Production method of 5.5 Ni steel for service low-temperature container at-196 DEG C
Through the specific component design and process flow, the problems of high heat treatment cost and difficulty in plate shape control of 5.5Ni steel are solved, and the production of 5.5Ni steel that meets service in -196℃ is achieved at low cost and high efficiency, and the low-temperature toughness and plate shape are optimized. Uniformity.
Patent Information
- Application Number
- CN202410510861.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-26
- Publication Date
- 2024-11-15
AI Technical Summary
The existing 5.5Ni steel has high heat treatment cost and low efficiency, and cannot meet the low-temperature service conditions of -196℃, making it difficult to control the plate shape.
Adopt specific components design and process flow, including converter smelting, LF+RH refining, two-cold water weak-cold continuous casting, two-stage controlled rolling and offline tempering and heat treatment, control heat treatment temperature and cooling process, reduce the content of precious metal elements, and improve tissue performance and plate shape uniformity.
It realizes low-cost and high-efficiency production of 5.5Ni steel that meets service in -196℃, optimizes plate shape control and low-temperature toughness, reduces alloy costs, and improves heat treatment efficiency and output.
Smart Images

Figure CN118957417A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel production, and in particular relates to a method for producing 5.5Ni steel for low-temperature containers that meet the requirements of -196°C service. Background Art
[0002] With the development of my country's LNG industry chain and the large-scale development of cryogenic storage tanks in the chemical industry, the demand for high-strength low-temperature container steel is increasing day by day. 9Ni steel is generally used to build large LNG storage tanks or large ethane, ethylene storage tanks and other facilities, but with the advancement of smelting technology and material organization and control technology, the performance margin of 9Ni steel has been greatly exceeded. In addition, Ni is a precious metal element, which makes the cost of 9Ni steel high. In order to support the high-quality and low-cost development of large-scale cryogenic storage tanks, on the basis of ensuring material performance, it is necessary to develop more economical materials to replace traditional 9Ni steel and enhance the competitiveness of the industrial chain.
[0003] In order to reduce the cost of 9Ni steel alloy, nickel-saving alloy design is the research and development trend of low-temperature materials. Ni-saving 7Ni steel has been successfully developed and applied internationally and has gradually replaced 9Ni steel in China, but the cost reduction is limited. The present invention further reduces the use of precious metal Ni on the basis of ensuring material performance, but its performance still reaches the level of traditional 9Ni steel.
[0004] At present, China's patents on 5.5Ni steel involving 5.5Ni steel alloy design, production and manufacturing processes are as follows: Chinese patent number CN116770170A discloses a 5.5Ni steel plate for ultra-low temperature environment and its manufacturing method, which manufactures 5~30mm thick 5.5Ni steel plates with guaranteed mechanical properties and process performance. From its case, 12mm can meet the low temperature toughness requirements of -196℃, but 25mm steel plates can only meet the low temperature toughness requirements of -100℃, and cannot meet the service conditions of -196℃. The heat treatment adopts the QLT process, that is, it needs to be quenched twice, once above the A3 line, and once in the two-phase region, and the heat treatment cost is high.
