Hot working method for remarkably improving dynamic recrystallization integral number of nickel-based superalloy

Through prestressed aging heat treatment and thermal deformation technology, the problem of delta phase precipitation along the grain boundary in nickel-based high-temperature alloys is solved, and the uniform distribution of delta phase and fine granularity is achieved, which significantly improves the dynamic recrystallization volume fraction and optimizes the nickel-based The structure and mechanical properties of high-temperature alloys.

CN118957462AActive Publication Date: 2024-11-15NORTHWESTERN POLYTECHNICAL UNIV

Patent Information

Application Number
CN202411165767.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

During the dynamic recrystallization process of existing nickel-based high-temperature alloys, the delta phase precipitates along the grain boundary, causing uneven structure, making it difficult to achieve the ideal grain refinement effect, and long-term heat treatment increases the process cost, and the delta phase size is too large or too small. It cannot effectively promote dynamic recrystallization.

Method used

By prestressed aging heat treatment, the δ phase is controlled to be uniformly precipitated in the grain boundaries and crystals, stresses of 100~160MPa are applied for aging treatment, and more than 60% of the total deformation calorimetric deformation is performed during the thermal deformation process to ensure the uniform distribution of the δ phase. and fine particles.

Benefits of technology

The dynamic recrystallization volume fraction of nickel-based high-temperature alloy is significantly improved, the problem of uneven structure is avoided, the precipitation time is reduced, the delta phase is excessively coarsified, the mechanical properties of the alloy are maintained, and grain refinement and uniform structure are achieved. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957462A_ABST
    Figure CN118957462A_ABST
Patent Text Reader

Abstract

The invention provides a hot working method for remarkably improving the dynamic recrystallization integral number of a nickel-based high-temperature alloy. The method comprises the following steps: firstly, putting an Inconel 625 alloy into a heat treatment furnace at the temperature of 1000-1100 DEG C, preserving heat for 30-90 minutes, carrying out solution treatment, and carrying out water cooling; heating the Inconel 625 alloy subjected to solid solution heat treatment to 700-750 DEG C, preserving heat for 50-100 hours, applying stress of 100-160 MPa at the same time, and performing water cooling to uniformly separate out a delta phase; and finally, the Inconel 625 alloy subjected to aging heat treatment is heated to 870-950 DEG C, heat preservation is conducted for 2-10 min, thermal deformation is conducted at the strain rate of 0.1-0.001 s <-1 >, and the total deformation amount is 60% or above. According to the method, a large number of uniformly-distributed delta phases with proper sizes are obtained within a relatively short time by applying external stress, the problems of along-crystal distribution and large sizes of the delta phases caused by traditional aging heat treatment are avoided, and the delta phases are ensured to fully play a role through proper process parameters in the subsequent thermal deformation process; and the dynamic recrystallization integral number is greatly increased, and the method has obvious advantages in the aspects of grain refinement and structure homogenization in the hot working process of the nickel-based high-temperature alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot working of nickel-based high-temperature alloys, and in particular relates to a hot working method for significantly improving the dynamic recrystallization volume fraction of nickel-based high-temperature alloys. Background Art

[0002] Nickel-based high-temperature alloys are widely used in the manufacture of high-temperature structural parts in the fields of aerospace, petrochemicals, etc. due to their good creep resistance, fatigue resistance, corrosion resistance, and oxidation resistance. In recent years, the continuous development of the process, structure, and performance of large-scale equipment such as aircraft engines has put forward increasingly stringent requirements on the organizational control of the nickel-based high-temperature alloy forming process.

[0003] Pre-precipitated δ phase can effectively promote dynamic recrystallization during the forging process of nickel-based superalloys, thereby assisting in grain refinement. This process is called Delta Process and has been applied to the industrial production of nickel-based superalloys. However, since the δ phase usually tends to precipitate along the grain boundaries during the aging process, dynamic recrystallization cannot be fully carried out, resulting in the formation of an uneven structure of fine recrystallized grains surrounding the original coarse deformed grains in the nickel-based superalloy prepared by the Delta Process, making it difficult to achieve the ideal grain refinement effect.

