Resourceful treatment method of hematite
By using a phased acid leaching method to control the amount of acid, the problems of high acid consumption and cost caused by high-concentration acid-enhanced leaching were solved, achieving efficient leaching and separation of elements such as iron and nickel in hematite and reducing processing costs.
Patent Information
- Application Number
- CN202411044028.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Existing hematite processing technologies involve high-concentration acid-enhanced leaching, which leads to high acid consumption and complex subsequent pH adjustments, increasing costs.
A staged leaching method is adopted. In the first leaching process, the acid amount is controlled to be less than the theoretical amount of acid required to leach all the iron in the hematite. In the second leaching process, the acid amount is controlled to be greater than or equal to the theoretical amount of acid required to leach all the iron in the first leaching residue. The acid amount is controlled in stages to reduce acid consumption and regulate pH value.
It effectively reduces acid consumption and lowers costs, while fully leaching and separating elements such as iron and nickel from hematite, thus achieving resource utilization.
Smart Images

Figure CN118957247A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of hematite processing, and in particular to a method for resource processing of hematite. Background Art
[0002] The main component of hematite is Fe2O3, and it may also contain various elements such as nickel and precious metals. Due to its high iron content, hematite is often used as a raw material for refining iron and other elements.
[0003] At present, the common hematite treatment process includes the use of high-concentration acid enhanced leaching method to directly leach various elements such as iron in hematite. However, when using high-concentration acid enhanced leaching, a large amount of acid is often required, resulting in a high residual acid content in the resulting leachate. The pH value of the leachate needs to be adjusted to meet the use requirements, which not only increases the acid consumption, but also increases the complexity of the treatment process, resulting in high costs. Summary of the invention
[0004] The present application provides a method for resource processing of hematite, which can fully leach various elements such as iron in the hematite, and can also reduce acid consumption and reduce costs.
[0005] The embodiment of the present application provides a resource processing method for hematite, comprising the following steps: a first leaching process, subjecting the hematite to a first acid leaching, and then obtaining a first leaching residue and a first leaching solution containing trivalent iron ions and nickel ions through solid-liquid separation; a second leaching process, subjecting the first leaching residue to a second acid leaching, and then obtaining a second leaching residue containing precious metals and a second leaching solution containing trivalent iron ions and nickel ions through solid-liquid separation; wherein the amount of acid used in the first leaching process is less than the theoretical amount of acid required to leach all the iron in the hematite, and the amount of acid used in the second leaching process is greater than or equal to the theoretical amount of acid required to leach all the iron in the first leaching residue.
[0006] The resource recovery treatment method provided in the embodiment of the present application adds acid to leach hematite in the first leaching process, and controls the amount of acid used to be less than the theoretical amount of acid required to leach all the iron in the hematite. At this time, part of the iron, nickel and other elements that may be contained in the hematite can be leached to obtain a first leachate containing trivalent iron ions and nickel ions, and the remaining iron and nickel in the hematite enter the first leaching residue; then, in the second leaching process, acid is added to leach the first leaching residue, and the amount of acid used is controlled to be greater than or equal to the theoretical amount of acid required to leach all the iron in the first leaching residue. At this time, all the iron, nickel and other elements that may be contained in the first leaching residue can be leached as much as possible to obtain a second leachate containing trivalent iron ions and nickel ions, and the precious metals and other elements that are difficult to be leached in the hematite are enriched in the second leaching residue, thereby realizing the separation of the iron, nickel, precious metals and other elements in the hematite.
[0007] Therefore, according to the resource recovery treatment method provided in the embodiment of the present application, by leaching the hematite in stages, the amount of acid required for leaching can be controlled in stages, which is beneficial to reduce acid consumption and regulate the pH value of the leachate, thereby reducing costs. At the same time, it can also fully leach and separate various elements such as iron and nickel in the hematite.
[0008] In some embodiments of the present application, the amount of acid used in the first leaching step is 0.4 to 0.9 times the theoretical amount of acid required to leach all the iron in the hematite.
[0009] In some embodiments of the present application, the amount of acid used in the second leaching step is 1.0 to 2.0 times the theoretical amount of acid required to completely leach out the iron in the first leaching slag.
[0010] In some embodiments of the present application, the first leaching process includes: a pretreatment process, in which the hematite is crushed and / or subjected to a first slurrying process to obtain a pre-treated material; a first acid leaching process, in which the pre-treated material is subjected to a first acid leaching, and then solid-liquid separation is performed to obtain a first leaching residue and a first leaching solution containing trivalent iron ions and nickel ions.
[0011] In some embodiments of the present application, the particle size of the hematite after crushing is less than or equal to 80 mesh, preferably less than or equal to 150 mesh.
[0012] In some embodiments of the present application, the first slurrying treatment includes mixing water and hematite to make slurry.
[0013] In some embodiments of the present application, the acid used in the first acid leaching step includes at least one of sulfuric acid and hydrochloric acid, preferably sulfuric acid.
[0014] In some embodiments of the present application, the acid leaching temperature of the first acid leaching step is 90°C-100°C.
[0015] In some embodiments of the present application, the acid leaching time of the first acid leaching step is 8h-10h.
[0016] In some embodiments of the present application, the pH value of the first leachate is 0-0.5.
[0017] In some embodiments of the present application, the second leaching process includes: an intermediate treatment process, in which the first leaching residue is subjected to a washing treatment and / or a second slurry treatment to obtain an intermediate treated material; a second acid leaching process, in which the intermediate treated material is subjected to a second acid leaching, and then solid-liquid separation is performed to obtain a second leaching residue containing precious metals and a second leachate containing trivalent iron ions and nickel ions.
[0018] In some embodiments of the present application, the washing treatment includes washing the first leached residue with water to obtain a first washing liquid and a first washed residue, wherein the first washed residue is used as the intermediate processed material or is used as the intermediate processed material after the second slurry treatment.
[0019] In some embodiments of the present application, the intermediate treatment process further includes mixing the first post-washing liquid with the first leachate to dilute the first leachate.
[0020] In some embodiments of the present application, the volume of water used for the washing treatment is 30%-40% of the volume of the first leachate.
[0021] In some embodiments of the present application, the second slurrying treatment includes mixing water with the first leached residue to make slurry.
