Sawtooth-shaped interface stainless steel coating material and preparation method thereof
By performing surface heating, embossing, stress removal annealing and plating on the aluminum alloy substrate, a sawtooth interface structure is formed, which solves the problem of low interface bonding strength of aluminum matrix/stainless steel coating and realizes high-performance coating Preparation, suitable for engineering applications.
Patent Information
- Application Number
- CN202410960853.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-15
AI Technical Summary
The aluminum matrix/stainless steel coating interface bonding strength is low, limiting its use in engineering applications.
Using aluminum alloy as the substrate, serrated protrusions, stress annealing, evaporation plating nickel layer and plasma spraying stainless steel coating are prepared by surface heating and imprinting to form a serrated interface structure to improve interface bonding strength .
It significantly improves the interface bonding strength between the aluminum matrix and the stainless steel coating, enhances the wear resistance and service life of the coating, and is suitable for the engineering field of high-performance coatings.
Smart Images

Figure BDA0004950215360000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating material preparation, and in particular to a sawtooth interface stainless steel coating material and a preparation method thereof. Background Art
[0002] Aluminum substrate stainless steel coating is a surface treatment technology that deposits a stainless steel layer on the surface of aluminum or aluminum alloy. This coating technology aims to improve the properties of the aluminum substrate, such as hardness, wear resistance, corrosion resistance, etc. The stainless steel coating can significantly improve the surface hardness of the aluminum substrate and make it have better wear resistance. Stainless steel itself has good corrosion resistance. Using it as a coating can further enhance the corrosion resistance of the aluminum substrate and extend its service life. The stainless steel coating can give the aluminum substrate a more beautiful appearance, such as a silvery-white luster. The stainless steel coating can reduce the reflection of the aluminum substrate surface and reduce light pollution.
[0003] The coating is mainly composed of austenite phase, with the remainder being a small amount of ferrite phase and oxide. As the coating thickness increases, the porosity and oxygen content in the coating may increase, but the fracture stiffness of the coating will be proportional to its thickness. Aluminum-based stainless steel coatings are widely used in aerospace, automobile manufacturing, machinery manufacturing and other fields to improve the wear resistance, corrosion resistance and service life of parts.
[0004] Aluminum-based stainless steel coating is an effective surface treatment technology that can significantly improve the performance of aluminum substrates and broaden their application areas. By selecting appropriate coating preparation technology and optimizing process parameters, aluminum-based stainless steel coatings with good performance can be obtained.
[0005] Aluminum-based stainless steel coatings have the characteristics of high elastic modulus, low density, and high specific strength. They are widely used in the manufacture of light armored tank wheels, aerospace power unit components, and automotive engine turbochargers. However, the bonding properties of aluminum-based stainless steel coatings limit their use in engineering practice. Therefore, how to improve the bonding ability of aluminum-based stainless steel coatings has become the focus of current research in this field. Summary of the invention
[0006] The present invention aims at the problem that the existing aluminum substrate / stainless steel coating interface has low bonding strength, which limits its engineering application, and provides a sawtooth interface stainless steel coating material and a preparation method thereof.
[0007] In order to achieve the above object, the present invention is implemented by adopting the following technical scheme:
[0008] In a first aspect, the present invention provides a sawtooth interface stainless steel coating material and a preparation method thereof, comprising the following steps:
[0009] An aluminum alloy substrate is used as a substrate, a surface of the substrate to be sprayed is heated, and a sawtooth-shaped protrusion is prepared on the heated surface of the substrate by an imprinting method, and then the sawtooth-shaped protrusion is subjected to stress relief annealing to obtain an aluminum alloy substrate to be sprayed;
[0010] A nickel layer is plated on the spraying surface of the aluminum alloy substrate by an evaporation coating method, and a stainless steel coating is sprayed on the coating surface by a plasma spraying method to obtain a sawtooth interface stainless steel coating material.
[0011] As a further improvement of the present invention, the aluminum alloy substrate is hard aluminum or wrought aluminum.
