is 36%. It does not change with time, reaching the level of artificial aging inspection and realizing the online aging plastic recovery of the wire rod. The grades of network cementite and martensite in the organization are both 1.0. After being sent to the user, it can be directly dephosphorized and drawn. The wire breakage rate is 1.0 times per 100 tons, and the strength of the finished steel strand is 2030MPa.

[0041] Example 2 The chemical composition (mass fraction) of the wire rod is: C: 0.85%, Si: 0.55%, Mn: 0.80%, P: 0.008%, S: 0.008%, Cr: 0.35%, Cu: 0.05%, Ni: 0.03%, N: 40ppm, O: 12ppm, H: 1.0ppm, and the rest are Fe and unavoidable impurities.

[0042] The H content of molten steel in the tundish was set to 3.0ppm.

[0043] Ingot stacking and slow cooling: The continuous casting billets are cut to size and then stacked and slowly cooled. The stacking slow cooling temperature is controlled at 350~450℃ and the stacking time is controlled at 32h.

[0044] The wire rod of the Stelmore air-cooled wire before phase transformation is obtained by heating the ingot in a walking beam heating furnace, high-speed wire rolling and spinning on a spinning machine. The ingot specification is 200mm×200mm, the uniform heating temperature during ingot heating is 1080~1150℃, the heating time is 140min, and the spinning temperature of the wire rod is controlled at 890±10℃ through water cooling control in a water tank after rolling.

[0045] The air cooling control parameters of the phase change process are: the initial roller speed is 0.56m / s, and increases by 0.01m / s step by step. (1) 890±10℃ to 650±10℃, with a maximum flow rate of 200,000m 3 / h, control the cooling rate to 9℃ / s to avoid the precipitation of pro-eutectoid cementite, and open the heat preservation cover at this time; (2) 650±10℃ to 590±10℃, use the maximum flow rate of 155,000m 3 / h fan, control the cooling rate to 3℃ / s, so that the high-temperature wire rod is supercooled to the sorbitization temperature range, fully sorbitized, and the transformation time is extended. At this time, the insulation cover is opened; (3) 590±10℃ to 500±10℃, turn off the fan, close the insulation cover, control the cooling rate to 1.5℃ / s, and the residence time in the insulation cover is 96s.

[0046] After coiling, the temperature of the wire rod entering the PF chain insulation corridor is controlled at 450℃±10℃, the residence time in the PF chain insulation corridor is 610s, and the temperature of the wire rod in the finishing process is controlled at 300℃±10℃.

[0047] The wire rod finishing, packaging and weighing processes are carried out in a closed environment. It is strictly forbidden to cool the wire rod by wind. This will further extend the release time of residual stress, nitrogen, hydrogen, etc. during high temperature, increase the cross-sectional shrinkage rate, and achieve online aging of residual heat of the wire rod.

[0048] Insulation in the slow cooling pit: The wire rod temperature entering the slow cooling pit is 200℃±10℃, and the slow cooling time is 24h.

[0049] After the wire rod is cooled to room temperature, the mechanical properties are tested. The tensile strength of the wire rod is in the range of 1300MPa, and the cross-sectional area reduction is 40%. It does not change with time, reaching the level of artificial aging test and realizing online aging plastic recovery of the wire rod. The grades of network cementite and martensite in the organization are both level 0. After being sent to the user, it can be directly dephosphorized and drawn. The wire breakage rate is 0.7 times per 100 tons, and the strength of the finished steel strand is 2050MPa.

[0050] Example 3 The chemical composition (mass fraction) of the wire rod is: C: 0.87%, Si: 0.50%, Mn: 0.60%, P: 0.015%, S: 0.010%, Cr: 0.25%, Cu: 0.04%, Ni: 0.03%, N: 31ppm, O: 8ppm, H: 0.5ppm, and the rest are Fe and unavoidable impurities.

[0051] The H content of molten steel in the tundish was set to 5.0ppm.

[0052] Ingot stacking and slow cooling: The continuous casting square billets are cut to a fixed length and then stacked and slowly cooled. The stacking slow cooling temperature is controlled at 350~450℃ and the stacking time is controlled at 48h.

[0053] The wire rod before the phase change of the Stelmore air-cooled wire is obtained by heating the ingot in a walking beam heating furnace, high-speed wire rolling and spinning on a spinning machine. The ingot specification is 200mm×200mm, the uniform heating temperature during ingot heating is 1080~1150℃, the heating time is 240min, and the spinning temperature of the wire rod is controlled at 890±10℃ through water cooling control in a water tank after rolling.