[0022] In some embodiments of the present application, the acid used in the second acid leaching step is at least one of sulfuric acid and hydrochloric acid, preferably sulfuric acid.
[0023] In some embodiments of the present application, the acid leaching temperature of the second acid leaching step is 70°C-100°C.
[0024] In some embodiments of the present application, the acid leaching time of the second acid leaching step is 4h-8h.
[0025] In some embodiments of the present application, the resource recovery method further includes: a circulation step of recycling the second leachate back to the first leaching step, so that the second leachate is mixed with the hematite for a first acid leaching.
[0026] In some embodiments of the present application, the resource recovery method further includes: a washing process, washing the second leaching residue to obtain a second washing liquid and a second washing residue, and the second washing liquid is recycled back to the first leaching process, so that the second washing liquid is mixed with the hematite for the first acid leaching.
[0027] In some embodiments of the present application, the washing process uses water washing.
[0028] In some embodiments of the present application, the volume of water used in the washing process is 30%-40% of the volume of the second leachate.
[0029] In some embodiments of the present application, the resource recovery method further includes: a reduction purification step, in which the first leaching solution is mixed with a nickel intermediate for reaction, and then a purified solution containing ferrous ions and nickel ions is obtained by solid-liquid separation.
[0030] In some embodiments of the present application, the amount of the nickel intermediate is 1.2 to 1.8 times the theoretical amount required to completely reduce the trivalent iron ions in the first leachate.
[0031] In some embodiments of the present application, the mixing reaction temperature is 60°C-70°C.
[0032] In some embodiments of the present application, the mixing reaction time is 2h-4h.
[0033] In some embodiments of the present application, the pH value of the purification solution is 1.0-2.5.
[0034] In some embodiments of the present application, the nickel intermediate product includes nickel matte.
[0035] In some embodiments of the present application, the particle size of the nickel matte is less than or equal to 100 mesh, preferably less than or equal to 200 mesh.
[0036] Additional technical solutions and advantages of the present application will be partially given in the following description, and partially become apparent from the following description, or be understood through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0038] Figure 1 A flow chart of a method for recycling hematite provided in some embodiments of the present application;
[0039] Figure 2 A flow chart of a method for recycling hematite provided in some embodiments of the present application;
[0040] Figure 3 A flow chart of a method for recycling hematite provided in some embodiments of the present application;
[0041] Figure 4 A flow chart of a method for recycling hematite provided in some embodiments of the present application;
[0042] Figure 5 A flow chart of a method for recycling hematite provided in some embodiments of the present application;
[0043] Figure 6 A flow chart of a method for resource recovery of hematite provided in some embodiments of the present application. DETAILED DESCRIPTION
[0044] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0045] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0046] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0047] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0048] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0049] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0050] In the present application, hematite refers to an iron oxide mineral, the main component of which is Fe2O3. For example, in some embodiments, the source of hematite can be naturally occurring iron minerals directly taken from nature, or can be hematite slag produced during the leaching and nickel extraction process using high-grade nickel matte as raw material.
[0051] Solid-liquid separation refers to the process of separating solids and liquids, and the method of solid-liquid separation can be any method of separating solids and liquids known in the art. For example, in some embodiments, solid-liquid separation can be performed by centrifugation, tilting, filtration, etc., and the solid-liquid separation herein can be performed with reference to the above methods.
[0052] Precious metals refer to metallic elements such as gold, silver and platinum group metals.
[0053] The theoretical amount of acid is to leach all Fe2O3 to obtain Fe 3+ The required amount of acid, the reactions that occur during the leaching process include: Fe2O3+6H + =2Fe 3+ +3H2O, the theoretical amount of acid required can be calculated by this formula. For example, in some embodiments, the theoretical amount of acid required to completely leach the iron in the hematite or the first leaching residue is to completely leach Fe2O3 in the hematite or the first leaching residue to obtain Fe 3+ The amount of acid required.
[0054] Pure water generally refers to water with a conductivity less than or equal to 10μS / cm, total organic carbon less than or equal to 20mg / L, metal ions (Na, K, Ca, Mg, etc.) less than or equal to 1000μg / L, and other ions (Cl, NO3 - Water with a concentration of less than or equal to 2000 μg / L.
[0055] Nickel intermediate refers to an intermediate product in the nickel smelting process, which contains a certain content of elements such as iron. For example, in some embodiments, the nickel intermediate may be nickel matte, which includes low-grade nickel matte and / or high-grade nickel matte.
[0056] Dry basis refers to the way of expressing the content of a component in wet solid or wet gas based on unit mass of anhydrous solid or dry gas.
[0057] Reference Figure 1 As shown, the embodiment of the present application provides a method for recycling hematite, comprising the following steps:
[0058] S100, a first leaching step, subjecting the hematite to a first acid leaching, and then obtaining a first leaching residue and a first leaching solution containing trivalent iron ions and nickel ions through solid-liquid separation.
[0059] S200, a second leaching step, subjecting the first leaching residue to a second acid leaching, and then obtaining a second leaching residue containing precious metals and a second leaching solution containing trivalent iron ions and nickel ions through solid-liquid separation; wherein the amount of acid used in the first leaching step is less than the theoretical amount of acid required to leach all the iron in the hematite, and the amount of acid used in the second leaching step is greater than or equal to the theoretical amount of acid required to leach all the iron in the first leaching residue.
[0060] The resource recovery treatment method provided in the embodiment of the present application adds acid to leach hematite in the first leaching process, and controls the amount of acid used to be less than the theoretical amount of acid required to leach all the iron in the hematite. At this time, part of the iron, nickel and other elements that may be contained in the hematite can be leached to obtain a first leachate containing trivalent iron ions and nickel ions, and the remaining iron and nickel in the hematite enter the first leaching residue; then, in the second leaching process, acid is added to leach the first leaching residue, and the amount of acid used is controlled to be greater than or equal to the theoretical amount of acid required to leach all the iron in the first leaching residue. At this time, all the iron, nickel and other elements that may be contained in the first leaching residue can be leached as much as possible to obtain a second leachate containing trivalent iron ions and nickel ions, and the precious metals and other elements that are difficult to be leached in the hematite are enriched in the second leaching residue, thereby realizing the separation of the iron, nickel, precious metals and other elements in the hematite.