[0012] As a further improvement of the present invention, the surface heating of the substrate to be sprayed comprises:
[0013] The substrate surface is heated by conduction heat transfer between the heating plate and the substrate, 3 to 5 layers of aluminum foil are laid between the heating plate and the substrate, the heating plate temperature is 340 to 370°C, and the heating time is 45 to 62 seconds.
[0014] As a further improvement of the present invention, the embossing method for preparing serrated protrusions on the heated surface of the substrate is processed using an embossing mold. During the processing, the pressing pressure is 75 to 87 MPa and the pressure is maintained for 24 to 28 seconds; the stress relief annealing temperature is 310 to 330°C and the time is 15 to 20 minutes.
[0015] As a further improvement of the present invention, the stamping mold is made of high-temperature steel material with a thickness of 5 to 8 mm and a surface density of 6 to 10 through holes of 0.5×0.5 mm2 distributed per square centimeter.
[0016] As a further improvement of the present invention, the method of coating a nickel layer on the surface to be sprayed of the aluminum alloy substrate to be sprayed by an evaporation coating method comprises:
[0017] Using nickel as the evaporation source, at 5×10 -4 ~2×10 -3 A nickel layer is plated on the surface to be sprayed of the substrate under the conditions of vacuum degree, evaporation rate of 0.8 to 1.1 nanometers per second and 62 to 68 minutes.
[0018] As a further improvement of the present invention, the method of spraying a stainless steel coating on the surface of the coating by a plasma spraying method comprises:
[0019] Plasma spraying uses 110-130 micron stainless steel powder as raw material, the spraying distance is 35-45 mm, the argon gas flow rate is 40-46 liters per minute, and the coating thickness is 87-95 microns.
[0020] In a second aspect, the present invention provides a serrated interface stainless steel coating material, which is prepared by the preparation method described in any one of claims 1 to 7.
[0021] As a further improvement of the present invention, the prepared stainless steel coating material has a sawtooth interface structure.
[0022] As a further improvement of the present invention, the prepared stainless steel coating material has a serrated interface structure, the coating and interface porosity is ≤0.6%, the coating / substrate interface bonding strength is ≥65MPa, the coating surface hardness is ≥480HV1, and the sliding friction test wear is ≤1.1 micrograms per square centimeter per hour.
[0023] Compared with the prior art, the present invention has the following characteristics and advantages:
[0024] The invention first uses aluminum alloy as a substrate, uses a heating plate device to perform surface heating on a surface to be sprayed, uses an embossing method to prepare sawtooth protrusions on the heated surface of the substrate, then performs stress relief annealing on the sawtooth protrusions, and then uses an evaporation plating method to plate a nickel layer on the surface to be sprayed of the substrate, and finally uses a plasma spraying method to spray a stainless steel coating on the coating surface; wherein hard aluminum or forged aluminum is used as the substrate, the fatigue resistance and toughness of the substrate can be guaranteed, and the service life of the material can be extended; the embossing technology uses a softened substrate surface treated at high temperature and neatly arranged embossing mold through holes to realize controllable preparation of the sawtooth protrusions on the surface to be sprayed of the substrate; an aluminum foil is added between the heating plate and the substrate to facilitate uniform heating of the entire substrate surface; and the nickel plating treatment of the sawtooth protrusions on the substrate surface is used to further strengthen the interface bonding performance between the coating and the substrate.
[0025] The stainless steel coating material prepared by the invention has a sawtooth interface structure, a coating and interface porosity of ≤0.6%, a coating / substrate interface bonding strength of ≥65MPa, a coating surface hardness of ≥480HV1, and a sliding friction test wear amount of ≤1.1 micrograms per square centimeter per hour. DETAILED DESCRIPTION
[0026] In order to make the method problems, method solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0027] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0028] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple.
[0029] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0030] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0031] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass in the embodiment description of the present application can be μg, mg, g, kg and other mass units known in the chemical industry.