[0005] Chinese patent number CN115341140A discloses a steel for ultra-low temperature pressure vessels and a production method thereof, which has a wide composition range, wherein the Ni content is 5.2~6.8%. According to the standard classification, the alloy element range covers three types of steel: 5.5Ni steel, 6Ni steel and 7Ni steel. The Ni content that meets the impact performance requirement of -196℃ is high, and the alloy cost is high; in this patent, two-phase zone quenching at about 750℃ is adopted, but in the industrial production process, the normalizing or quenching temperature of most steel types is higher than 800℃. To cool the furnace temperature to such a low temperature for quenching, the heat treatment requires a long time for empty furnace cooling, which seriously affects the heat treatment output; two-phase zone quenching has extremely high water inlet temperature. Once the water inlet temperature and cooling rate are not matched properly, the ratio of α and γ phases cannot be accurately controlled within a reasonable range, which will lead to large performance fluctuations. In addition, phase change occurs simultaneously during the water entry process, and the plate shape is difficult to control under the influence of complex working conditions of temperature difference stress and phase change stress. Summary of the invention
[0006] The purpose of the present invention is to solve the problems of high heat treatment cost, low efficiency, poor plate shape and inability to meet the low temperature service of -196°C of the existing 5.5Ni steel. A production method of 5.5Ni steel for low-temperature containers that can meet the service at -196°C is provided, which can reduce alloy costs, meet the service at -196°C conditions, facilitate production organization and plate shape control, and improve processing efficiency and output.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions: A method for producing 5.5Ni steel for low-temperature containers that meet the service temperature of -196°C, comprising the following composition design, calculated by mass percentage: C 0.03-0.06%, Si 0.15-0.20%, Mn 0.9-1.2%, S ≤ 0.002%, P ≤ 0.005%, Ni 5.3-5.7%, Cr 0.3-0.7%, Mo 0.12-0.22%, Alt 0.010-0.030%, O ≤ 0.0020%, and the balance being Fe and impurities.
[0008] In order to further achieve the purpose of the present invention, a method for producing 5.5Ni steel for low-temperature containers that meet -196°C service temperature using the above-mentioned composition is also provided, and the specific steps are as follows, including: (1) Steelmaking: converter smelting and LF+RH refining; (2) Continuous casting: The continuous casting is carried out by using secondary cooling water weak cooling and low casting speed. The thickness of the continuous casting billet is 150 mm, and the billet is subjected to pile cooling treatment; (3) Slab heating: In order to control the original austenite grain size, surface quality and plate shape before hot rolling, the temperature uniformity of the entire slab is ≤10°C; (4) Hot rolling: Steel plates with a thickness of ≥15 mm are rolled in two stages. After hot rolling, laminar cooling is performed to a certain temperature before the steel plates are cooled offline. (5) Heat treatment: Offline tempering heat treatment process is adopted.
[0009] Furthermore, after the heat treatment, a structure having tempered martensite as a matrix and a small amount of austenite is finally obtained.
[0010] Furthermore, the yield strength of the steel plate is ≥630MPa, the tensile strength is 690-780MPa, the elongation is ≥20%, the standard sample -196℃ KV2 is ≥120J, and the plate shape of the 5-30mm steel plate is ≤6mm / m.
[0011] Furthermore, in the step (1), the vacuum degree during the RH treatment is controlled to be ≤0.3 torr, and the vacuum treatment time is ≥30 min.
[0012] Furthermore, in the step (2), the superheat of the molten steel during the continuous casting process is controlled at 25-40°C.
[0013] Furthermore, in the step (3), the furnace temperature of the slab with a size of 15 mm or more is 1130-1160°C, and the furnace temperature of the slab with a size of less than 15 mm is 1180-1220°C.
[0014] Furthermore, in step (4), the hot rolling of the steel plate with a thickness of ≥15 mm adopts two-stage controlled rolling, and the specific steps are as follows: S41: Rough rolling is carried out in the austenite recrystallization zone, the starting temperature of rough rolling is 1050~1100℃, and the total reduction is 30~60%; S42: Finish rolling is carried out in the austenite non-recrystallization zone, the starting rolling temperature is lower than 880℃, and the final rolling temperature is 800~830℃.
[0015] Furthermore, in the step (4), laminar cooling is performed after hot rolling, the red-return temperature is controlled between 600-650°C, and the laminar cooling is performed after the steel is cooled to a certain temperature and then the steel is stacked off-line for cooling.
[0016] Furthermore, in the step (5), the hot-rolled plate is subjected to an offline tempering heat treatment, and a quenching + tempering process is used for heat treatment at a temperature above Ac3. The steel plate is heated to 800-840°C and kept at this temperature for 20-50 min, and then water quenched on a roller quenching machine; then heated to 610-640°C and tempered for 50-120 min, and then air-cooled after being taken out of the furnace.