[0061] Therefore, according to the resource recovery treatment method provided in the embodiment of the present application, by leaching the hematite in stages, the amount of acid required for leaching can be controlled in stages, which is beneficial to reduce acid consumption and regulate the pH value of the leachate, thereby reducing costs. At the same time, it can also fully leach and separate various elements such as iron and nickel in the hematite.
[0062] In some embodiments, the amount of acid used in the first leaching process is 0.4 to 0.9 times the theoretical amount of acid required to leach all the iron in the hematite. If the amount of acid used in the first leaching process is too large, the acid utilization rate is low, the acid consumption is large, and the cost is high; if the amount of acid used in the first leaching process is too small, it is difficult to meet the requirements of preliminary leaching of hematite, affecting the leaching of elements such as iron and nickel. In the embodiment of the present application, the amount of acid used in the first leaching process is controlled within the above-mentioned appropriate range, which can not only improve the utilization rate of the acid, but also effectively leach part of the iron, nickel and other elements that may be contained in the hematite, thereby facilitating the separation of elements such as iron, nickel, and precious metals.
[0063] In some embodiments, the amount of acid used in the second leaching process is 1.0 to 2.0 times the theoretical amount of acid required to leach all the iron in the first leaching residue. If the amount of acid used in the second leaching process is too large, the acid consumption is high and the residual acid content in the second leachate is high. The second leachate needs to be neutralized and the pH value adjusted to meet the use requirements, which is costly; if the amount of acid used in the second leaching process is too small, the leaching of iron, nickel and other elements in the hematite is insufficient. In the embodiment of the present application, the amount of acid used in the second leaching process is controlled within the above-mentioned appropriate range, which can not only save the amount of acid and reduce costs, but also fully leach some of the iron, nickel and other elements in the hematite, so as to facilitate the separation of products containing iron, nickel, precious metals and other elements with higher purity from the hematite.
[0064] Reference Figure 2 As shown, in some embodiments, the first leaching process includes:
[0065] S110, a pre-treatment step, subjecting the hematite to a crushing treatment and / or a first slurry treatment to obtain a pre-treated material.
[0066] S120, a first acid leaching step, subjecting the pre-treated material to a first acid leaching, and obtaining a first leaching residue and a first leaching solution containing trivalent iron ions and nickel ions through solid-liquid separation.
[0067] In the embodiment of the present application, the hematite is crushed before the first acid leaching to make the particle size of the hematite smaller, and the first slurrying treatment of the hematite can initially disperse the hematite to form a slurry, which is conducive to mixing the acid and the hematite as evenly as possible, thereby improving the leaching effect.
[0068] For example, in some embodiments, the crushing process may be to convert the hematite into a powder with a smaller particle size by stirring, extruding, grinding, etc.
[0069] In some embodiments, the particle size of the hematite after crushing is less than or equal to 80 mesh, preferably less than or equal to 150 mesh, which is conducive to sufficient leaching of the hematite.
[0070] In some embodiments, the first slurrying process includes mixing water and hematite to prepare slurry. For example, the first slurrying process may be mixing hematite with pure water to prepare slurry.
[0071] In the first acid leaching step, the leaching rates of trivalent iron ions and nickel ions in the first leachate can be adjusted to be within the range of 40%-90%, preferably 60%-90%, by adjusting appropriate process parameters. This can improve the utilization rate of the acid to reduce the leaching cost, and can also help improve the utilization rate of the acid in the first leaching step.
[0072] In some embodiments, the acid used in the first acid leaching step includes at least one of sulfuric acid and hydrochloric acid, preferably sulfuric acid. Various elements contained in the hematite can be fully leached by sulfuric acid and hydrochloric acid, and the introduction of anionic impurities can be avoided as much as possible, which is conducive to reducing the cost of impurity removal.
[0073] Specifically, taking the acid used in the first acid leaching process as 98% sulfuric acid as an example, the reactions occurring during the acid leaching process include: Fe2O3+6H + =2Fe 3+ +3H2O. If the amount of acid used in the first leaching step is controlled to be 0.4 to 0.9 times the theoretical amount of acid required to leach all the iron in the hematite, the amount of sulfuric acid can be calculated by the following formula: V (98% sulfuric acid) / m 3 =m(Fe) / t÷56×1.5×(0.4-0.9)×98÷98%÷1.84.
[0074] In some embodiments, the acid leaching temperature of the first acid leaching process is 90° C.-100° C. In some embodiments, the acid leaching time of the first acid leaching process is 8 h-10 h. In this embodiment, the acid leaching temperature and time are within the above-mentioned suitable range, which can fully utilize the acid added in the first acid leaching process and effectively leach the iron, nickel and other elements contained in the hematite.
[0075] In some embodiments, the pH value of the first leachate is 0-0.5. If the pH value of the first leachate is too high, it means that the amount of acid used for leaching may be insufficient and the leaching is insufficient; if the pH value of the first leachate is too low, it means that the amount of acid used for leaching is too much and the acid consumption is large. In this embodiment, the amount of acid used for leaching is controlled so that the pH value of the first leachate is within a suitable range, which is conducive to sufficient leaching, and can minimize acid consumption and reduce costs.
[0076] Reference Figure 3 As shown, in some embodiments, the second leaching process includes:
[0077] S210, an intermediate treatment step, performing a washing treatment and / or a second slurry treatment on the first leaching residue to obtain an intermediate treated material.
[0078] S220, a second acid leaching step, wherein the intermediate treated material is subjected to a second acid leaching, and then solid-liquid separation is performed to obtain a second leaching residue containing precious metals and a second leaching solution containing trivalent iron ions and nickel ions.
[0079] In the embodiment of the present application, after washing the first leaching residue before the second acid leaching, the soluble metal ions such as iron ions and nickel ions carried by the first leaching residue can be washed away, so as to prevent the carried soluble metal ions such as iron ions and nickel ions from entering the second acid leaching system and inhibiting the acid leaching reaction, thereby facilitating the full leaching of various elements contained in the first leaching residue. In addition, the second slurrying treatment of the first leaching residue before the second acid leaching can disperse the first leaching residue into slurry, thereby facilitating the acid and the first leaching residue to be mixed as evenly as possible, thereby improving the leaching effect.