[0032] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of method features indicated. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0033] The first object of the present invention is to provide a method for preparing a sawtooth interface stainless steel coating material, comprising:
[0034] An aluminum alloy substrate is used as a substrate, a surface of the substrate to be sprayed is heated, and a sawtooth-shaped protrusion is prepared on the heated surface of the substrate by an imprinting method, and then the sawtooth-shaped protrusion is subjected to stress relief annealing to obtain an aluminum alloy substrate to be sprayed;
[0035] A nickel layer is plated on the spraying surface of the aluminum alloy substrate by an evaporation coating method, and a stainless steel coating is sprayed on the coating surface by a plasma spraying method to obtain a sawtooth interface stainless steel coating material.
[0036] The serrated interface stainless steel coating material and its preparation method proposed in the present invention significantly improve the interface bonding strength between the aluminum substrate and the stainless steel coating through a series of careful process steps, thereby overcoming the problems of low interface bonding strength and poor wear resistance between the aluminum substrate and the stainless steel coating in the prior art. The principle is as follows:
[0037] With hard aluminum or forged aluminum as the substrate, the substrate is heated by conduction heat transfer between the heating plate and the substrate, so that the substrate surface reaches a certain temperature, providing ideal conditions for subsequent embossing and coating preparation.
[0038] Using a specific high-temperature steel mold, a sawtooth-shaped protrusion is prepared on the heated surface of the substrate. This structure can increase the contact area between the substrate and the coating and improve the interface bonding strength.
[0039] The substrate after embossing is subjected to stress relief annealing treatment to eliminate the residual stress inside the material and further improve the bonding strength of the coating.
[0040] A nickel layer is plated on the surface of the substrate as a transition layer between the stainless steel coating and the aluminum substrate to enhance the compatibility and bonding between the two.
[0041] Using plasma spraying technology, the stainless steel coating is sprayed on the nickel layer to form a uniform and dense coating structure.
[0042] The interface bonding strength between the aluminum substrate and the stainless steel coating is significantly improved by surface heating, embossing and stress relief annealing of the substrate, as well as the transition effect of the nickel layer. The stainless steel coating has excellent wear resistance and can effectively extend the service life of the material. Each process step in the method can be precisely controlled by adjusting the parameters, ensuring the quality and performance stability of the coating. The optimized process steps and parameter settings make the preparation method have high process stability and repeatability, which is convenient for industrial production. The serrated interface stainless steel coating material has high interface bonding strength and wear resistance, and is suitable for various engineering fields that require high-performance coatings.
[0043] The present invention successfully prepares a serrated interface stainless steel coating material with strong interface bonding and excellent wear resistance through a series of careful process steps and parameter optimization, providing an effective solution for related engineering fields. The specific solution includes the following steps:
[0044] 1) Using hard aluminum or forged aluminum as a substrate, heating the substrate surface by conduction heat transfer between a heating plate and the substrate, laying 3 to 5 layers of aluminum foil between the heating plate and the substrate, the heating plate temperature is 340 to 370° C., the heating time is 45 to 62 seconds, and then using an embossing technique to prepare a sawtooth protrusion on the heated surface of the substrate, the embossing mold is a high-temperature steel material with a thickness of 5 to 8 mm and a surface density of 6 to 10 through holes of 0.5×0.5 square millimeters distributed per square centimeter, the pressing pressure is 75 to 87 MPa, the pressure is maintained for 24 to 28 seconds, and then the sawtooth protrusion is subjected to stress relief annealing at a temperature of 310 to 330° C. for 15 to 20 minutes to obtain an aluminum alloy substrate to be sprayed;
[0045] 2) Using nickel as the evaporation source, the evaporation plating method was used to deposit 5×10 -4 ~2×10 -3 A nickel layer is plated on the surface to be sprayed of the substrate under the conditions of vacuum degree, evaporation rate of 0.8 to 1.1 nanometers per second and 62 to 68 minutes, and finally a stainless steel coating is sprayed on the plated surface by a plasma spraying method. 110 to 130 micron stainless steel powder is selected as the raw material, the spraying distance is 35 to 45 mm, the argon gas flow rate is 40 to 46 liters per minute, the coating thickness is 87 to 95 microns, and finally a serrated interface stainless steel coating material is obtained.
