Preparation method of TiC-Ti3AlC2 toughened alpha2-Ti3Al base with core-ring structure
By preplacing the mixture of Ti and Al element powders with WC ceramic powder on the surface of the titanium alloy, combined with laser cladding and scanning electron beam modification technology, the electron beam technology in coating preparation is solved. The problem in this paper significantly improves the high-temperature wear resistance and mechanical properties of the surface of titanium alloy.
Patent Information
- Application Number
- CN202411158333.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-15
Smart Images

Figure CN118957571A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for enhancing high temperature wear resistance of a TiAl / WC cladding layer modified by a scanning electron beam, and in particular to a method for preparing a TiC-Ti3AlC2 toughened α2-Ti3Al-based layer with a core-ring structure. Background Art
[0002] At present, titanium alloys and titanium aluminides account for one-third of the weight of modern aircraft engines, becoming the second most popular engine material after nickel-based high-temperature alloys. Among them, TC21 titanium alloy has many attractive advantages such as high specific strength, excellent corrosion resistance, and stable temperature strength. However, TC21 titanium alloy also faces the common problems of low surface hardness and insufficient wear resistance, which limits its application as a high-temperature component of contemporary aircraft engines. The current mainstream treatment method is to prepare a specific strengthening coating on the metal surface, and carbide ceramic coatings have characteristics that make them suitable for operating scenarios that require harsh use conditions. In particular, WC is one of the most widely used ceramic carbide materials, with excellent hardness, high temperature resistance and wear resistance. It is mixed with metal materials to form a composite powder system that is developing rapidly.
[0003] For aircraft engines, the core performance indicator is the engine's thrust-to-weight ratio. Among various metal-based materials, TiAl coating, a new type of lightweight high-temperature structural material, is the most widely studied protective coating. Under high temperature conditions, TiAl alloy has both good creep resistance and certain antioxidant capacity, and the yield strength of TiAl alloy is much higher than that of titanium alloy. Moreover, TiAl alloy is similar to titanium alloy in composition, has a lower thermal expansion coefficient, and its thermal expansion coefficient changes with temperature are close to some typical structural materials, making it easy to metallurgically bond. Therefore, it is irreplaceable to prepare high-temperature coating materials using Ti powder and Al powder as binders and WC as reinforcing particles. In addition, the Ti-Al-C MAX phase is formed inside the coating, which is of great significance as the second phase to regulate and enhance the toughness and high-temperature resistance of the coating, thereby giving the coating a wider range of applications.
[0004] With the vigorous development of surface engineering technology, the surface of titanium alloy is particularly suitable for the preparation of coatings by thermal spraying, cold spraying, laser cladding, etc. Thermal spraying technology is to heat the raw alloy powder to a molten or semi-molten state, and then deposit and rapidly solidify it on the metal substrate. Unlike thermal spraying, cold spraying, as a solid-state process, can deposit the powder on the substrate through strong plastic deformation caused by high-speed impact below the melting temperature. However, the introduction of suitable ceramic reinforcement materials in alloy powder for spraying process still faces challenges in improving the quality and performance of coatings. The inherent deficiencies of thermal spraying and cold spraying, including limited bonding between particles and between coating and substrate, cannot fully meet extremely harsh service environments, such as high temperature, high wear and high fatigue environments. In contrast, laser cladding preparation achieves a dense protective coating that exhibits a strong metallurgical bond with the substrate. Laser cladding can react to produce favorable phase-enhanced coatings, such as ceramic reinforcement phases, self-lubricating phases, etc. Therefore, LC technology occupies an important position in the field of metal coatings. Sui et al. (Sui X, Weng Y, Zhang L, et al. Uncovering the Effect of CeO2 on the Microstructure and Properties of TiAl / WC Coatings on Titanium Alloy[J]. Coatings, 2024, 14(5):543.) successfully prepared Ti-Al / WC composite coating on the surface of titanium alloy by laser cladding technology. They found that hard TiC and self-lubricating Ti2AlC MAX phase were generated in situ, and the hardness and wear resistance of the cladding layer were significantly improved.
[0005] It is well known that Ti3AlC2MAX phase has better self-lubricating properties than Ti2AlC MAX phase in terms of hardness and wear resistance, which makes Ti3AlC2 potentially perform better in friction applications. However, Ti3AlC2 phase requires higher energy density to accelerate the interaction between Ti and Al elements and C elements to generate.
