Microalloyed high-strength high-plasticity efficient extruded magnesium alloy and preparation method thereof
Through low alloy composition design and simplified process, the high energy consumption and cracking problems in the improvement of magnesium alloy strength and plasticity are solved, and the industrial production of high-efficiency extruded magnesium alloy is achieved, which significantly improves the mechanical properties and production efficiency of the alloy.
Patent Information
- Application Number
- CN202411076304.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art has high energy consumption, high production costs and alloy cracking problems in improving the strength and plasticity of magnesium alloys, and high-content alloy elements and rare earth elements need to be added to affect the alloy performance.
Using low alloy composition design and simplified process, by melting and gravity casting under the protection of CO2 and SF6 mixed gases, followed by hot extrusion in the preheated mold, reducing or omitting long-term solid solution or homogenization treatment at high temperatures. Improve the extrusion speed and extrusion ratio to achieve microalloyed high-strength plastic and high-efficiency extrusion magnesium alloy.
It significantly reduces production costs and energy consumption, improves the comprehensive mechanical properties of the alloy, achieves the improvement of high yield strength, tensile strength and elongation, and avoids alloy cracking, which is suitable for industrial production.
Smart Images

Figure CN118979182A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal material processing, and in particular relates to a micro-alloyed high-strength plastic high-efficiency extruded magnesium alloy and a preparation method thereof. Background Art
[0002] As the lightest metal structural material, magnesium alloy is known as the "green material of the 21st century". It has the advantages of low density, high specific strength and specific stiffness, good damping and cutting properties, and easy recycling. It plays an important role in aerospace, automobile, rail transportation, 3C products and medical equipment. my country has abundant reserves of magnesium alloys. Under the national trend of energy conservation, magnesium alloys have received more and more attention. However, due to its low strength and poor plasticity, the application field and scope of magnesium alloys are far less than that of steel and aluminum alloys. The main ways to improve the performance of magnesium alloys are alloying, hot working, heat treatment, etc., but the existing technology often improves the performance of magnesium alloys by adding high alloy content elements or rare earth elements and using complex process means. For example, in a paper entitled "Study on Extrusion Process and Microstructure Performance of Mg-9Gd-8Y-2Nd-1.2Zr Magnesium Alloy" published in 2014, it was reported that the cast structure of the highly alloyed Mg-9Gd-8Y-2Nd-1.2Zr magnesium alloy contains a large amount of intermetallic compounds, and the alloy content is as high as 20.2%, of which the rare earth content is as high as 19%. After a two-stage homogenization heat treatment of 520℃-8h+560℃-6h, the structure is uniform, and then extrusion is performed. After extrusion at 400℃, the performance of the Mg-9Gd-8Y-2Nd-1.2Zr magnesium alloy is optimal, with a yield strength of 189MPa, a tensile strength of 283MPa, and an elongation of 16%. It is found from the above-mentioned prior art that in order to improve the strength and elongation, high-energy-consuming methods such as adding high-content alloying elements and rare earth elements to magnesium alloys, performing long-term high-temperature homogenization treatment, and high-temperature extrusion are adopted, and the addition of a large amount of rare earth elements not only increases the production cost, but also produces harmful second phases, affecting the performance of the alloy. It can be seen from this that in order to improve the strength and plasticity of the alloy, the prior art needs to increase the content of alloying elements and rare earths, which increases the production cost, and adopts complex preparation processes such as high-temperature and long-term heat treatment and high-temperature deformation, which have long processes and high energy consumption, which greatly limits the production and application of the alloy. Therefore, the development of a magnesium alloy with simple process, easy production, low alloy content and high strength and plasticity has become a technical problem that needs to be solved urgently. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a microalloyed high-strength plastic high-efficiency extruded magnesium alloy, which is composed of the following components by mass percentage: bismuth: 0.4-2.2wt.%, manganese: 0.3-0.6wt.%, zinc: 0.2-0.5wt.%, cerium: 0.4-0.7wt.%, inevitable impurity content ≤0.05%, the balance is magnesium, and the alloy component content is ≤4wt.%;