[0046] Improving the bonding strength of the aluminum substrate / stainless steel coating interface through a series of technologies such as surface heating, embossing, stress relief annealing, evaporation coating and spraying is the key means to solve the above engineering problems.
[0047] In the process of preparing stainless steel coating materials, the present invention aims at the problem that the existing aluminum substrate / stainless steel coating has low interface bonding strength and limits its engineering application. Through a series of technologies such as surface heating, embossing, stress relief annealing, evaporation plating and spraying, the relationship between substrate type, surface heating process, embossing process, stress relief annealing process, nickel plating process, spraying process and stainless steel coating interface bonding and friction performance is studied, that is, for stainless steel coating materials, the best substrate type, surface heating process, embossing process, stress relief annealing process, nickel plating process and spraying process to maintain high interface bonding and friction performance. This method has strong controllability, strong process stability and repeatability, and can achieve strong interface bonding and excellent wear resistance of stainless steel coating.
[0048] The interface bonding and friction properties of the stainless steel coating materials prepared in the following examples are shown in Table 1.
[0049] Example 1
[0050] 1) Using hard aluminum as a substrate, the substrate surface is heated by conduction heat transfer between a heating plate and the substrate, 3 layers of aluminum foil are laid between the heating plate and the substrate, the heating plate temperature is 340°C, the heating time is 45 seconds, and then a serrated protrusion is prepared on the heated surface of the substrate by embossing technology. The embossing mold is a high-temperature steel material with a thickness of 5 mm and a surface density of 6 through holes of 0.5×0.5 square millimeters distributed per square centimeter. The pressing pressure is 75 MPa, the pressure is maintained for 24 seconds, and then the serrated protrusion is subjected to stress relief annealing at a temperature of 310°C for 15 minutes to obtain an aluminum alloy substrate to be sprayed;
[0051] 2) Using nickel as the evaporation source, the evaporation plating method was used to deposit 5×10 -4 A nickel layer is plated on the surface to be sprayed of the substrate under vacuum, an evaporation rate of 0.8 nanometers per second and 62 minutes. Finally, a stainless steel coating is sprayed on the plated surface by a plasma spraying method. 110 micron stainless steel powder is used as the raw material, the spraying distance is 35 mm, the argon gas flow rate is 40 liters per minute, the coating thickness is 87 microns, and finally a serrated interface stainless steel coating material is obtained.
[0052] Example 2
[0053] 1) Using forged aluminum as a substrate, the substrate surface is heated by conduction heat transfer between a heating plate and the substrate, 5 layers of aluminum foil are laid between the heating plate and the substrate, the heating plate temperature is 370° C., the heating time is 62 seconds, and then a serrated protrusion is prepared on the heated surface of the substrate by embossing technology. The embossing mold is a high-temperature steel material with a thickness of 8 mm and a surface density of 10 through holes of 0.5×0.5 mm2 distributed per square centimeter. The pressing pressure is 87 MPa, the pressure is maintained for 28 seconds, and then the serrated protrusion is subjected to stress relief annealing at a temperature of 330° C. for 20 minutes to obtain an aluminum alloy substrate to be sprayed;
[0054] 2) Using nickel as the evaporation source, the evaporation plating method was used to deposit 2×10 -3 A nickel layer is plated on the surface to be sprayed of the substrate under vacuum, an evaporation rate of 1.1 nanometers per second and 68 minutes. Finally, a stainless steel coating is sprayed on the plated surface by a plasma spraying method. 130 micron stainless steel powder is used as the raw material, the spraying distance is 45 mm, the argon gas flow rate is 46 liters per minute, the coating thickness is 95 microns, and finally a serrated interface stainless steel coating material is obtained.