[0006] At present, electron beam technology, as one of the high-energy beams, is considered to be an effective modification method that can enhance surface properties and optimize microstructure without changing the substrate material. Because it has a higher energy density than laser, it can promote a more uniform distribution of Ti, Al and C elements in the coating. In addition, grain refinement can be achieved under sudden heating and extreme cooling to greatly improve material performance. The extremely fast cooling rate will reduce the formation of undesirable phases and is conducive to the formation of stable Ti3AlC2 MAX phase. At the same time, electron beam material modification is carried out in a vacuum environment to ensure that there are no pollutants or impurities, low energy consumption and high reliability. However, the key problem of electron beam technology is that it is not suitable for the preparation of coatings. On the one hand, the airflow generated in the vacuum chamber at the moment of evacuation will take away the powdered material; on the other hand, the force of the electron beam on the metal powder changes the accumulation state of the powder, limiting its good application in coating. Summary of the invention
[0007] The purpose of the present invention is to effectively solve the problem that electron beam technology is not suitable for preparing coatings, and to provide a preparation method for generating a TiC-Ti3AlC2 reinforced α2-Ti3Al-based preparation having a core-ring structure in a TiAl / WC coating, thereby enhancing the high temperature wear resistance of the coating.
[0008] The technical solution for achieving the purpose of the present invention is: A method for preparing a TiC-Ti3AlC2 toughened α2-Ti3Al-based core-ring structure, firstly, powders including Ti and Al elements are mixed evenly with WC ceramic powder, and after mixing, the powders are pre-placed on the surface of titanium alloy or titanium aluminum alloy to form a pre-coating layer; Then, the pre-coated layer is laser clad to obtain a titanium alloy or titanium aluminum alloy with a TiAl / WC cladding layer; Finally, the surface of the TiAl / WC cladding layer was modified by scanning electron beam to obtain a modified TiAl / WC coating. According to the preparation method, during the solidification process, TiC is preferentially precipitated into a "core" due to the low Gibbs free energy associated with the formation of TiC. The energy density and the cooling rate are changed by controlling the scanning speed, thereby causing the edge of the precipitated TiC phase to locally react with the unsolidified Ti-Al melt to generate a "ring" Ti3AlC2 MAX phase, forming a TiC-Ti3AlC2 core-ring structure, and further strengthening the metal matrix coating with the reinforcing phase, thereby greatly improving the mechanical properties and high-temperature wear resistance of the titanium-aluminum-based composite material.
[0009] Furthermore, the Ti powder of the pre-set powder raw material in the preparation method has a purity of ≥99.9% and ≥300 mesh; Al powder, purity ≥99.9%, 200~300 mesh; WC ceramic powder, purity ≥99.9%, particle size <10μm; The atomic ratio of Ti:Al is 1:1, and the WC ceramic particles are 20wt.%.
[0010] Furthermore, the Ti powder, Al powder and WC ceramic powder are prepared and then fully ground for 1-2 hours to make the powders evenly dispersed; The ground powder is placed in a vacuum drying oven and dried at 50-100°C for 12-36 hours to remove moisture from the powder. The obtained dry mixed powder is evenly coated on the surface of the sample to be clad to form a preset coating layer with a powder thickness of 1-2 mm.
[0011] Furthermore, the laser cladding machine in the preparation method performs cladding processing under the protection of high-purity argon gas, with a spot diameter of 3 mm, an operating wavelength of 1070 nm, a defocusing amount of 20 mm, a laser power of 900 W-1100 W, and a scanning speed of 3 mm / s-6 mm / s.
[0012] Furthermore, the preparation method uses a scanning electron beam to modify the surface of the TiAl / WC cladding layer, and the vacuum degree of the scanning electron beam is P≤6.5×10 -3 Pa, acceleration voltage is 58-62kV, scanning frequency is 300Hz, beam current is 2-6mA, scanning ring diameter is 4mm, and scanning speed is 2-10mm / s.
[0013] The preparation method of the present invention introduces WC ceramic particles into the TiAl-based coating, and C dissolves in the Ti-Al melt to react. When the solid solubility decreases, the core-ring structured TiC-Ti3AlC2, separate TiC and Ti3AlC2 MAX phases are evenly distributed on the α2-Ti3Al intermetallic matrix, which enhances toughness and improves the comprehensive performance of the cladding layer; the W atoms in the coating are evenly dispersed and pinned to the grain boundaries, thereby hindering the movement of the grain boundaries and the growth of grains. This pinning effect not only improves the thermal stability of the material, but also enhances the mechanical properties of the coating metal matrix, such as strength and hardness; the modified TiAl / WC cladding layer has good wettability with the titanium alloy matrix, and the distribution of Ti and Al atoms in the melting zone at the bottom of the coating naturally and evenly transitions to each other, and the interface metallurgical bonding is firm.