[0080] In some embodiments, the washing treatment includes washing the first leached residue with water to obtain a first washed liquid and a first washed residue, wherein the first washed residue is used as an intermediate processed material or as an intermediate processed material after a second slurry treatment. Exemplarily, the washing treatment may be washing the first leached residue with pure water.
[0081] Since the first post-wash liquid may contain a small amount of soluble metal ions such as iron ions and nickel ions, the first post-wash liquid can be mixed with the first leachate to fully recover the washed soluble metal ions. In some embodiments, the intermediate treatment process also includes mixing the first post-wash liquid with the first leachate to dilute the first leachate. In this embodiment, after the first post-wash liquid is mixed with the first leachate, the first leachate can be diluted to facilitate the subsequent further processing of the first leachate to obtain a product containing elements such as iron and nickel, and the soluble metal ions such as iron ions and nickel ions can be fully recovered to facilitate further improvement of the leaching rate of metal elements such as nickel and iron.
[0082] In some embodiments, the volume of water used for washing is 30%-40% of the volume of the first leachate. If the amount of water used for washing is too little, washing is insufficient; if the amount of water is too much, the concentration of elements such as iron and nickel contained in the first leachate after the first wash liquid is mixed with the first leachate is too low, which is not conducive to the subsequent treatment of the first leachate to obtain a product containing elements such as iron and nickel.
[0083] In some embodiments, the second slurrying process includes mixing water with the first leached residue to prepare slurry. For example, the second slurrying process may be mixing the first leached residue with pure water to prepare slurry.
[0084] In some embodiments, the acid used in the second acid leaching step is at least one of sulfuric acid and hydrochloric acid, preferably sulfuric acid. Various elements contained in the first leaching residue can be fully leached by sulfuric acid and hydrochloric acid, and the introduction of anionic impurities can be avoided as much as possible, which is conducive to reducing the cost of impurity removal.
[0085] In some embodiments, the acid leaching temperature of the second acid leaching process is 70° C.-100° C. In some embodiments, the acid leaching time of the second acid leaching process is 4 h-8 h. In this embodiment, the acid leaching temperature and time are within the above-mentioned suitable range, which can fully utilize the acid added in the second acid leaching process and effectively leach the elements such as iron and nickel contained in the first leaching residue.
[0086] Reference Figure 4 As shown, in some embodiments, the resource processing method further includes:
[0087] S300, a circulation process, circulating the second leaching solution back to the first leaching process, so that the second leaching solution is mixed with the hematite for the first acid leaching.
[0088] In the embodiment of the present application, the hematite is first subjected to the first acid leaching, and then the first leaching residue is subjected to the second acid leaching, and the total leaching rate of iron and nickel can reach more than 99%. In addition, the second leachate is recycled and used in the first leaching process. On the one hand, a small amount of acid contained in the second leachate can be used as the base acid for the first acid leaching, thereby improving the acid utilization rate, reducing acid consumption, and reducing costs. On the other hand, the iron, nickel and other elements contained in the second leachate can be gathered into the first leachate through the first leaching process, so as to facilitate the subsequent centralized treatment of the first leachate to obtain products containing iron, nickel and other elements.
[0089] Reference Figure 5 As shown, in some embodiments, the resource processing method further includes:
[0090] S400, a washing process, washing the second leached residue to obtain a second washed liquid and a second washed residue, and the second washed liquid is recycled back to the first leaching process, so that the second washed liquid is mixed with the hematite for the first acid leaching.
[0091] In the embodiment of the present application, washing the second leaching residue can wash away a small amount of soluble metal ions such as iron ions and nickel ions carried by the second leaching residue, so that a second leaching residue containing noble metals with higher purity can be obtained, which is conducive to the subsequent recycling of noble metals. In addition, after the second post-washing liquid is recycled back to the first leaching process, the soluble metal ions such as iron ions and nickel ions contained in the second post-washing liquid can be gathered into the first leaching liquid through the first leaching process, so as to facilitate the subsequent centralized treatment of the first leaching liquid to obtain a product containing elements such as iron and nickel.
[0092] In some embodiments, the washing process uses water washing. Exemplarily, the washing process includes washing the second leached residue with pure water.
[0093] In some embodiments, the volume of water used in the washing process is 30%-40% of the volume of the second leachate, which can fully wash away the soluble metal ions carried by the second leaching residue and reduce the amount of water consumed in washing.
[0094] Reference Figure 6 As shown, in some embodiments, the resource processing method further includes:
[0095] S500, a reduction purification step, mixing the first leaching solution with the nickel intermediate product for reaction, and then performing solid-liquid separation to obtain a purified solution containing ferrous ions and nickel ions.
[0096] In the embodiment of the present application, the first leachate containing ferric ions and nickel ions is mixed with the nickel intermediate for reaction, and the reducing substances contained in the nickel intermediate, such as iron element, are used to react with the ferric ions, so that the ferric ions can be reduced to ferrous ions, thereby obtaining a purified solution containing ferrous ions and nickel ions, and the obtained purified solution can be used in industrial scenarios where ferrous ions and nickel ions are required. In particular, when the acid used for the first acid leaching and the second acid leaching is sulfuric acid, the obtained purified solution is a ferrous sulfate nickel solution, which can be used in the battery field, for example, as a raw material for preparing a precursor of a positive electrode material for a battery.
[0097] In some embodiments, the amount of the nickel intermediate is 1.2 to 1.8 times the theoretical amount required to completely reduce the trivalent iron ions in the first leachate. If the amount of the nickel intermediate is too large, it will cause waste; if the amount of the nickel intermediate is too small, it will be difficult to fully reduce. In the embodiment of the present application, the amount of the nickel intermediate is controlled within the above-mentioned appropriate range, which can not only fully reduce the trivalent iron ions, but also minimize the consumption of the nickel intermediate and reduce costs.