[0055] Example 3
[0056] 1) Using hard aluminum as a substrate, the substrate surface is heated by conduction heat transfer between a heating plate and the substrate, 4 layers of aluminum foil are laid between the heating plate and the substrate, the heating plate temperature is 350° C., the heating time is 49 seconds, and then a serrated protrusion is prepared on the heated surface of the substrate by embossing technology. The embossing mold is a high-temperature steel material with a thickness of 6 mm and a surface density of 8 through holes of 0.5×0.5 square millimeters distributed per square centimeter. The pressing pressure is 77 MPa, the pressure is maintained for 26 seconds, and then the serrated protrusion is subjected to stress relief annealing at a temperature of 320° C. for 17 minutes to obtain an aluminum alloy substrate to be sprayed;
[0057] 2) Using nickel as the evaporation source, the evaporation plating method was used at 7×10 -4 A nickel layer is plated on the surface to be sprayed of the substrate under vacuum, an evaporation rate of 0.9 nanometers per second and 64 minutes. Finally, a stainless steel coating is sprayed on the plated surface by a plasma spraying method. 120-micron stainless steel powder is used as the raw material, the spraying distance is 38 mm, the argon gas flow rate is 43 liters per minute, the coating thickness is 92 microns, and finally a serrated interface stainless steel coating material is obtained.
[0058] Example 4
[0059] 1) Using forged aluminum as a substrate, the substrate surface is heated by conduction heat transfer between a heating plate and the substrate, 4 layers of aluminum foil are laid between the heating plate and the substrate, the heating plate temperature is 360° C., the heating time is 45 seconds, and then a serrated protrusion is prepared on the heated surface of the substrate by embossing technology. The embossing mold is a high-temperature steel material with a thickness of 8 mm and a surface density of 6 through holes of 0.5×0.5 mm2 distributed per square centimeter. The pressing pressure is 87 MPa, the pressure is maintained for 28 seconds, and then the serrated protrusion is subjected to stress relief annealing at a temperature of 330° C. for 20 minutes to obtain an aluminum alloy substrate to be sprayed;
[0060] 2) Using nickel as the evaporation source, the evaporation plating method was used to deposit 2×10 -3 A nickel layer is plated on the surface to be sprayed of the substrate under vacuum, an evaporation rate of 1.1 nanometers per second and 67 minutes. Finally, a stainless steel coating is sprayed on the plated surface by a plasma spraying method. 130 micron stainless steel powder is used as the raw material, the spraying distance is 45 mm, the argon gas flow rate is 45 liters per minute, the coating thickness is 95 microns, and finally a serrated interface stainless steel coating material is obtained.
[0061] The performance parameters of the stainless steel coating materials prepared in Examples 1 to 4 are shown in Table 1:
[0062] Table 1
[0063]
[0064] It can be concluded from the above table that the stainless steel coating material prepared by the present invention has a sawtooth interface structure, the coating and interface porosity ≤0.6%, the coating / substrate interface bonding strength ≥65MPa, the coating surface hardness ≥480HV1, and the sliding friction test wear amount ≤1.1 micrograms per square centimeter per hour.
[0065] Example 5
[0066] 1) Using hard aluminum as the substrate, the substrate surface is heated by conduction heat transfer between the heating plate and the substrate, 4 layers of aluminum foil are laid between the heating plate and the substrate, the heating plate temperature is 350° C., the heating time is 46 seconds, and then a serrated protrusion is prepared on the heated surface of the substrate by embossing technology. The embossing mold is a high-temperature steel material with a thickness of 5 mm and a surface density of 7 through holes of 0.5×0.5 square millimeters distributed per square centimeter. The pressing pressure is 76 MPa, the pressure is maintained for 25 seconds, and then the serrated protrusion is subjected to stress relief annealing at a temperature of 315° C. for 16 minutes to obtain an aluminum alloy substrate to be sprayed;
[0067] 2) Using nickel as the evaporation source, the evaporation plating method was used to deposit 6×10 -4 A nickel layer is plated on the surface to be sprayed of the substrate under vacuum, an evaporation rate of 0.9 nanometers per second and 65 minutes. Finally, a stainless steel coating is sprayed on the plated surface by a plasma spraying method. 115-micron stainless steel powder is used as the raw material, the spraying distance is 36 mm, the argon gas flow rate is 42 liters per minute, the coating thickness is 88 microns, and finally a serrated interface stainless steel coating material is obtained.