[0014] The preparation method of the present invention performs laser cladding on the pre-coating to obtain a titanium alloy with a cladding layer, and then uses a scanning electron beam to perform surface modification treatment on the coating. The modified TiAl / WC cladding layer has good molding quality and no obvious defects. The addition of an appropriate amount of carbide (<10wt.%) will improve the wettability and compatibility of the TiAl / WC cladding layer with the TC21 titanium alloy substrate.
[0015] In addition, since the gas generated by the thermal decomposition of the adhesive is easy to contaminate the surface of the titanium alloy and cause defects in the cladding layer, the method of the present invention does not use any adhesive.
[0016] Compared with the prior art, the present invention has the following beneficial effects: (1) The modified TiAl / WC composite cladding layer prepared by the present invention has a hardness of 609.6HV 0.1 ~780.1HV 0.1 , which is 1.69~2.17 times of TC21 titanium alloy substrate; the coating is 800 ◦ The average wear resistance at high temperature is 1.838~5.952h / mm 3 Its wear resistance is 1.379~4.47 times that of the substrate. This is mainly due to the presence of α2-Ti3Al intermetallic compounds, the formation of a large number of petal-shaped TiC-Ti3AlC2 core-ring structures, the formation of a single rigid supporting hard TiC, and the self-lubricating Ti3AlC2MAX phase, all of which contribute to a significant improvement in the comprehensive mechanical properties of the coating.
[0017] (2) Compared with the invention patent (patent number: CN107414086B, name: A carbide and titanium alloy layer synergistically strengthened TiAl-based alloy and its preparation method), there are essential differences. First, the metal ceramic powder is different. The ceramic powder of the authorized patent is TiC. Secondly, the composition ratio of Ti powder and Al powder is also different, which directly affects the chemical composition and structural properties of the coating. Secondly, the authorized patent is to alternately stack the mixed powder and the titanium alloy thin plate with a through structure layer by layer, and fill the through structure with the mixed powder, obtain the green body and then sinter it to obtain the carbide and titanium alloy layer synergistically strengthened TiAl-based alloy, while the present invention is to first prepare a pre-cladding coating by laser cladding technology with the mixed powder pre-placed on the surface of the titanium alloy, and then use a scanning electron beam to perform surface modification on the cladding layer to obtain a carbide and TiAl intermetallic compound synergistically strengthened titanium alloy. Finally, the authorized patent is about the reaction of TiC with Ti-Al alloy to generate carbides Ti2AlC and Ti3AlC2, while the present invention is about the reaction of WC with Ti-Al alloy to generate carbides TiC and Ti3AlC2, forming a core-ring structure of TiC-Ti3AlC2, which has more competitive advantages in high-temperature and harsh service environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the X-ray diffraction pattern of the modified TiAl / WC cladding layer described in Example 2 of the present invention (scanning speed is 6 mm / s); Figure 2 This is a SEM image showing the microstructure of the modified TiAl / WC cladding layer described in Example 2 of the present invention (scanning speed is 6 mm / s). DETAILED DESCRIPTION
[0019] The present invention is described in detail below in conjunction with the embodiments and drawings, but they should not be construed as limiting the protection scope of the present invention. Example 1
[0020] A method for preparing a TiC-Ti3AlC2 toughened α2-Ti3Al-based core-ring structure, comprising the following steps: (1) The TC21 titanium alloy block was wire-cut into 30 mm × 15 mm × 8 mm rectangular specimens. The surface of each specimen was grinded and polished with 180-grit sandpaper to remove the oxide layer to ensure the flatness and smoothness of the surface to be clad. The specimen was ultrasonically cleaned with alcohol to remove oil stains. Finally, the pretreated TC21 titanium alloy matrix specimen was dried. (2) Pre-preparing powder raw materials according to the atomic ratio of Ti:Al of 1:1 and WC ceramic particles of 20wt.