[0017] The composition design principle of the present invention is as follows: C: A strengthening element of steel and an austenite stabilizing element. Reversing the austenite enrichment with C will significantly reduce the Ms point and improve its stability. However, too high a C content will increase the toughness-brittle transition temperature, which is harmful to the low-temperature toughness of the HAZ. When designing, the content should be as low as possible while ensuring strength. The range of this patent is 0.03%~0.06%.
[0018] Ni: It can form α and γ phase solid solutions with Fe, and can be infinitely dissolved in the γ phase. It can expand the γ phase area and is an austenite forming and stabilizing element. It can make screw dislocations difficult to decompose, ensure the occurrence of cross slip, and improve the plastic deformation performance of the material. It is very important for stabilizing the reversed austenite. The reversed austenite rich in Ni and other austenite stabilizing elements is stable at extremely low temperatures and can absorb part of the strain energy during deformation. It can also be transformed into the α´ phase through deformation-induced phase transformation, which is one of the toughening mechanisms. It is beneficial to improve hardenability and improve strength through solid solution strengthening. However, Ni is a precious metal element and mainly relies on imports. The usage should be reduced on the basis of ensuring performance. The scope of this patent is 5.3%~5.7%.
[0019] Mn: It is an austenite stabilizing element. Its enrichment in austenite is conducive to reversing the stability of austenite. It is also a matrix strengthening element. It can improve the strength through solid solution strengthening and precipitation strengthening. It can significantly improve the hardenability of the material. If the Mn content is too high, it is easy to segregate, which is not conducive to the stability of performance. Considering comprehensively, the Mn content of this patent is in the range of 0.90%~1.2%.
[0020] Si: It is a deoxidizing element; it can inhibit the segregation of P and Mn at the grain boundaries; but too high Si content is not conducive to the precipitation of cementite in the HAZ during the welding cooling process, affecting the low-temperature toughness of the welded joint. This patent controls it at 0.15%~0.20%.
[0021] S and P: S easily forms precipitate MnS with Mn, which reduces low-temperature toughness. P easily segregates at grain boundaries, reduces the grain boundary crack growth resistance, and deteriorates low-temperature toughness. Therefore, considering material properties, welding performance and production efficiency, it should be controlled to a minimum.
[0022] Mo: can improve hardenability, thereby improving strength; improve the tempering stability of steel; when coexisting with chromium or manganese, it can reduce or inhibit the temper brittleness caused by other elements. However, too high Mo content is not conducive to welding performance. The Mo content range of the present invention is 0.12%~0.22%.
[0023] Cr: A content of 0.2% or more can improve the hardenability of steel and is conducive to the formation of full martensite structure during quenching. After heat treatment, a stable structure can be obtained, and the low-temperature toughness level can be improved. If the Cr content exceeds 0.70%, large sparks will appear during welding, affecting the welding quality. Therefore, the Cr content of the present invention is in the range of 0.40% to 0.60%.
[0024] O: Steel purity is the prerequisite for ensuring the toughness of steel. Too high O content will lead to excessive oxide inclusions in the steel. O, N and Al are likely to form high-melting-point precipitates Al2O3 and AlN. Moreover, the precipitates are relatively large in diameter, reaching several microns. It is easy to cause stress concentration near the precipitates and become a crack source, seriously affecting the low-temperature toughness of the matrix. Therefore, this design controls the O content to ≤0.0020%.