[0004] The method for preparing the magnesium alloy comprises the following steps:
[0005] (1) According to the proportion of alloy components, pure magnesium, magnesium-manganese master alloy, magnesium-cerium master alloy, pure bismuth and pure zinc are sequentially smelted at 570-710° C. under the protection of a mixed gas of CO2 and SF6 with a volume ratio of 95-99:5-1, and after the alloy is completely melted, it is stirred and slag removed for 5-20 minutes, argon gas is introduced, and it is kept at room temperature for 15-30 minutes to obtain an alloy melt, and the alloy melt is poured into a mold preheated to 150-250° C. by gravity casting to obtain a magnesium alloy ingot;
[0006] (2) lathing the alloy ingot obtained in step (1) to obtain a magnesium alloy billet;
[0007] (3) hot extrusion: preheating the billet obtained in step (2) and the extrusion die at 300-320° C. for 2-3 hours, and then extruding the billet at 300-320° C., with an extrusion speed of 8-10 m / min and an extrusion ratio of 25-30:1, to obtain a microalloyed high-strength, high-plasticity and high-efficiency extruded magnesium alloy, wherein the average grain size of the magnesium alloy is ≤2.8 μm, the yield strength of the alloy is ≥274 MPa, the tensile strength is ≥300 MPa, and the elongation is ≥16.7%.
[0008] Furthermore, in terms of mass percentage, the bismuth is 0.5-2.1wt.%, manganese is 0.4-0.55wt.%, zinc is 0.3-0.45wt.%, and cerium is 0.5-0.65wt.%.
[0009] Furthermore, the average grain size of the magnesium alloy obtained in step (3) is 1.5-2.5 μm.
[0010] Compared with the prior art, the present invention has the following characteristics:
[0011] Compared with the prior art, the present invention achieves the following advantages through the coordinated regulation of alloy component ratios, processes and process parameters, and only within the scope of protection of the claims of the present invention: the present invention obtains a micro-alloyed high-strength, high-plastic and high-efficiency extruded magnesium alloy through the synergistic effect of low-alloy component design and preparation process, which has good comprehensive mechanical properties and is of great significance in the field of engineering industrialization applications.
[0012] (1) The prior art adds high-content alloying elements and high-content rare earth elements, and adopts high-temperature and long-time heat treatment, high-temperature hot extrusion and other processes. However, the heat treatment processes such as long-time solid solution or homogenization are time-consuming and labor-intensive, which significantly increase the production cost and production time. The present invention reduces the amount of alloy and rare earth alloy added, optimizes the alloy preparation process, omits the high-temperature and long-time solid solution or homogenization and other heat treatment processes, shortens the alloy preparation process by directly performing rapid extrusion, reduces energy consumption, and can achieve an extrusion speed of ≥8m / min, significantly improving the extrusion speed, breaking the technical bottleneck that the existing slow extrusion and rapid extrusion will cause the alloy to crack, improving the alloy production efficiency, and facilitating industrial production;
[0013] (2) In addition, the existing high-content alloyed magnesium alloys achieve the improvement of alloy mechanical properties through second phase strengthening, fine grain strengthening or solid solution strengthening, but a coarse second phase will be generated in the process, causing the alloy to crack during subsequent deformation. The alloying elements added in the present invention have a low content, the total weight percentage of alloy components is ≤4wt.%, and the rare earth content is ≤0.7wt.%, which meets the requirements of lightweight alloy materials and significantly reduces the cost of raw materials. The preferred alloying elements can interact with each other during alloy deformation, and achieve multiple strengthening effects such as second phase grain refinement, grain refinement, second phase strengthening, a large number of nano-scale thermally stable phases, dispersed phases, bimodal structures, and grain boundary segregation, including the formation of a high melting point nano-scale second phase with a size of less than 50nm, pinning dislocations, refining grains, and improving alloy strength and plasticity. At the same time, the formed nano-scale fine particles are dispersed in the matrix, promoting dynamic recrystallization, and segregating at the grain boundaries, effectively improving the thermal stability of the grain boundaries. The bimodal structure formed by the dynamically recrystallized grains and the non-recrystallized areas along the extrusion direction, while a large amount of non-basal slip is activated, the deformation ability and comprehensive performance of the alloy are enhanced, so that the alloy still does not crack under a large extrusion ratio and rapid extrusion.