%, mixing the powders including Ti and Al elements with WC ceramic powder and grinding them thoroughly for 1.5h to make the powders evenly dispersed; The ground powder was placed in a vacuum drying oven and dried at 50°C for 24 hours to remove moisture from the powder. The obtained dry mixed powder was evenly coated on the surface of the TC21 titanium alloy sample to be clad to form a pre-coated layer with a powder thickness of 1 mm. (3) performing laser cladding on the pre-deposited coating layer to obtain a titanium alloy having a TiAl / WC cladding layer; The laser cladding machine performs cladding processing under the protection of high-purity argon gas, with a protective gas flow rate of 15L / min, a spot diameter of 3mm, an operating wavelength of 1070nm, a defocus amount of 20mm, a laser power of 1000W, and a scanning speed of 3mm / s; (4) The surface of the TiAl / WC cladding layer is modified by a scanning electron beam to obtain a modified TiAl / WC coating; The vacuum degree of the scanning electron beam equipment is P≤6.5×10 -3 Pa, acceleration voltage is 60 kV, scanning frequency is 300 Hz, beam current is 4 mA, scanning ring diameter is 4 mm, scanning speed is 4 mm / s; (5) The modified TiAl / WC coating was subjected to standard mechanical grinding and polishing treatment, and then etched with Kroll reagent (a liquid mixture of 2 ml HF, 4 ml HNO3 and 100 ml H2O) at room temperature for about 15 s. X-ray diffraction and microstructure characterization SEM were performed, and the cross-sectional hardness of the sample along the depth direction and the surface high temperature wear resistance at 800°C were tested. Example 2
[0021] The laser cladding sample prepared in Example 1 was subjected to scanning electron beam modification, and the specific treatment method was as follows: The surface of the TiAl / WC cladding layer was modified by scanning electron beam to obtain a modified TiAl / WC coating; the vacuum degree of the scanning electron beam equipment was P≤6.5×10 -3 Pa, accelerating voltage is 60 kV, scanning frequency is 300 Hz, beam current is 4 mA, scanning ring diameter is 4 mm, and scanning speed is 6 mm / s; The modified TiAl / WC coating was subjected to standard mechanical grinding and polishing, and then etched with Kroll reagent (a liquid mixture of 2 ml HF, 4 ml HNO3 and 100 ml H2O) at room temperature for about 15 s, and X-ray diffraction (such as Figure 1 ) and microstructure characterization SEM (as shown Figure 2 The cross-sectional hardness of the samples along the depth direction and the surface high temperature wear resistance at 800°C were tested.
[0022] from Figure 1 It can be seen that the modified coating is mainly composed of α-Ti, TiC, α2-Ti3Al and Ti3AlC2 phases. 39.1 ◦ The intensity of the diffraction peak at 39.1 is high and narrow, which indicates that the TiC content in the coating is high and the TiC grain size is also large. ◦ With the increase of TiC content, the content of Ti3AlC2 phase in the coating also increases.
[0023] from Figure 2 It can be seen that the microstructure of the modified layer is uniform without dendrite segregation. A large number of gray petal-like phases (core-ring structure TiC-Ti3AlC2), bright white rod-like phases (TiC), bright white needle-like phases (Ti3AlC2 MAX phases) and a small amount of dispersed spherical particles (α-Ti) are evenly distributed on the dark gray matrix. TiC as a reinforcing phase can promote the transformation of Ti3AlC2MAX phase to a core-ring structure, and the core-ring structure with undissolved TiC as the core and Ti3AlC2MAX phase solid solution as the ring phase can inhibit grain growth and improve the strength, hardness and toughness of the coating. Example 3
[0024] The laser cladding sample prepared in Example 1 was subjected to scanning electron beam modification, and the specific treatment method was as follows: The surface of the TiAl / WC cladding layer was modified by scanning electron beam to obtain a modified TiAl / WC coating; the vacuum degree of the scanning electron beam equipment was P≤6.5×10 -3 Pa, accelerating voltage is 60 kV, scanning frequency is 300 Hz, beam current is 4 mA, scanning ring diameter is 4 mm, and scanning speed is 8 mm / s; The modified TiAl / WC coating was subjected to standard mechanical grinding and polishing treatment, and then etched with Kroll reagent (a liquid mixture of 2 ml HF, 4 ml HNO3 and 100 ml H2O) at room temperature for about 15 s, and X-ray diffraction and microstructure characterization SEM were performed. The cross-sectional hardness of the sample along the depth direction and the surface high temperature wear resistance at 800°C were tested.
[0025] The friction and wear test of Examples 1 to 3 was carried out at 800°C for 30 minutes using a high-temperature CFT-1 comprehensive material tester. After the sample was clamped, the temperature in the furnace was increased from room temperature to 800°C at a rate of 10K / min, and then maintained at the working temperature for 30 minutes. During the friction and wear process, the Si3N4 ceramic ball was pressed into the surface of the substrate under the action of the load applied in the vertical direction, resulting in large plastic deformation, and then making high-speed reciprocating relative movement in the horizontal direction.