[0068] Example 6
[0069] 1) Using forged aluminum as a substrate, the substrate surface is heated by conduction heat transfer between a heating plate and the substrate, 4 layers of aluminum foil are laid between the heating plate and the substrate, the heating plate temperature is 355° C., the heating time is 61 seconds, and then a serrated protrusion is prepared on the heated surface of the substrate by embossing technology. The embossing mold is a high-temperature steel material with a thickness of 6.5 mm and a surface density of 9 through holes of 0.5×0.5 mm2 distributed per square centimeter. The pressing pressure is 86 MPa, the pressure is maintained for 27 seconds, and then the serrated protrusion is subjected to stress relief annealing at a temperature of 325° C. for 20 minutes to obtain an aluminum alloy substrate to be sprayed;
[0070] 2) Using nickel as the evaporation source, the evaporation plating method was used to deposit 1×10 -3 A nickel layer is plated on the surface to be sprayed of the substrate under vacuum, an evaporation rate of 1.0 nanometers per second and 65 minutes. Finally, a stainless steel coating is sprayed on the plated surface by a plasma spraying method. 120 micron stainless steel powder is used as the raw material, the spraying distance is 42 mm, the argon gas flow rate is 43 liters per minute, the coating thickness is 93 microns, and finally a serrated interface stainless steel coating material is obtained.
[0071] Example 7
[0072] 1) Using hard aluminum as a substrate, the substrate surface is heated by conduction heat transfer between a heating plate and the substrate, 4 layers of aluminum foil are laid between the heating plate and the substrate, the heating plate temperature is 360° C., the heating time is 50 seconds, and then a serrated protrusion is prepared on the heated surface of the substrate by embossing technology. The embossing mold is a high-temperature steel material with a thickness of 6.5 mm and a surface density of 9 through holes of 0.5×0.5 mm2 distributed per square centimeter. The pressing pressure is 78 MPa, the pressure is maintained for 25 seconds, and then the serrated protrusion is subjected to stress relief annealing at a temperature of 322° C. for 16 minutes to obtain an aluminum alloy substrate to be sprayed;
[0073] 2) Using nickel as the evaporation source, the evaporation plating method was used to deposit 8×10 -4 A nickel layer is plated on the surface to be sprayed of the substrate under vacuum, an evaporation rate of 0.8 nanometers per second and 65 minutes. Finally, a stainless steel coating is sprayed on the plated surface by a plasma spraying method. 116-micron stainless steel powder is used as the raw material, the spraying distance is 39 mm, the argon gas flow rate is 42 liters per minute, the coating thickness is 88 microns, and finally a serrated interface stainless steel coating material is obtained.
[0074] Example 8
[0075] 1) Using forged aluminum as a substrate, the substrate surface is heated by conduction heat transfer between a heating plate and the substrate, 4 layers of aluminum foil are laid between the heating plate and the substrate, the heating plate temperature is 355° C., the heating time is 47 seconds, and then a serrated protrusion is prepared on the heated surface of the substrate by embossing technology. The embossing mold is a high-temperature steel material with a thickness of 6 mm and a surface density of 9 through holes of 0.5×0.5 mm2 distributed per square centimeter. The pressing pressure is 77 MPa, the pressure is maintained for 26 seconds, and then the serrated protrusion is subjected to stress relief annealing at a temperature of 320° C. for 15 minutes to obtain an aluminum alloy substrate to be sprayed;
[0076] 2) Using nickel as the evaporation source, the evaporation plating method was used to deposit 2×10 -3 A nickel layer is plated on the surface to be sprayed of the substrate under vacuum, an evaporation rate of 0.9 nanometers per second and 66 minutes. Finally, a stainless steel coating is sprayed on the plated surface by a plasma spraying method. 125-micron stainless steel powder is used as the raw material, the spraying distance is 38 mm, the argon gas flow rate is 45 liters per minute, the coating thickness is 94 microns, and finally a serrated interface stainless steel coating material is obtained.