[0025] Compared with the prior art, the advantages of the technical solution of the present invention are: (1) The alloy range in the composition designed by the present invention is narrow, which is conducive to controlling the stability of the structure and performance; (2) The present invention reduces the content of two precious metal elements, Mo and Ni, thereby reducing the alloy cost; (3) The 5.5Ni steel of the present invention can meet the service conditions of -196°C and has excellent low-temperature toughness; (4) The present invention adopts quenching at a temperature above A3 line, which is beneficial to production organization and control of plate shape. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a metallographic photograph of the tempered structure at 1 / 4 thickness of a 5 mm steel plate corroded by 4% nitric acid alcohol solution in the present invention; Figure 2 This is a metallographic photograph of the tempered structure at 1 / 4 thickness of a 25 mm steel plate corroded by 4% nitric acid alcohol solution in the present invention; Figure 3 The following is a photograph of the steel plate structure of the steel plate of the present invention taken under a scanning electron microscope. DETAILED DESCRIPTION Example
[0027] To make the present invention more clearly understood, the following is a further description of a method for producing 5.5Ni steel for low-temperature containers that meet -196°C service requirements in conjunction with the accompanying drawings. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0028] In this embodiment, the composition of 5.5Ni steel can be designed as follows, see Table 1.
[0029]
[0030] The steel plates with different chemical compositions are produced according to the following production methods, and the specific steps are as follows: (1) Steelmaking: converter smelting and LF+RH refining; (2) Continuous casting: The continuous casting is carried out by using secondary cooling water weak cooling and low casting speed. The thickness of the continuous casting billet is 150 mm, and the billet is subjected to pile cooling treatment; (3) Slab heating: In order to control the original austenite grain size, surface quality and plate shape before hot rolling, the temperature uniformity of the entire slab is ≤10°C; (4) Hot rolling: Steel plates with a thickness of ≥15 mm are rolled in two stages. After hot rolling, they are cooled to a certain temperature and then stacked for cooling. (5) Heat treatment: Offline tempering heat treatment process is adopted.
[0031] In this embodiment, LF furnace is used for deoxidation, desulfurization and precision alloying, and continuous casting superheat control; in order to reduce the influence of gas inclusions such as H on low-temperature toughness, RH vacuum degassing treatment is used, and the vacuum degree is maintained at ≤0.3torr for ≥30min, and the H element content is controlled below 2ppm. Continuous casting produces 150mm thick ingots, and the whole process of continuous casting is gas-protected casting, and the superheat of molten steel is controlled in the range of 25~40℃ to ensure the quality of ingots.
[0032] In order to control the shape of thin-gauge rolled plates, high-temperature steelmaking is adopted for plates with a thickness of less than 15 mm, and low-temperature steelmaking is adopted for plates with a thickness of ≥ 15 mm. In order to refine the rolled structure, two-stage controlled rolling is adopted for plates with a thickness of ≥ 15 mm.
[0033] Specifically, the manufacturing process parameters such as heating, rolling and heat treatment of steels in Examples 1 to 4 under different chemical compositions in Table 1 are shown in Table 2.
[0034]
[0035] After adopting the production method of the present invention, the final mechanical properties of the steel plates of Examples 1 to 4 are shown in Table 3. Among them, after the 5 mm thick steel plate is corroded by 4% nitric acid alcohol solution, the tempered structure photograph at 1 / 4 thickness is as follows Figure 1 As shown in the figure, after a 25 mm thick steel plate was corroded with 4% nitric acid alcohol solution, the tempered structure photograph at 1 / 4 of the thickness is as follows Figure 2 shown.
[0036]
[0037] In the present invention, all steel plates are subjected to offline heat treatment to obtain a mixed structure of tempered martensite and a small amount of austenite, thereby ensuring that the material has high strength and excellent low-temperature toughness, which can fully meet the service requirements under -196°C conditions. The shape of the finished plate in the thickness range of 5~30mm is controlled to be ≤6mm / m in any direction.
[0038] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.
Claims
1. A method for producing 5.5Ni steel for low-temperature containers that meet -196°C service temperature, comprising the following composition design, characterized in that: The components by mass percentage are: C 0.03-0.06%, Si 0.15-0.20%, Mn 0.9-1.2%, S ≤ 0.002%, P ≤ 0.005%, Ni 5.3-5.7%, Cr 0.3-0.7%, Mo 0.12-0.22%, Alt 0.010-0.030%, O ≤ 0.0020%, and the balance is Fe and impurities.