[0014] (3) Compared with the prior art, the present invention achieves the following advantages through the interaction between alloy components, proportions, processes and synergistic regulation of process parameters, and only within the scope of protection of the claims of the present invention: simultaneous significant refinement of the alloy microstructure and improvement of the alloy strength and elongation, wherein the average grain size is ≤2.8μm, the yield strength is ≥274MPa, the tensile strength is ≥300MPa, and the elongation is ≥16.7%. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a room temperature mechanical property curve of magnesium alloy 1 obtained in Example 1. DETAILED DESCRIPTION
[0016] Example 1
[0017] The alloy is composed of the following components in mass percentage: Bi: 0.5wt.%, Mn: 0.4wt.%, Zn: 0.3wt.%, Ce: 0.6wt.%, inevitable impurity content ≤ 0.05%, and the balance is Mg; the preparation method comprises the following steps:
[0018] (1) According to the proportion of alloy components, pure magnesium, magnesium-manganese master alloy, magnesium-cerium master alloy, pure bismuth and pure zinc are smelted in sequence at 580-700° C. under the protection of a mixed gas of CO2 and SF6 in a volume ratio of 99:1, and after the alloy is completely melted, it is stirred and slag removed for 5-10 minutes, argon gas is introduced, and the alloy is kept at a temperature for 15-20 minutes to obtain an alloy melt, and the alloy melt is injected into a mold preheated at 150-250° C. by gravity casting to obtain a magnesium alloy ingot.
[0019] (2) lathing the alloy ingot obtained in step (1) to obtain a magnesium alloy billet;
[0020] (3) Hot extrusion: preheat the billet and the extrusion die obtained in step (2) at 300° C. for 2 hours, and then extrude the billet at 300° C. at an extrusion speed of 10 m / min and an extrusion ratio of 28:1 to obtain a microalloyed high-strength, plastic and high-efficiency extruded magnesium alloy 1, the grain size of the alloy being 2.17 μm, the yield strength of the alloy being 286 MPa, the tensile strength being 308 MPa, and the elongation being 18.2%.
[0021] Example 2
[0022] The alloy is composed of the following components in mass percentage: Bi: 1.3wt.%, Mn: 0.6wt.%, Zn: 0.4wt.%, Ce: 0.5wt.%, inevitable impurity content ≤ 0.05%, and the balance is Mg; the preparation method comprises the following steps:
[0023] (1) According to the proportion of alloy components, pure magnesium, magnesium-manganese master alloy, magnesium-cerium master alloy, pure bismuth and pure zinc are smelted in sequence at 590-710° C. under the protection of a mixed gas of CO2 and SF6 in a volume ratio of 97:3, and after the alloy is completely melted, it is stirred and slag removed for 8-10 minutes, argon gas is introduced, and it is kept at a temperature for 15-25 minutes to obtain an alloy melt, and the alloy melt is injected into a mold preheated at 150-250° C. by gravity casting to obtain a magnesium alloy ingot.