[0098] In some embodiments, the mixed reaction temperature of the first leachate and the nickel intermediate is 60°C-70°C. In some embodiments, the mixed reaction time is 2h-4h. In some embodiments, the pH value of the purified solution is 1.0-2.5. In some embodiments, the particle size of the nickel intermediate is less than or equal to 100 mesh, preferably less than or equal to 200 mesh. By controlling the reaction conditions of the mixed reaction within the above-mentioned appropriate range, it is beneficial to fully convert trivalent iron ions into ferrous ions, thereby obtaining a purified solution containing ferrous ions and nickel ions that meets the requirements.
[0099] For example, in some embodiments, the nickel intermediate product may be low-grade nickel matte. As an intermediate product in the nickel smelting process, low-grade nickel matte mainly consists of nickel, iron sulfide and nickel-iron alloy, and has an extremely low impurity content, which can avoid introducing too many impurities during the reduction process. After the first leaching solution is mixed with the low-grade nickel matte for reaction, the iron element contained in the low-grade nickel matte can be used to reduce the Fe 3+ And increase the concentration of ferrous ions, and the dissolution of low-grade nickel will consume H +And generate nickel ions to increase the nickel ion concentration, while the low-grade nickel matte can replace other impurity ions such as copper ions and chromium ions contained in the first leachate and generate precipitation, thereby removing impurities such as Cu and Cr. In this way, it is possible to extract and transform high-value nickel ferrous sulfate solution from hematite, and nickel iron in the low-grade nickel matte is also extracted, which is conducive to obtaining a higher purity nickel ferrous sulfate solution.
[0100] Specifically, taking nickel intermediate as low matte nickel as an example, the mixed reaction includes: Fe+2Fe 3+ =3Fe 2+ At this time, if the amount of nickel matte is to be controlled to be 1.2 to 1.8 times the theoretical amount required to reduce all the trivalent iron ions in the first leachate to divalent iron ions, the amount of nickel matte can be calculated by the following formula: nickel matte mass m (kg) = Fe content of the first leachate (g / L) × volume of the first leachate (m 3 )÷2×(1.2-1.8)÷Fe content of low nickel matte (%).
[0101] The following examples describe the disclosure of the present application in more detail, and these examples are only used for illustrative purposes, because it is obvious to those skilled in the art that various modifications and variations are made within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on mass, and all reagents and raw materials used in the examples are commercially available or synthesized according to conventional methods, and the instruments used in the examples are commercially available.
[0102] The compositions of hematite and nickel matte used in the following examples and comparative examples are shown in Table 1.
[0103] Table 1. Composition of hematite and nickel matte
[0104]
[0105]
[0106] In the following examples and comparative examples, the calculation methods of leaching rate and slag rate are as follows:
[0107] The iron leaching rate of the first acid leaching step = the mass of iron in the first leaching solution / the mass of iron in the hematite.
[0108] The total iron leaching rate of the first acid leaching and the second acid leaching = the sum of the mass of iron in the first leaching solution and the second leaching solution / the mass of iron in the hematite.
[0109] The nickel leaching rate of the first acid leaching process = the mass of nickel in the first leaching solution / the mass of nickel in the hematite;
[0110] The total nickel leaching rate of the first acid leaching and the second acid leaching = the sum of the mass of nickel in the first leaching solution and the second leaching solution / the mass of nickel in the hematite.
[0111] The slag rate of the first leaching residue (on a dry basis) = the dry basis mass of the first leaching residue / the dry basis mass of hematite.
[0112] The total slag rate (dry basis) of the first acid leaching and the second acid leaching = the dry basis mass of the second leaching slag / the dry basis mass of hematite.
[0113] Example 1
[0114] This embodiment provides a method for recycling hematite, comprising the following steps:
[0115] In the pre-treatment process, the hematite slag and low-grade nickel matte are placed in a vertical mill respectively, and the hematite powder (150 mesh) and low-grade nickel matte powder (100 mesh) are obtained after the abrasive is crushed for standby use. 3 Pure water is used as the base water, 3t of dry hematite powder is added, and slurrying is carried out for 15 minutes.
[0116] In the first acid leaching process, after slurrying, the first leaching tank begins to heat up and add 0.77m 3 The first acid leaching was carried out with 98% concentrated sulfuric acid, the amount of acid added was 0.4 times the theoretical amount of acid required to completely leach the iron in the hematite, the leaching reaction temperature was set at 95°C, the reaction was carried out for 8 hours, and after the reaction was completed, the first leaching residue and the first leachate with a pH value of 0.43 were obtained by filter pressing. The slag rate (dry basis) of the first acid leaching process was 50.22%, and the Fe and Ni leaching rates were 41.17% and 46.72%, respectively.
[0117] In the intermediate treatment process, 4.5m 3 The residue is washed with pure water online, and the filtrate (washing liquid) after filtration is added to the first leaching liquid, and the residue is sent to the second leaching tank. 3.85m 3 Pure water was used as the bottom water, and filter residue (water content 30%) was added and slurried for 15 minutes.
[0118] In the second acid leaching process, after slurrying, the second leaching tank begins to heat up and add 1.93m 3 The second acid leaching was carried out with 98% concentrated sulfuric acid, and the amount of acid added was twice the theoretical amount of acid required to completely leach out the iron in the first leaching residue. The leaching reaction temperature was set to 75°C and the reaction was carried out for 4 hours. After the reaction was completed, the second leaching residue and the second leaching liquid were obtained by filter pressing.
[0119] In the circulation process, the second leachate is circulated back for mixing with hematite to make pulp and perform the first acid leaching.
[0120] In the washing process, the second leaching residue is washed to obtain a second washing liquid and a second washing residue, and the second washing liquid is recycled to the first leaching process so that the second washing liquid is mixed with the hematite for the first acid leaching. 2.7m 3 The slag is washed online with pure water, and the filtrate (washing liquid) after filtration is added to the second leaching liquid and reused together with the hematite for pulping and the first acid leaching. The filter residue (precious metal enriched residue) is packaged and temporarily stored, and can be used for further recovery and extraction of precious metals later. The total residue rate of the first and second acid leaching is 0.85% (dry basis), and the total leaching rates of Fe and Ni are 99.27% and 99.79% respectively.