[0004] Although sufficient intragranular δ phase can be formed through long-term peak aging, it will inevitably lead to excessively coarse δ phase size. Excessive and oversized residual δ phase after hot working will deteriorate the mechanical properties of nickel-based high-temperature alloys, and long-term heat treatment also increases the process cost. In addition, if the δ phase size is too small, it cannot effectively promote the nucleation of dynamic recrystallization grains. Therefore, there is an urgent need for a method that can obtain a dispersed distribution, suitable size and sufficient number of δ phases in a relatively short time to further promote the dynamic recrystallization of nickel-based high-temperature alloys for refinement and uniform organization. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a method for significantly increasing the volume fraction of dynamic recrystallization of nickel-based high-temperature alloys, by controlling the uniform precipitation of δ phase at grain boundaries and within grains through prestressed aging heat treatment, thereby avoiding dynamic recrystallization occurring only at grain boundaries during subsequent hot working, thereby promoting more sufficient dynamic recrystallization within the grain, and ultimately making the grain size more uniform and fine.

[0006] The specific technical solutions of the present invention are as follows: The present invention provides a hot working method for significantly improving the dynamic recrystallization volume fraction of a nickel-based high-temperature alloy, comprising the following steps: Step 1: Solution heat treatment: raise the temperature of the heat treatment furnace to 1000-1100°C, put Inconel 625 alloy in for solution heat treatment, keep warm for 30-90 minutes, and cool with water; Step 2, aging heat treatment: the Inconel 625 alloy after solution heat treatment is heated to 700-750°C and kept at this temperature for 50-100 hours, and at the same time, a stress of 100-160 MPa is applied for prestress aging treatment, and water cooling is performed; Step 3: Thermal deformation: Heat the Inconel 625 alloy after aging heat treatment to 870~950℃ and keep it at this temperature for 2~10min. -1 The thermal deformation is carried out at a strain rate of , and the total deformation is above 60%.

[0007] As a further illustration of the present invention, in step 2, the prestressing aging heat treatment temperature is selected to be 750° C., and the holding time is 90 h.

[0008] As a further illustration of the present invention, the δ phase in the Inconel 625 alloy after the prestress aging treatment in step 2 is dispersedly distributed with a volume fraction of more than 40%, and the average major axis size can be maintained between 1 and 3 μm.

[0009] As a further illustration of the present invention, the thermal deformation treatment in step 3 is specifically any one of forging, hot rolling or hot compression.

[0010] As a further illustration of the present invention, the thermal deformation temperature in step 3 is 900° C. and the insulation time is specifically 5 minutes.

[0011] As a further illustration of the present invention, the strain rate in step 3 is specifically 0.01s -1 .

[0012] Compared with the prior art, the present invention has the following beneficial technical effects: The present invention overcomes the difficulty of controlling the characteristics of the δ phase by regulating the distribution, size and quantity of the δ phase by applying external stress. The uniformly distributed micron-sized δ phase obtained can significantly promote the dynamic recrystallization inside the original grains, thereby avoiding the problem of δ phase distribution along the grain and uneven organization during subsequent thermal deformation caused by traditional aging heat treatment.

[0013] The present invention accelerates the precipitation of δ phase based on external stress regulation, reduces the time required for precipitation of sufficient δ phase and also avoids excessive coarsening of δ phase caused by too long heat treatment time. Appropriate hot deformation process parameters also ensure that the residual incompletely dissolved δ phase after hot deformation will also be dispersed in the form of fine particles, thereby not deteriorating the mechanical properties of the nickel-based high-temperature alloy.

[0014] Other features and advantages of the technical solution will be described in the subsequent description, and partly become apparent from the description, or understood by implementing the technical solution. The purpose and other advantages of the technical solution can be achieved and obtained through the structures specifically pointed out in the written description and the drawings.

[0015] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The accompanying drawings are used to provide further understanding of the present technical solution and constitute a part of the specification. Together with the embodiments of the present technical solution, they are used to explain the present technical solution and do not constitute a limitation to the present technical solution.

[0017] Figure 1 This is a microstructure diagram of Inconel 625 alloy in Example 1 of the present invention after prestress aging at 750°C for 60 hours.