[0054] The air cooling control parameters of the phase change process are: the initial roller speed is 0.56m / s, and increases by 0.01m / s step by step. (1) 890±10℃ to 650±10℃, with a maximum flow rate of 200,000m 3 / h fan, control the cooling rate to 10℃ / s to avoid the precipitation of pro-eutectoid cementite, and open the heat preservation cover at this time; (2) 650±10℃ to 590±10℃, use the maximum flow rate of 155,000m 3 / h fan, control the cooling rate to 4℃ / s, so that the high-temperature wire rod is supercooled to the sorbitization temperature range, fully sorbitized, and the transformation time is extended. At this time, the insulation cover is opened; (3) 590±10℃ to 500±10℃, turn off the fan, close the insulation cover, control the cooling rate to 0.5℃ / s, and the residence time in the insulation cover is 96s.

[0055] After coiling, the temperature of the wire rod entering the PF chain insulation corridor is controlled at 450℃±10℃, the residence time in the PF chain insulation corridor is 605s, and the temperature of the wire rod in the finishing process is controlled at 300℃±10℃.

[0056] The wire rod finishing, packaging and weighing processes are carried out in a closed environment. It is strictly forbidden to cool the wire rod by wind. This will further extend the release time of residual stress, nitrogen, hydrogen, etc. during high temperature, increase the cross-sectional shrinkage rate, and achieve online aging of residual heat of the wire rod.

[0057] Insulation in the slow cooling pit: The wire rod temperature entering the slow cooling pit is 200℃±10℃, and the slow cooling time is 24h.

[0058] After the wire rod is cooled to room temperature, the mechanical properties are tested. The tensile strength of the wire rod is in the range of 1320MPa, and the cross-sectional area reduction is 30%. It does not change with time, reaching the level of artificial aging inspection and realizing online aging plastic recovery of the wire rod. The grades of network cementite and martensite in the organization are both 0.5. After being sent to the user, it can be directly dephosphorized and drawn. The wire breakage rate is 0.5 times per 100 tons, and the strength of the finished steel strand is 1990MPa.

[0059] Example 4 The chemical composition (mass fraction) of the wire rod is: C: 0.84%, Si: 0.60%, Mn: 0.71%, P: 0.012%, S: 0.008%, Cr: 0.28%, Cu: 0.04%, Ni: 0.03%, N: 39ppm, O: 11ppm, H: 0.6ppm, and the rest is Fe and unavoidable impurities.

[0060] The H content of molten steel in the tundish was 4.2ppm.

[0061] Ingot stacking and slow cooling: The continuous casting square billets are cut to a fixed length and then stacked and slowly cooled. The stacking slow cooling temperature is controlled at 350~450℃ and the stacking time is controlled at 40h.

[0062] The wire rod of the Stelmore air-cooled wire before phase transformation is obtained by heating the ingot in a walking beam heating furnace, high-speed wire rolling and spinning on a spinning machine. The ingot specification is 200mm×200mm, the uniform heating temperature during ingot heating is 1080~1150℃, the heating time is 220min, and the spinning temperature of the wire rod is controlled at 890±10℃ through water cooling control in a water tank after rolling.

[0063] The air cooling control parameters of the phase change process are: the initial roller speed is 0.56m / s, and increases by 0.01m / s step by step. (1) 890±10℃ to 650±10℃, with a maximum flow rate of 200,000m 3 / h fan, control the cooling rate to 9℃ / s to avoid the precipitation of pro-eutectoid cementite, and open the heat preservation cover at this time; (2) 650±10℃ to 590±10℃, use the maximum flow rate of 155,000m 3 / h fan, control the cooling rate to 5℃ / s, so that the high-temperature wire rod is supercooled to the sorbitization temperature range, fully sorbitized, and the transformation time is extended. At this time, the insulation cover is opened; (3) 590±10℃ to 500±10℃, turn off the fan, close the insulation cover, control the cooling rate to 0.8℃ / s, and the residence time in the insulation cover is 96s.

[0064] After coiling, the temperature of the wire rod entering the PF chain insulation corridor is controlled at 450℃±10℃, the residence time in the PF chain insulation corridor is 650s, and the temperature of the wire rod in the finishing process is controlled at 300℃±10℃.

[0065] The wire rod finishing, packaging and weighing processes are carried out in a closed environment. It is strictly forbidden to cool the wire rod by wind. This will further extend the release time of residual stress, nitrogen, hydrogen, etc. during high temperature, increase the cross-sectional shrinkage rate, and achieve online aging of residual heat of the wire rod.

[0066] Insulation in the slow cooling pit: The wire rod temperature entering the slow cooling pit is 200℃±10℃, and the slow cooling time is 24h.

[0067] After the wire rod is cooled to room temperature, the mechanical properties are tested. The tensile strength of the wire rod is in the range of 1310MPa, and the cross-sectional area reduction is 35%. It does not change with time, reaching the level of artificial aging inspection and realizing the online aging plastic recovery of the wire rod. The network cementite in the structure is level 1.0 and the martensite is level 0.5. After being sent to the user, it can be directly dephosphorized and drawn. The wire breakage rate is 0.8 times per 100 tons, and the strength of the finished steel strand is 2000MPa.