[0024] (2) lathing the alloy ingot obtained in step (1) to obtain a magnesium alloy billet;
[0025] (3) Hot extrusion: preheat the billet and the extrusion die obtained in step (2) at 310° C. for 2.5 hours, and then extrude the billet at 310° C. at an extrusion speed of 8.5 m / min and an extrusion ratio of 25:1 to obtain a microalloyed high-strength, plastic and high-efficiency extruded magnesium alloy 2, the grain size of the alloy being 2.5 μm, the yield strength being 278 MPa, the tensile strength being 300 MPa, and the elongation being 17.3%.
[0026] Example 3
[0027] The alloy is composed of the following components in mass percentage: Bi: 2.2wt.%, Mn: 0.6wt.%, Zn: 0.5wt.%, Ce: 0.7wt.%, inevitable impurity content ≤ 0.05%, and the balance is Mg; the preparation method comprises the following steps:
[0028] (1) According to the proportion of alloy components, pure magnesium, magnesium-manganese master alloy, magnesium-cerium master alloy, pure bismuth and pure zinc are smelted in sequence at 570-710° C. under the protection of a mixed gas of CO2 and SF6 in a volume ratio of 98:2, and after the alloy is completely melted, it is stirred and slag removed for 8-15 minutes, argon gas is introduced, and it is kept at a temperature for 20-25 minutes to obtain an alloy melt, and the alloy melt is injected into a mold preheated at 150-250° C. by gravity casting to obtain a magnesium alloy ingot.
[0029] (2) lathing the alloy ingot obtained in step (1) to obtain a magnesium alloy billet;
[0030] (3) Hot extrusion: The billet and the extrusion die obtained in step (2) were preheated at 320° C. for 3 hours, and then the billet was extruded at 320° C. with an extrusion speed of 9 m / min and an extrusion ratio of 27:1 to obtain a microalloyed high-strength, plastic and high-efficiency extruded magnesium alloy 3, the grain size of the alloy was 2.8 μm, the yield strength was 274 MPa, the tensile strength was 305 MPa, and the elongation was 16.7%.
[0031] Comparative Example 1
[0032] The master's thesis entitled "Effect of Sn and Sr Composite Addition on Microstructure and Mechanical Properties of Mg-4Al-0.4Mn Alloy" was published. It was mentioned in the experiment that the addition of Sn and Sr elements to the Mg-4Al-0.4Mn alloy resulted in the best-performing Mg-4Al-0.4Mn-1.2Sn-0.6Sr magnesium alloy, which was calculated by mass percentage as follows: Al: 4wt.%, Mn: 0.4wt.%, Sn: 1.2wt.%, Sr: 0.6wt.%, and the balance was Mg. Before hot extrusion deformation, the alloy was homogenized at 420℃-12h, and then hot extruded at an extrusion temperature of 390℃, with an extrusion ratio of 16:1 and an extrusion outlet rate of 0.96m / min. The average grain size of the alloy obtained was 6.7μm, the room temperature yield strength was 239MPa, the tensile strength was 269MPa, and the elongation was 9.32%. Compared with the present invention, the cast alloy of comparative example 1 was homogenized for a long time before extrusion, and the extrusion temperature was higher than all embodiments of the present invention, and the extrusion speed was lower than the embodiments of the present invention, which had a complex process and high energy consumption, and was not conducive to industrial production. At the same time, the amount of alloying elements added in comparative example 1 (6.2wt.%) was much higher than the maximum amount of alloying elements added in the present invention (≤4wt.%), and the alloy component content used in the present invention was lower than that in comparative example 1. In addition, although the trace amount of Sn and Sr added in comparative example 1 can form a highly thermally stable second phase and play a role in refining the grains, the grain size of the alloy is still larger than the maximum grain size (2.8μm) of the alloy of the present invention, and the highest mechanical properties and plasticity of the alloy are lower than the lowest mechanical properties and plasticity of the present invention. In summary, compared with comparative example 1, the alloy content of the present invention is low, the long-term heat treatment process is omitted, the extrusion temperature is low, the extrusion speed is fast, and the lowest mechanical properties and plasticity of the alloy are higher than those of comparative example 1 under the premise of low energy consumption and easy production, so as to achieve the simultaneous improvement of strong plasticity.