[0018] Figure 2 This is a microstructure diagram of Inconel 625 alloy in Example 2 of the present invention after prestress aging at 750°C for 90 hours.

[0019] Figure 3 This is the microstructure diagram of Inconel 625 alloy in Comparative Example 1 after conventional aging at 750°C for 200 hours.

[0020] Figure 4 This is a microstructure diagram of the Inconel 625 alloy after thermal deformation at 900° C. after prestress aging for 60 hours in Example 1 of the present invention.

[0021] Figure 5 This is a microstructure diagram of the Inconel 625 alloy after thermal deformation at 900°C that has undergone 90h prestress aging heat treatment in Example 2 of the present invention.

[0022] Figure 6 This is the microstructure of the Inconel 625 alloy after thermal deformation at 900°C after conventional aging for 200 hours in Comparative Example 1.

[0023] Figure 7 It is a statistical chart of the volume fraction of the δ phase after aging and the volume fraction of recrystallized grains after hot deformation of Inconel 625 alloy in Example 1, Example 2 and Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0024] The preferred embodiments of the present technical solution are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present technical solution, and are not used to limit the present technical solution.

[0025] At present, sufficient intragranular δ phase can be formed through long-term peak aging, but it is bound to cause the δ phase to be too coarse. Excessive and oversized residual δ phase after hot working will deteriorate the mechanical properties of nickel-based high-temperature alloys, and long-term heat treatment also increases the process cost. In addition, if the δ phase size is too small, it cannot effectively promote the nucleation of dynamic recrystallization grains. Therefore, there is an urgent need for a method that can obtain a dispersed distribution, suitable size and sufficient number of δ phases in a relatively short time to further promote the dynamic recrystallization of nickel-based high-temperature alloys for refinement and uniform organization.

[0026] Based on this, the present invention provides a hot working method for significantly improving the dynamic recrystallization volume fraction of a nickel-based high-temperature alloy, comprising the following steps: Step 1: Solution heat treatment: Raise the temperature of the heat treatment furnace to 1000-1100°C, put Inconel 625 alloy in for solution heat treatment, keep warm for 30-90 minutes, and water cool to homogenize the alloy matrix composition and dissolve the primary carbides back.

[0027] Specifically, the temperature of the above-mentioned solution heat treatment can be set to, for example, 1000°C, 1030°C, 1050°C, 1070°C, 1100°C, etc.; the holding time can be set to, for example, 30min, 40min, 50min, 60min, 70min, 90min, etc.

[0028] Step 2: Aging heat treatment: The Inconel 625 alloy after solution heat treatment is heated to 700-750°C and kept at this temperature for 50-100 hours. At the same time, a stress of 100-160 MPa is applied for prestressed aging treatment, and water-cooled to uniformly precipitate the δ phase.

[0029] Specifically, the prestressed aging heat treatment temperature can be selected as 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, etc., preferably 750°C; the holding time can be 50h, 60h, 70h, 80h, 90h, 100h, etc., preferably 90h. The aging heat treatment temperature is preferably 750°C, and the holding time is preferably 90h, which can ensure that the volume fraction of the δ phase is above 40% and the major axis size is greater than 1μm. Specifically, the δ phase in the Inconel 625 alloy after prestressed aging treatment is dispersed, with a volume fraction of more than 40%, and the average major axis size can be maintained between 1 and 3μm.

[0030] Step 3: Thermal deformation: Heat the Inconel 625 alloy after aging heat treatment to 870~950℃ and keep it at this temperature for 2~10min. -1 The thermal deformation is carried out at a strain rate of , and the total deformation is above 60%.

[0031] The thermal deformation treatment is specifically any one of forging, hot rolling or hot compression.

[0032] Specifically, the temperature of the above-mentioned heat deformation temperature can be, for example, 870°C, 900°C, 920°C, 950°C, etc., preferably 900°C, to prevent the δ phase from dissolving rapidly due to high temperature or the dynamic recrystallization from being insufficiently carried out due to low temperature; the above-mentioned heat deformation holding time can be, for example, 2min, 5min, 7min, 10min, etc.; preferably 5min, to prevent the δ phase from dissolving prematurely due to long time or the temperature of Inconel 625 alloy from being uneven due to short time. The heat deformation strain rate can be, for example, 0.1s -1 、0.05s -1 、0.01s -1 , 0.005s -1 、0.001s -1 etc.; preferably 0.01s -1 , thereby ensuring that there is sufficient time for dynamic recrystallization to occur during thermal deformation and preventing the dissolution of the δ phase and increased costs caused by too long a time.