[0077] Examples 5 to 8 prepared stainless steel coating materials for performance testing, and it can be concluded that the stainless steel coating materials prepared by the present invention have a sawtooth interface structure, a coating and interface porosity ≤ 0.6%, a coating / substrate interface bonding strength ≥ 65MPa, a coating surface hardness ≥ 480HV1, and a sliding friction test wear loss ≤ 1.1 micrograms per square centimeter per hour. The problem of low bonding strength of the existing aluminum substrate / stainless steel coating interface, which limits its engineering application, is solved.
[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a sawtooth interface stainless steel coating material, characterized in that: include: An aluminum alloy substrate is used as a substrate, a surface of the substrate to be sprayed is heated, and a sawtooth-shaped protrusion is prepared on the heated surface of the substrate by an imprinting method, and then the sawtooth-shaped protrusion is subjected to stress relief annealing to obtain an aluminum alloy substrate to be sprayed; A nickel layer is plated on the spraying surface of the aluminum alloy substrate by an evaporation coating method, and a stainless steel coating is sprayed on the coating surface by a plasma spraying method to obtain a sawtooth interface stainless steel coating material.
2. The method for preparing the sawtooth interface stainless steel coating material according to claim 1, characterized in that: The aluminum alloy substrate is hard aluminum or forged aluminum.
3. The method for preparing the sawtooth interface stainless steel coating material according to claim 1, characterized in that: The method of heating the surface of the substrate to be sprayed comprises: The substrate surface is heated by conduction heat transfer between the heating plate and the substrate, 3 to 5 layers of aluminum foil are laid between the heating plate and the substrate, the heating plate temperature is 340 to 370°C, and the heating time is 45 to 62 seconds.
4. The method for preparing the sawtooth interface stainless steel coating material according to claim 1, characterized in that: The embossing method is used to prepare the sawtooth protrusions on the heated surface of the substrate by using an embossing mold. During the processing, the pressing pressure is 75-87MPa and the pressure is maintained for 24-28 seconds; the stress relief annealing temperature is 310-330°C and the time is 15-20 minutes.
5. The method for preparing the sawtooth interface stainless steel coating material according to claim 1, characterized in that: The stamping mold is made of high-temperature steel material with a thickness of 5 to 8 mm and a surface density of 6 to 10 through holes of 0.5×0.5 mm2 distributed per square centimeter.
6. The method for preparing the sawtooth interface stainless steel coating material according to claim 1, characterized in that: The method of coating a nickel layer on the surface of the aluminum alloy substrate to be sprayed by an evaporation coating method comprises: Using nickel as the evaporation source, at 5×10 -4 ~2×10 -3 A nickel layer is plated on the surface to be sprayed of the substrate under the conditions of vacuum degree, evaporation rate of 0.8 to 1.1 nanometers per second and 62 to 68 minutes.
7. The method for preparing the sawtooth interface stainless steel coating material according to claim 1, characterized in that: The method of spraying a stainless steel coating on the surface of the coating by a plasma spraying method comprises: Plasma spraying uses 110-130 micron stainless steel powder as raw material, the spraying distance is 35-45 mm, the argon gas flow rate is 40-46 liters per minute, and the coating thickness is 87-95 microns.
8. A sawtooth interface stainless steel coating material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 7.
9. The sawtooth interface stainless steel coating material according to claim 8, characterized in that: The prepared stainless steel coating material has a sawtooth interface structure.
10. The sawtooth interface stainless steel coating material according to claim 8, characterized in that: The coating and interface porosity of the prepared stainless steel coating material is ≤0.6%, the coating / substrate interface bonding strength is ≥65MPa, the coating surface hardness is ≥480HV1, and the sliding friction test wear amount is ≤1.1 micrograms per square centimeter per hour.