[0033] Comparative Example 2
[0034] The master's thesis entitled "Study on Extrusion Process and Microstructure Performance of Mg-9Gd-8Y-2Nd-1.2Zr Magnesium Alloy" was published. It was mentioned in the experiment that the selected Mg-9Gd-8Y-2Nd-1.2Zr alloy (the alloy element addition amount of Example 2 (20.2wt.%) is higher than the maximum alloy element addition amount of the present invention (4wt.%), and a large amount of expensive rare earth elements (19wt.%) are added, while the present invention adds ≤0.7wt.% of rare earth elements). Before hot extrusion, Example 2 was subjected to a two-stage homogenization heat treatment of 520℃-8h+560℃-6h (while the present invention did not perform any heat treatment process before extrusion), and then hot extruded at a temperature of 350℃-450℃, with an extrusion ratio of 9-25:1, an extrusion speed of 5mm / min, an average grain size of 12μm, a yield strength of 189MPa, a tensile strength of 283MPa, and an elongation of 16%. Compared with Comparative Example 2, the extrusion temperature of the present invention (maximum 320°C) is lower than the minimum extrusion temperature of Comparative Example 2, and the extrusion ratios of the two are different. The minimum extrusion speed of the present invention (8m / min) is much greater than the extrusion speed of the alloy of Comparative Example 2 (5mm / min), and the average grain size (≤2.8μm) is much smaller than the grain size of the alloy of Comparative Example 2 (12μm). The minimum strength and plasticity of the alloy of the present invention are respectively greater than the maximum strength and plasticity of the alloy obtained in Comparative Example 2. In summary, compared with Comparative Example 2, the present invention has a small amount of alloy element addition, low energy consumption in the extrusion scheme, and realizes rapid extrusion, which is suitable for industrial production, and the comprehensive mechanical properties of the alloy obtained are higher than those of Comparative Example 2. Under the premise of saving raw materials and time costs, the present invention achieves simultaneous improvement of strength and plasticity.
[0035] Comparative Example 3
[0036] The alloy is composed of the following components in mass percentage: Bi: 0.3wt.%, Mn: 0.2wt.%, Zn: 0.1wt.%, Ce: 0.3wt.%, inevitable impurity content ≤ 0.05%, and the balance is Mg; the preparation method comprises the following steps:
[0037] (1) According to the proportion of alloy components, pure magnesium, magnesium-manganese master alloy, magnesium-cerium master alloy, pure bismuth and pure zinc were smelted in sequence at 720°C under the protection of a mixed gas of CO2 and SF6 in a volume ratio of 93:7. After the alloy was completely melted, it was stirred and slag removed for 4 minutes, argon gas was introduced, and it was kept at room temperature for 13 minutes to obtain an alloy melt. The alloy melt was poured into a mold preheated to 145°C by gravity casting to obtain a magnesium alloy ingot.
[0038] (2) lathing the alloy ingot obtained in step (1) to obtain a magnesium alloy billet;
[0039] (3) Hot extrusion: The billet obtained in step (2) and the extrusion die are preheated at 280° C. for 4 hours, and then the billet is extruded at 280° C. with an extrusion speed of 7 m / min and an extrusion ratio of 24:1 to obtain an extruded magnesium alloy with a grain size of 5.8 μm, a yield strength of 205 MPa, a tensile strength of 224 MPa, and an elongation of 8.2%.
[0040] Comparative Example 3 uses similar components and processes as those used in the present invention, but the relevant component ratios and process parameters are not within the scope of protection of the claims of the present invention. As a result, the maximum grain size (2.8 μm) of the alloy obtained by the present invention is smaller than the grain size (5.8 μm) of Comparative Example 3, and the minimum strength and plasticity are higher than the relevant properties of the alloy obtained in Comparative Example 3.