[0121] In the reduction purification process, 2170 kg of low-matte nickel powder was added to the first leachate, and the amount of low-matte nickel powder added was 1.4 times the theoretical amount required to completely reduce the trivalent iron ions in the first leachate. The reaction temperature was controlled at 65 ° C and the reaction time was 3 hours. After the reaction was completed, the purified liquid with a pH value of 1.16 was obtained by filter pressing. The composition of the purified liquid (ferrous nickel sulfate solution) is shown in Table 2.
[0122] Example 2
[0123] This embodiment provides a method for recycling hematite, comprising the following steps:
[0124] In the pre-treatment process, the hematite slag and low-grade nickel matte are placed in a vertical mill respectively, and the hematite powder (120 mesh) and low-grade nickel matte powder (150 mesh) are obtained after the abrasive is crushed for standby use. 3 Bottom water (0.4m 3 Pure water +11.6m 3 The second leachate, from Example 1), was added with 3 t dry hematite powder and slurried for 15 min.
[0125] In the first acid leaching process, after slurrying, the first leaching tank begins to heat up and 1.74m 3 The first acid leaching was carried out with 98% concentrated sulfuric acid, the amount of acid added was 0.9 times the theoretical amount of acid required to leach all the iron in the hematite, the leaching reaction temperature was set to 95°C, the reaction was carried out for 8 hours, and after the reaction was completed, the first leaching residue and the first leaching solution with a pH value of 0.09 were obtained by filter pressing. The slag rate (dry basis) of the first acid leaching process was 9.89%, and the Fe and Ni leaching rates were 88.66% and 89.85%, respectively.
[0126] In the intermediate treatment process, 4.5m 3 The residue is washed with pure water online, and the filtrate (washing liquid) after filtration is added to the first leaching liquid, and the residue is sent to the second leaching tank. Add 0.85m 3 Pure water was used as the bottom water, and filter residue (water content 30%) was added and slurried for 15 minutes.
[0127] In the second acid leaching process, after slurrying, the second leaching tank begins to heat up and add 0.38m 3 The second acid leaching was carried out with 98% concentrated sulfuric acid, the amount of acid added was 1.2 times the theoretical amount of acid required to completely leach out the iron in the first leaching residue, the leaching reaction temperature was set at 95°C, the reaction was carried out for 8 hours, and after the reaction was completed, the second leaching residue and the second leaching liquid were obtained by filter pressing.
[0128] In the circulation process, the second leachate is circulated back for mixing with hematite to make pulp and perform the first acid leaching.
[0129] In the washing process, the second leaching residue is washed to obtain a second washing liquid and a second washing residue, and the second washing liquid is recycled to the first leaching process so that the second washing liquid is mixed with the hematite for the first acid leaching. 0.6m 3 The slag is washed online with pure water, and the filtrate (washing liquid) after filtration is added to the second leaching liquid and reused together with the hematite for pulping and the first acid leaching. The filter residue (precious metal enriched residue) is packaged and temporarily stored, and can be used for further recovery and extraction of precious metals. The total residue rate of the first and second acid leaching is 0.98% (dry basis), and the total leaching rates of Fe and Ni are 99.13% and 98.86% respectively.
[0130] In the reduction purification process, 2480 kg of low-matte nickel powder was added to the first leachate, and the amount of low-matte nickel powder added was 1.6 times the theoretical amount required to completely reduce the trivalent iron ions in the first leachate. The reaction temperature was controlled at 65 ° C and the reaction time was 3 hours. After the reaction was completed, the purified liquid with a pH value of 1.75 was obtained by filter pressing. The composition of the purified liquid (ferrous nickel sulfate solution) is shown in Table 2.
[0131] Example 3
[0132] This embodiment provides a method for recycling hematite, comprising the following steps:
[0133] In the pre-treatment process, the hematite slag and low-grade nickel matte are placed in a vertical mill respectively, and the abrasive materials are crushed to obtain hematite powder (80 mesh) and low-grade nickel matte powder (200 mesh) for standby use. Add 24m 3 Bottom water (0.8m 3 Pure water +23.2m 3 The second leachate, from Example 1), was added with 6 t dry hematite powder and slurried for 15 min.
[0134] In the first acid leaching process, after slurrying, the first leaching tank begins to heat up and add 2.7m 3The first acid leaching was carried out with 98% concentrated sulfuric acid, the amount of acid added was 0.7 times the theoretical amount of acid required to leach all the iron in the hematite, the leaching reaction temperature was set to 90°C, the reaction was carried out for 9 hours, and after the reaction was completed, the first leaching residue and the first leaching liquid with a pH value of 0.25 were obtained by filter pressing. The slag rate (dry basis) of the first acid leaching process was 8.77%, and the Fe and Ni leaching rates were 68.21% and 71.85%, respectively.
[0135] In the intermediate treatment process, 9m 3 The residue is washed with pure water online, and the filtrate (washing liquid) after filtration is added to the first leaching liquid, and the residue is sent to the second leaching tank. 1.7m 3 Pure water was used as the bottom water, and filter residue (water content 30%) was added and slurried for 15 minutes.
[0136] In the second acid leaching process, after slurrying, the second leaching tank begins to heat up and add 1.74m 3 The second acid leaching was carried out with 98% concentrated sulfuric acid, the amount of acid added was 1.5 times the theoretical amount of acid required to completely leach out the iron in the first leaching residue, the leaching reaction temperature was set at 85°C, the reaction was carried out for 6 hours, and after the reaction was completed, the second leaching residue and the second leaching liquid were obtained by filter pressing.
[0137] In the circulation process, the second leachate is circulated back for mixing with hematite to make pulp and perform the first acid leaching.
[0138] In the washing process, the second leaching residue is washed to obtain a second washing liquid and a second washing residue, and the second washing liquid is recycled to the first leaching process so that the second washing liquid is mixed with the hematite for the first acid leaching. 1.2m 3 The slag is washed online with pure water, and the filtrate (washing liquid) after filtration is added to the second leaching liquid and reused together with the hematite for pulping and the first acid leaching. The filter residue (precious metal enriched residue) is packaged and temporarily stored, and can be used for further recovery and extraction of precious metals later. The total residue rate of the first and second acid leaching is 0.81% (dry basis), and the total leaching rates of Fe and Ni are 99.52% and 99.49% respectively.