[0033] The present invention is described in detail below in conjunction with specific embodiments and drawings. Example 1

[0034] In this embodiment, the method for significantly increasing the dynamic recrystallization volume fraction of a nickel-based high-temperature alloy comprises the following steps: The temperature of the heat treatment furnace was raised to 1050°C at a heating rate of 6°C / min. After being kept at this temperature for 5 minutes to stabilize the furnace temperature, the Inconel 625 alloy sample was placed in the furnace for solution heat treatment. The temperature was kept at this temperature for 60 minutes and the sample was cooled with water to dissolve the primary carbides.

[0035] The Inconel 625 alloy after solution heat treatment was reheated to 750°C at a heating rate of 6°C / min and a stress of 150 MPa was applied. It was kept for 60 hours for prestressed aging heat treatment and water-cooled to obtain a uniformly distributed δ phase.

[0036] The prestressed Inconel 625 alloy was heated to 900°C at a heating rate of 10°C / min, kept at this temperature for 5 min, and then hot-compressed at 900°C with a strain rate of 0.01s -1 , deformation is 60%, water cooling.

[0037] like Figure 1 As shown in the figure, prestress aging forms a dispersed δ phase in Inconel 625 alloy with a volume fraction of about 41% and an average size of about 1 μm.

[0038] like Figure 4As shown in Figure 2, the volume fraction of dynamically recrystallized grains in Inconel 625 alloy after hot deformation is about 56%. Example 2

[0039] In this embodiment, the method for significantly increasing the dynamic recrystallization volume fraction of a nickel-based high-temperature alloy comprises the following steps: The temperature of the heat treatment furnace was raised to 1050°C at a heating rate of 6°C / min. After being kept at this temperature for 5 minutes to stabilize the furnace temperature, the Inconel 625 alloy sample was placed in the furnace for solution heat treatment. The temperature was kept at this temperature for 60 minutes and the sample was cooled with water to dissolve the primary carbides.

[0040] The Inconel 625 alloy after solution heat treatment was reheated to 750°C at a heating rate of 6°C / min and a stress of 150MPa was applied. It was kept for 90h for prestressed aging heat treatment and water-cooled to obtain a uniformly distributed δ phase.

[0041] The prestressed Inconel 625 alloy was heated to 900°C at a heating rate of 10°C / min, kept at this temperature for 5 min, and then hot-compressed at 900°C with a strain rate of 0.01s -1 , deformation is 60%, water cooling.

[0042] like Figure 2 As shown in the figure, prestress aging forms a dispersed δ phase in Inconel 625 alloy with a volume fraction of about 43% and an average size of about 2μm.

[0043] like Figure 5 As shown in the figure, the volume fraction of dynamically recrystallized grains in Inconel 625 alloy after hot deformation is about 68%, and there are only a few residual deformed grains due to insufficient recrystallization inside the original deformed grains.

[0044] Comparative Example 1 The temperature of the heat treatment furnace was raised to 1050°C at a heating rate of 6°C / min. After being kept at this temperature for 5 minutes to stabilize the furnace temperature, the Inconel 625 alloy sample was placed in the furnace for solution heat treatment. The temperature was kept at this temperature for 60 minutes and the sample was cooled with water to dissolve the primary carbides.

[0045] The Inconel 625 alloy after solution heat treatment was reheated to 750°C at a heating rate of 6°C / min, kept at this temperature for 200h for conventional aging heat treatment, and water-cooled to obtain the grain boundary δ phase.

[0046] The Inconel 625 alloy with traditional aging treatment was heated to 900℃ at a heating rate of 10℃ / min, kept at this temperature for 5min, and then hot compressed at 900℃ with a strain rate of 0.01s -1 , deformation is 60%, water cooling.