[0041] In summary, the prior art increases the alloy element content or adds high rare earth element content, and adopts complex processes such as high temperature heat treatment and low extrusion speed, which results in high energy consumption, and it is difficult to achieve simultaneous improvement in the strength and plasticity of the obtained alloy. Compared with the prior art, the present invention uses less raw material addition content and controls the alloy content to ≤4wt.%, thereby reducing costs and having the advantage of being lightweight. It omits heat treatment processes such as high temperature and long-term solid solution or homogenization, has a simple production process, and uses an extrusion speed higher than the prior art. In addition, the component ratios and process parameters used in Examples 1-3 of the present invention are different, among which the alloy obtained in Example 1 has the best comprehensive performance, but its alloy addition amount is not the highest. In summary, the present invention achieves a large number of nano-scale products through the synergistic regulation of the interaction, ratio, process and process parameters between the alloy components. Under the multiple strengthening effects of thermally stable phase, dispersed phase, bimodal structure, grain boundary segregation, etc., the technical bottleneck of slow extrusion in the prior art and avoiding cracks caused by rapid extrusion in the prior art is broken, and the mechanical properties of the obtained micro-alloyed high-strength plastic high-efficiency extruded magnesium alloy are higher than those of the magnesium alloy obtained by the prior art. Compared with the prior art, the present invention improves the microstructure of the alloy while simultaneously improving the strength and plasticity of the alloy to realize industrial production. Only within the scope of protection of the claims of the present invention can the average grain size of the alloy be ≤2.8μm, the yield strength be ≥274MPa, the tensile strength be ≥300MPa, and the elongation be ≥16.7%.
Claims
1. A micro-alloyed high-strength, high-plasticity and high-efficiency extruded magnesium alloy. Features: In terms of mass percentage, the alloy consists of the following components composition: Bismuth: 0.4-2.2wt.%, manganese: 0.3-0.6wt.%, zinc: 0.2-0.5wt.%, cerium: 0.4-0.7wt.%, inevitable impurity content ≤0.05%, the balance is magnesium, the alloy component content ≤4wt.%; The method for preparing the magnesium alloy comprises the following steps: (1) According to the alloy composition ratio, the volume ratio of CO is 95-99:5-1. 2 and SF 6 Under the protection of a mixed gas, pure magnesium, magnesium-manganese master alloy, magnesium-cerium master alloy, pure bismuth and pure zinc are sequentially smelted at 570-710°C, and after the alloy is completely melted, it is stirred and slag removed for 5-20 minutes, argon gas is introduced, and it is kept still for 15-30 minutes to obtain an alloy melt, and the alloy melt is poured into a mold preheated at 150-250°C by gravity casting to obtain a magnesium alloy ingot; (2) lathing the alloy ingot obtained in step (1) to obtain a magnesium alloy billet; (3) hot extrusion: preheating the billet obtained in step (2) and the extrusion die at 300-320° C. for 2-3 hours, and then extruding the billet at 300-320° C., with an extrusion speed of 8-10 m / min and an extrusion ratio of 25-30:1, to obtain a microalloyed high-strength, high-plasticity and high-efficiency extruded magnesium alloy, wherein the average grain size of the magnesium alloy is ≤2.8 μm, the yield strength of the alloy is ≥274 MPa, the tensile strength is ≥300 MPa, and the elongation is ≥16.7%.
2. A microalloyed high-strength, high-plasticity and high-efficiency extruded magnesium alloy according to claim 1, Features: Calculated by mass percentage, the bismuth is 0.5-2.1wt.%, manganese is 0.4-0.55wt.%, zinc is 0.3-0.45wt.%, and cerium is 0.5-0.65wt.%.
3. A microalloyed high-strength, high-plasticity and high-efficiency extruded magnesium alloy according to claim 1 or 2, Features: The average grain size of the magnesium alloy obtained in step (3) is 1.5-2.5 μm.