[0139] In the reduction purification process, 5580 kg of low-grade nickel powder was added to the first leachate, and the amount of low-grade nickel powder added was 1.8 times the theoretical amount required to completely reduce the trivalent iron ions in the first leachate. The reaction temperature was controlled at 70 ° C and the reaction time was 4 hours. After the reaction was completed, the purified liquid with a pH value of 2.38 was obtained by filter pressing. The composition of the purified liquid (nickel ferrous sulfate solution) is shown in Table 2.
[0140] Example 4
[0141] This embodiment provides a method for recycling hematite, comprising the following steps:
[0142] In the pre-treatment process, the hematite slag and low-grade nickel matte are placed in a vertical mill respectively, and the hematite powder (200 mesh) and low-grade nickel matte powder (300 mesh) are obtained after the abrasive is crushed for standby use. 3 Bottom water (0.4m 3 Pure water +11.6m 3 The second leachate, from Example 1), was added with 3 t dry hematite powder and slurried for 15 min.
[0143] In the first acid leaching process, after slurrying, the first leaching tank begins to heat up and add 1.16m 3 The first acid leaching was carried out with 98% concentrated sulfuric acid, the amount of acid added was 0.6 times the theoretical amount of acid required to leach all the iron in the hematite, the leaching reaction temperature was set to 98°C, the reaction was carried out for 10 hours, and after the reaction was completed, the first leaching residue and the first leachate with a pH value of 0.32 were obtained by filter pressing. The slag rate (dry basis) of the first acid leaching process was 11.26%, and the Fe and Ni leaching rates were 56.84% and 65.53%, respectively.
[0144] In the intermediate treatment process, 4.5m 3 The residue is washed with pure water online, and the filtrate (washing liquid) after filtration is added to the first leaching liquid, and the residue is sent to the second leaching tank. Add 0.85m 3 Pure water was used as the bottom water, and filter residue (water content 30%) was added and slurried for 15 minutes.
[0145] In the second acid leaching process, after slurrying, the second leaching tank begins to heat up and add 1.31m 3 The second acid leaching was carried out with 98% concentrated sulfuric acid, the amount of acid added was 1.7 times the theoretical amount of acid required to completely leach out the iron in the first leaching residue, the leaching reaction temperature was set at 70°C, the reaction was carried out for 6 hours, and after the reaction was completed, the second leaching residue and the second leaching liquid were obtained by filter pressing.
[0146] In the circulation process, the second leachate is circulated back for mixing with hematite to make pulp and perform the first acid leaching.
[0147] In the washing process, the second leaching residue is washed to obtain a second washing liquid and a second washing residue, and the second washing liquid is recycled to the first leaching process so that the second washing liquid is mixed with the hematite for the first acid leaching. 0.6m 3 The slag is washed online with pure water, and the filtrate (washing liquid) after filtration is added to the second leaching liquid and reused together with the hematite for pulping and the first acid leaching. The filter residue (precious metal enriched residue) is packaged and temporarily stored, and can be used for further recovery and extraction of precious metals later. The total residue rate of the first and second acid leaching is 0.75% (dry basis), and the total leaching rates of Fe and Ni are 99.68% and 99.52% respectively.
[0148] In the reduction purification process, 1860 kg of low-matte nickel powder was added to the first leachate, and the amount of low-matte nickel powder added was 1.2 times the theoretical amount required to completely reduce the trivalent iron ions in the first leachate. The reaction temperature was controlled at 60°C and the reaction time was 2 hours. After the reaction was completed, the purified liquid with a pH value of 1.05 was obtained by filter pressing. The composition of the purified liquid (ferrous nickel sulfate solution) is shown in Table 2.
[0149] Comparative Example 1
[0150] The difference from Example 1 is that the leaching uses a one-stage leaching and a different reducing agent, and specifically includes the following steps:
[0151] In the pre-treatment process, 12m 3 Pure water is used as the base water, 3t of dry hematite powder is added, and slurrying is carried out for 15 minutes.
[0152] In the acid leaching process, after slurrying, the first leaching tank starts to heat up and add 3.47m 3 Acid leaching was carried out with 98% concentrated sulfuric acid, and the amount of acid added was 1.8 times the theoretical amount of acid required to leach all the iron in the hematite. The leaching reaction temperature was set to 95°C and the reaction was carried out for 8 hours. After the reaction was completed, the first leaching residue and the leachate with a pH value of -0.95 (relative acid was relatively high) were obtained by filter pressing. The Fe content of the leachate was 130.37 g / L, and the Ni content was 13.22 g / L.
[0153] In the washing process, the leached residue is washed to obtain a wash liquid and a wash residue. The wash liquid is recycled to the first leaching process so that the wash liquid is mixed with the hematite for acid leaching. The wash residue (precious metal enriched residue) is packaged and temporarily stored, and can be used for further recovery and extraction of precious metals later. The total slag rate is 1.15% (dry basis), and the total leaching rates of Fe and Ni are 97.14% and 99.66% respectively.
[0154] In the reduction purification process, the first leachate is transferred to the purification tank, and pure water is added at a volume ratio of 1:1 for dilution. After adding water and stirring for 15 minutes, 1.01t of manganese powder (purity 99.7%, the amount added is 1.1 times the theoretical amount of manganese powder required to completely reduce the trivalent iron ions in the first leachate) is added. After the manganese powder is added, react at room temperature for 2 hours. After the reaction is completed, filter press to obtain a purified liquid with a pH value of 0.96. The composition of the purified liquid is shown in Table 2.
[0155] Table 2: Composition of the purified liquid obtained in each embodiment and comparative example
[0156] Element (g / L) <![CDATA[Fe 2+ ]]> <![CDATA[Ni 2+ ]]> <![CDATA[Cu 2+ ]]> <![CDATA[Cr 3+ ]]> <![CDATA[Fe 3+ ]]> Example 1 72.65 7.45 0.005 0.029 0.054 Example 2 92.62 10.41 0.002 0.025 0.035 Example 3 90.48 10.65 0.0005 0.015 0.02 Example 4 85.95 9.36 0.03 0.03 0.08 Comparative Example 1 60.13 6.47 0.004 0.0003 0.031
[0157] Referring to Table 1-Table 2, it can be seen from Example 1-Example 2 that the recovery rate of iron and nickel in hematite can reach more than 99% by using the resource recovery treatment method provided in the examples of the present application, and the precious metals in the hematite can be effectively separated, and the total slag rate of leaching can be less than 1%. In addition, by further treating the leachate, a purified liquid containing ferrous ions and nickel ions can be obtained, which can be directly used as a raw material for producing a precursor of a positive electrode material for a battery. In Comparative Example 1, hematite is treated under reaction conditions different from those in the examples of the present application, and the ferrous content in the purified liquid is significantly lower than the ferrous content in Examples 1-4, and the nickel content is also lower than the nickel content in Examples 1-4.