2. The method for producing 5.5Ni steel for low-temperature containers that meet -196°C service temperature according to claim 1, wherein the specific steps are as follows, characterized in that: (1) Steelmaking: converter smelting and LF+RH refining; (2) Continuous casting: The continuous casting is carried out by using secondary cooling water weak cooling and low casting speed. The thickness of the continuous casting billet is 150 mm, and the billet is subjected to pile cooling treatment; (3) Slab heating: In order to control the original austenite grain size, surface quality and plate shape before hot rolling, the temperature uniformity of the entire slab is ≤10°C; (4) Hot rolling: Steel plates with a thickness of ≥15 mm are rolled in two stages. After hot rolling, laminar cooling is performed to a certain temperature before the steel plates are cooled offline. (5) Heat treatment: Offline tempering heat treatment process is adopted.
3. The method for producing 5.5Ni steel for low-temperature containers that meet -196°C service requirements according to claim 2, characterized in that: After the heat treatment, a structure with tempered martensite as the matrix and a small amount of austenite is finally obtained.
4. The method for producing 5.5Ni steel for low-temperature containers that meet -196°C service requirements according to claim 2, characterized in that: The yield strength of the steel plate is ≥630MPa, the tensile strength is 690-780MPa, the elongation is ≥20%, the standard sample -196℃ KV2 is ≥120J, and the plate shape of the 5-30mm steel plate is ≤6mm / m.
5. The method for producing 5.5Ni steel for low-temperature containers that meet -196°C service temperature according to claim 2, characterized in that: In the step (1), the vacuum degree during the RH treatment is controlled to be ≤0.3 torr, and the vacuum treatment time is ≥30 min.
6. The method for producing 5.5Ni steel for low-temperature containers that meet -196°C service temperature according to claim 2, characterized in that: In the step (2), the superheat of the molten steel is controlled at 25-40°C during the continuous casting process.
7. The method for producing 5.5Ni steel for low-temperature containers that meet -196°C service temperature according to claim 2, characterized in that: In the step (3), the furnace temperature of the slab with a size of 15 mm or more is 1130-1160°C, and the furnace temperature of the slab with a size of less than 15 mm is 1180-1220°C.
8. The method for producing 5.5Ni steel for low-temperature containers that meet -196°C service temperature according to claim 2, characterized in that: In step (4), the hot rolling of the steel plate with a thickness of ≥15 mm adopts two-stage controlled rolling, and the specific steps are as follows: S41: Rough rolling is carried out in the austenite recrystallization zone, the starting temperature of rough rolling is 1050~1100℃, and the total reduction is 30~60%; S42: Finish rolling is carried out in the austenite non-recrystallization zone, the starting rolling temperature is lower than 880℃, and the final rolling temperature is 800~830℃.
9. The method for producing 5.5Ni steel for low-temperature containers that meet -196°C service temperature according to claim 2, characterized in that: In the step (4), laminar cooling is performed after hot rolling, and the red-return temperature is controlled between 600-650°C. After laminar cooling reaches a certain temperature, the steel is stacked and cooled offline.
10. The method for producing 5.5Ni steel for low-temperature containers that meet -196°C service requirements according to claim 2, characterized in that: In the step (5), the hot-rolled plate is subjected to an offline tempering heat treatment, and a quenching + tempering process is used for heat treatment at a temperature above Ac3. The steel plate is heated to 800-840°C and kept at this temperature for 20-50 minutes, and then water quenched on a roller quenching machine; then heated to 610-640°C and tempered for 50-120 minutes, and then air-cooled after being taken out of the furnace.
Citation Information
Cited By
Method for improving impact toughness of 5.5 Ni steel of medium plate
CN120350203A
Low-temperature high-toughness steel plate for methanol washing tower and manufacturing method of low-temperature high-toughness steel plate
CN121406978A
Nickel-based low-temperature steel having high crack arrest performance in low-temperature environment of -165°c, and manufacturing method therefor
WO2026200095A1
Production method for high-strength 5ni steel for cryogenic vessel for service at -140°c
WO2026214061A1