[0026] The test parameters are: normal load 5N, friction pair is a silicon nitride ball with a diameter of 4mm, motor speed is 300rpm, wear time is 30min, and wear scar length is 5mm.
[0027] Compared with the wear surfaces of the TC21 substrate and the TiAl / WC cladding layers modified in Examples 1 to 3 after dry sliding friction and wear tests at 800°C, the surface of the TC21 substrate is impacted by the grinding ball and produces severe plastic deformation. The wear surface morphology has deep furrows and many flaky adhesions, so the wear mechanism is mainly adhesive wear, accompanied by abrasive wear and oxidative wear.
[0028] The friction and wear morphology of the modified TiAl / WC cladding layer in Example 2 is smoother. The evenly distributed W atoms play a role in pinning the grain boundaries in the wear test, hindering the sliding of the grain boundaries and reducing the plastic flow of the α2-Ti3Al intermetallic compound matrix under the side effects of friction. There are a small amount of TiO2 wear oxidation debris, shallow furrows and flaky adhesions on the wear surface of the coating. The friction pair Si3N4 slides on the surface of the cladding layer to form a micro-cutting effect, inducing plastic deformation. At the same time, the formation of TiC and Ti3AlC2 hard phases slows down the degree of adhesive wear, and its wear mechanism is still abrasive wear. As the TiO2 wear debris continues to increase, the wear debris in the cutting process of the friction pair Si3N4 is added to the grinding process of the cladding layer, resulting in three-body wear. Therefore, it is shown that the TiAl / WC coating has slight adhesive wear, and abrasive wear and oxidation wear act together. A gray petal-like phase (core-ring structure TiC-Ti3AlC2) is generated, the hard TiC has a rigid supporting effect and the Ti3AlC2MAX phase has a self-lubricating effect, which significantly improves the high-temperature wear resistance of the surface.
[0029] The specific implementation modes of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes, and changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A TiC-Ti with a core-ring structure 3 AlC 2 Strengthening α 2 -Ti 3 Al-based preparation method, It is characterized in that The preparation method: First, powders including Ti and Al elements are mixed evenly with WC ceramic powder, and then pre-placed on the surface of titanium alloy or titanium aluminum alloy to form a pre-coating layer; Then, the pre-coated layer is laser clad to obtain a titanium alloy or titanium aluminum alloy with a TiAl / WC cladding layer; Finally, the surface of the TiAl / WC cladding layer was modified by scanning electron beam to obtain a modified TiAl / WC coating. In the preparation method, during the solidification process, due to the low Gibbs free energy associated with the formation of TiC, TiC is preferentially precipitated into a "core", and the energy density and cooling rate are changed by controlling the scanning speed, thereby causing the edge of the precipitated TiC phase to locally react with the unsolidified Ti-Al melt to form a "ring" Ti 3 AlC 2 MAX phase, forming TiC-Ti 3 AlC 2 The core-ring structure is formed, and the metal matrix coating is strengthened with the reinforcing phase to improve the mechanical properties and high temperature wear resistance of the titanium-aluminum matrix composite material.
2. The preparation method according to claim 1, Features: The Ti powder of the pre-set powder raw material has a purity of ≥99.9% and a mesh size of ≥300; Al powder, purity ≥99.9%, 200~300 mesh; WC ceramic powder, purity ≥99.9%, particle size <10μm; The atomic ratio of Ti:Al is 1:1, and the WC ceramic particles are 20wt.%.
3. The preparation method according to claim 2, Features: The Ti powder, Al powder and WC ceramic powder are mixed and fully ground for 1-2 hours to make the powders evenly dispersed; The ground powder is placed in a vacuum drying oven and dried at 50-100°C for 12-36 hours to remove moisture from the powder. The obtained dry mixed powder is evenly coated on the surface of the sample to be clad to form a preset coating layer with a powder thickness of 1-2 mm.
4. The preparation method according to claim 1, Features: The laser cladding machine performs cladding processing under the protection of high-purity argon gas, with a spot diameter of 3 mm, an operating wavelength of 1070 nm, a defocusing amount of 20 mm, a laser power of 900 W-1100 W, and a scanning speed of 3 mm / s-6 mm / s.
5. The preparation method according to claim 1, Features: The surface of the TiAl / WC cladding layer is modified by using a scanning electron beam, and the vacuum degree of the scanning electron beam is P≤6.5×10 -3 Pa, acceleration voltage is 58-62kV, scanning frequency is 300Hz, beam current is 2-6mA, scanning ring diameter is 4mm, and scanning speed is 2-10mm / s.