[0158] It can be seen that in the embodiment of the present application, the soluble metal elements such as iron and nickel contained in the hematite can be selectively separated from the elements such as precious metals through two acid leaching, thereby realizing the resource utilization of the hematite. Moreover, the auxiliary materials used in the resource treatment method of the present application are only acid and water, with low acid consumption, low treatment cost, no wastewater and waste residue generated, and good application prospects.
[0159] The various technical features described above can be combined arbitrarily. Although all possible combinations of these technical features are not described, any combination of these technical features should be considered to be covered by this specification as long as there is no contradiction in such combination.
[0160] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A method for recycling hematite, characterized in that: The following steps are involved: A first leaching step, wherein the hematite is subjected to a first acid leaching, and then solid-liquid separation is performed to obtain a first leaching residue and a first leaching solution containing trivalent iron ions and nickel ions; A second leaching step, subjecting the first leaching residue to a second acid leaching, and then performing solid-liquid separation to obtain a second leaching residue containing precious metals and a second leaching solution containing trivalent iron ions and nickel ions; The amount of acid used in the first leaching step is less than the theoretical amount of acid required to completely leach the iron in the hematite, and the amount of acid used in the second leaching step is greater than or equal to the theoretical amount of acid required to completely leach the iron in the first leaching residue.
2. The method for recycling hematite according to claim 1, characterized in that: The amount of acid used in the first leaching step is 0.4 to 0.9 times the theoretical amount of acid required to leach all the iron in the hematite; and / or The amount of acid used in the second leaching step is 1.0 to 2.0 times the theoretical amount of acid required to completely leach out the iron in the first leaching slag.
3. The resource processing method of hematite according to claim 1, characterized in that: The first leaching step comprises: A pre-treatment step, subjecting the hematite to crushing and / or first slurrying treatment to obtain a pre-treated material; In the first acid leaching step, the pre-treated material is subjected to the first acid leaching, and then solid-liquid separation is performed to obtain the first leaching residue and the first leaching solution containing trivalent iron ions and nickel ions.
4. The resource processing method of hematite according to claim 3, characterized in that: The particle size of the hematite after crushing is less than or equal to 80 mesh, preferably less than or equal to 150 mesh; Optionally, the first slurrying treatment includes mixing water and hematite to make slurry; Optionally, the acid used in the first acid leaching step includes at least one of sulfuric acid and hydrochloric acid, preferably sulfuric acid; Optionally, the acid leaching temperature of the first acid leaching step is 90°C-100°C; Optionally, the acid leaching time of the first acid leaching step is 8h-10h; Optionally, the pH value of the first leachate is 0-0.
5.
5. The method for recycling hematite according to claim 1, characterized in that: The second leaching step comprises: An intermediate treatment step, wherein the first leached residue is subjected to a washing treatment and / or a second slurry treatment to obtain an intermediate treated material; In the second acid leaching step, the intermediate treated material is subjected to a second acid leaching, and then solid-liquid separation is performed to obtain a second leaching residue containing precious metals and a second leaching solution containing trivalent iron ions and nickel ions.
6. The method for recycling hematite according to claim 5, characterized in that: The washing treatment comprises washing the first leached residue with water to obtain a first washed liquid and a first washed residue, wherein the first washed residue is used as the intermediate processed material or is used as the intermediate processed material after the second slurry treatment; Optionally, the intermediate treatment process further comprises mixing the first post-washing liquid with the first leaching liquid to dilute the first leaching liquid; Optionally, the volume of water used for the washing treatment is 30%-40% of the volume of the first leachate.
7. The resource processing method of hematite according to claim 5, characterized in that: The second slurrying treatment includes mixing water with the first leached residue to make slurry; Optionally, the acid used in the second acid leaching step is at least one of sulfuric acid and hydrochloric acid, preferably sulfuric acid; Optionally, the acid leaching temperature of the second acid leaching step is 70°C-100°C; Optionally, the acid leaching time of the second acid leaching step is 4h-8h.
8. The method for recycling hematite according to claim 1, characterized in that: The resource processing method also includes: A circulation process is to circulate the second leachate back to the first leaching process, so that the second leachate is mixed with the hematite to perform the first acid leaching.
9. The method for recycling hematite according to claim 1, characterized in that: The resource processing method also includes: A washing step, washing the second leached residue to obtain a second washed liquid and a second washed residue, wherein the second washed liquid is recycled and used in the first leaching step, so that the second washed liquid is mixed with the hematite for a first acid leaching; Optionally, the washing process uses water washing; Optionally, the volume of water used in the washing process is 30%-40% of the volume of the second leachate.
10. The resource processing method of hematite according to any one of claims 1 to 9, characterized in that: The resource processing method also includes: a reduction purification step, wherein the first leaching solution is mixed with the nickel intermediate product for reaction, and then solid-liquid separation is performed to obtain a purified solution containing ferrous ions and nickel ions; Optionally, the amount of the nickel intermediate is 1.2 to 1.8 times the theoretical amount required to completely reduce the trivalent iron ions in the first leachate; Optionally, the mixed reaction temperature is 60°C-70°C; Optionally, the mixing reaction time is 2h-4h; Optionally, the pH value of the purified liquid is 1.0 to 2.5; Optionally, the nickel intermediate product comprises nickel matte; Optionally, the particle size of the nickel matte is less than or equal to 100 mesh, preferably less than or equal to 200 mesh.
Citation Information
Patent Citations
Method for recovering valuable metals from electroplating sludge
CN113564366A
Method for separately realizing open circuits of nickel, copper and iron in high nickel matte and concentrating precious metals
CN113957243A