[0047] In this comparative example, the aging time was selected as 200 h because the precipitation kinetics of the traditional aging δ phase were slow, so the time was extended to ensure that sufficient grain boundary δ phase was formed in the Inconel 625 alloy.

[0048] like Figure 3 As shown in the figure, the δ phase formed in the Inconel 625 alloy by conventional aging is concentrated near the grain boundary, and there is only a very small amount of δ phase in the grain. The volume fraction of the δ phase is about 9%, and the average size is about 4μm.

[0049] like Figure 6 As shown in the figure, after hot deformation of the traditionally aged Inconel 625 alloy, dynamic recrystallization only occurred near the grain boundaries of the original deformed grains, and most of the original deformed grains did not undergo dynamic recrystallization and remained inside, and the volume fraction of dynamically recrystallized grains was only about 14%.

[0050] Obviously, if Figure 7 As shown, the results of the embodiments and comparative examples indicate that, compared with obtaining grain boundary δ through traditional long-term aging heat treatment, the present invention obtains a large amount of uniformly distributed δ phase in a shorter time by applying external stress, and provides more dynamic recrystallization nucleation sites in the crystal during subsequent thermal deformation, thereby greatly improving the dynamic recrystallization volume fraction. This method has obvious advantages in grain refinement and uniform organization during hot working of nickel-based high-temperature alloys.

[0051] Obviously, those skilled in the art can make various changes and modifications to the technical solution without departing from the spirit and scope of the technical solution. Thus, if these modifications and variations of the technical solution fall within the scope of the claims of the technical solution and their equivalents, the technical solution is also intended to include these modifications and variations.

Claims

1. A hot working method for significantly increasing the volume fraction of dynamic recrystallization of a nickel-based high-temperature alloy, characterized in that: The steps include: Step 1: Raise the temperature of the heat treatment furnace to 1000~1100℃, put Inconel 625 alloy in for solution heat treatment, keep warm for 30~90min, and water cool; Step 2: Heat the solution heat treated Inconel 625 alloy to 700-750°C for 50-100 hours, apply 100-160 MPa stress for prestress aging treatment, and water cool. Step 3: Heat the aging heat treated Inconel 625 alloy to 870~950℃ and keep it for 2~10min. -1 The thermal deformation is carried out at a strain rate of , and the total deformation is above 60%.

2. The hot working method for significantly increasing the dynamic recrystallization volume fraction of a nickel-based high-temperature alloy according to claim 1, characterized in that: In step 2, the prestressing aging heat treatment temperature is selected to be 750°C and the holding time is 90h.

3. The hot working method for significantly increasing the dynamic recrystallization volume fraction of a nickel-based high-temperature alloy according to claim 1, characterized in that: After the prestress aging treatment in step 2, the δ phase in the Inconel 625 alloy is dispersed, with a volume fraction of more than 40%, and the average major axis size can be maintained between 1 and 3 μm.

4. The hot working method for significantly increasing the dynamic recrystallization volume fraction of a nickel-based high-temperature alloy according to claim 1, characterized in that: The thermal deformation treatment in step 3 is specifically any one of forging, hot rolling or hot compression.

5. The hot working method for significantly increasing the dynamic recrystallization volume fraction of a nickel-based high-temperature alloy according to claim 1, characterized in that: In step 3, the heat deformation temperature is 900° C. and the holding time is specifically 5 minutes.

6. The hot working method for significantly increasing the dynamic recrystallization volume fraction of a nickel-based high-temperature alloy according to claim 1, characterized in that: The strain rate in step 3 is specifically 0.01s -1 .

Citation Information

Patent Citations

  • Method for thinning nickel base alloy forge piece crystalline grains and improving microstructure uniformity

    CN109457201A

  • Aging heat treatment process for efficiently strengthening nickel-based superalloy

    CN114214583A

  • Hot working method for producing high-uniformity ultra-fine grain nickel-based superalloy

    CN115261753A

  • Under-aging heat treatment process for nickel-based wrought superalloy

    CN115491620A

  • Aging heat treatment method for prolonging creep endurance life of nickel-based superalloy

    CN115747688A

Cited By

  • Heat treatment method for grain refinement of nickel alloy with high tungsten content

    CN119753545A