[0068] The above are exemplary embodiments disclosed in the present invention, but it should be noted that various changes and modifications may be made without departing from the scope disclosed in the embodiments of the present invention as defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.

[0069] It should be understood that, as used herein, the singular forms "a", "an" are intended to include the plural forms as well, unless the context clearly supports an exception. It should also be understood that, as used herein, "and / or" refers to any and all possible combinations including one or more of the associated listed items.

[0070] The serial numbers of the embodiments disclosed in the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.

[0071] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the above embodiments of the present invention, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.

Claims

1. An online aging method for large-size high-strength steel strand wire rods. It is characterized in that The process includes: hydrogen setting in tundish → slow cooling of billet stacking → heating of billet → high-speed wire rolling → spinning → insulation after phase change on Stelmor line → coiling → insulation on PF transport chain → finishing, packaging, weighing → insulation in slow cooling pit to obtain wire rod. During the insulation process after phase change on Stelmor line, the initial speed of the roller is 0.56m / s, and increases by 0.01m / s step by step. The insulation process is carried out in stages, including: The first stage: the temperature is 890±10℃~650±10℃, the fan is turned on, the cooling speed is controlled to 8~10℃ / s, and the heat preservation cover is opened; The second stage: the temperature is 650±10℃~590±10℃, the cooling speed is controlled at 3~5℃ / s, and the heat preservation cover is opened; The third stage: the temperature is 590±10℃~500±10℃, the fan is turned off, the heat preservation cover is closed, the cooling speed is controlled to 0.5~1.5℃ / s, and the residence time in the heat preservation cover is ≥90s; The fourth stage: the temperature is 450±10℃~300±10℃, and the insulation is completed in the insulation corridor; The fifth stage: The temperature is 200℃±10℃~room temperature, and insulation is completed in the aging pit.

2. The online aging method for wire rods for large-size high-strength steel strands according to claim 1, It is characterized in that Measured by mass fraction, the chemical composition of the wire rod includes: C: 0.84%~0.87%, Si: 0.50%~0.60%, Mn: 0.60%~0.80%, P≤0.015%, S≤0.010%, Cr: 0.25%~0.35%, Cu≤0.20%, Ni≤0.10%, N≤40ppm, O≤12ppm, H≤1.0ppm, and the rest is Fe and unavoidable impurities.

3. The online aging method for wire rods for large-size high-strength steel strands according to claim 1, It is characterized in that After coiling, the temperature of the wire rod entering the PF chain insulation corridor is controlled at 450℃±10℃, the residence time in the PF chain insulation corridor is ≥600s, and the temperature of the wire rod in the finishing process is controlled at 300℃±10℃.

4. The online aging method for wire rods for large-size high-strength steel strands according to claim 1, It is characterized in that In the ingot stacking slow cooling process, the temperature is controlled at 350-450° C., and the stacking time is controlled at 32-48 hours.

5. The online aging method for wire rods for large-size high-strength steel strands according to claim 1, It is characterized in that In the tundish hydrogen determination process, the hydrogen content in the molten steel is monitored in real time, and the hydrogen content does not exceed 5.0 ppm.

6. The online aging method for wire rods for large-size high-strength steel strands according to claim 1, It is characterized in that In the casting billet heating process, the casting billet is heated at an average temperature of 1080-1150° C., and the heating time t=(0.7-1.2)H, wherein H is the casting billet thickness in mm, and the heating time t is in min.

7. The online aging method for wire rods for large-size high-strength steel strands according to claim 1, It is characterized in that The casting is heated by a walking beam heating furnace.

8. The online aging method for wire rods for large-size high-strength steel strands according to claim 1, It is characterized in that After the high-speed wire rolling process, water cooling control is performed in a post-rolling water tank so that the wire drawing temperature of the wire rod is controlled to be 890±10°C.

9. The online aging method for wire rods for large-size high-strength steel strands according to claim 1, It is characterized in that The maximum flow rate of the fan in the first stage is 200,000 m 3 / h, the maximum flow rate of the fan in the second stage is 155,000m 3 / h.

10. The online aging method for wire rods for large-size high-strength steel strands according to claim 1, It is characterized in that The temperature of the wire rod entering the slow cooling pit is 200°C ± 10°C, and the slow cooling time is 22~24h.

Citation Information

Patent Citations

  • Stelmor controlled cooling method for 55SiCrA spring steel wire rod

    CN102747210A

  • Method for controlling internal defects in production of coil bar for welding wire

    CN110834168A

  • Large-specification high-carbon chromium bearing steel hot-rolled wire rod and high-speed wire rod production method thereof

    CN112355054A

  • Production method for reducing aging time of high-carbon wire rod

    CN114918250A

  • Steel wire rod for 1420MPa-grade delayed brittle fracture-resistant prestressed steel bar and production method of steel wire rod

    CN117165861A

Cited By

  • High-conductivity ultra-low carbon steel wire rod and preparation method thereof

    CN120967229A