Preparation process and application of sulfur-doped nanorod electrode material

By doping trace sulfur elements on the surface of Bi2S3 nanorods to form sulfur-doped nanorod electrode materials with high active sites, the problems of reaction kinetics limitation and competitive reactions in electrocatalytic CO2 reduction technology are solved, and high selectivity and Stable CO2 reduction, especially under electrodes loaded with sulfur-doped nanorod electrode materials, the efficiency of CO2 conversion to formic acid reaches 95.6%.

CN118957666APending Publication Date: 2024-11-15ENERGY RES INST OF SHANDONG ACAD OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411164272.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Electrocatalytic CO2 reduction technology is affected by slow reaction kinetics limitations and competitive reaction hydrogen evolution reactions, resulting in lower selectivity and activity of CO2 reduction products.

Method used

The sulfur-doped nanorod electrode material is used to form more active sites by doping trace sulfur elements on the surface of Bi2S3 nanorods, thereby enhancing the activity of CO2 reduction reaction. Specific processes include reacting bismuth chloride and sodium sulfide in hydrochloric acid, washing and drying after forming a black solid product, preparing sulfur-doped nanorod electrode material with high selectivity and stability, and coating it on the electrode surface. To improve catalytic performance.

Benefits of technology

It achieves high selectivity and stability in electrocatalytic carbon dioxide reduction reaction, significantly improving the activity of CO2 reduction products. Especially under the electrodes loaded with sulfur-doped nanorod electrode materials, the efficiency of CO2 conversion to formic acid reaches 95.6%. And maintain high current density and Faraday efficiency within a wide potential range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957666A_ABST
    Figure CN118957666A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of CO2 electrocatalysis, and particularly discloses a preparation process and application of a sulfur-doped nanorod electrode material, and the preparation process comprises the following steps: S1, adding bismuth chloride into hydrochloric acid, and stirring until bismuth chloride is completely dissolved to obtain a solution A for later use; s2, adding sodium sulfide into hydrochloric acid, and stirring until sodium sulfide is completely dissolved to obtain a solution B for later use; and S3, dropwise adding the solution A into the solution B, stirring the mixed solution after adding, then separating out a black solid product, washing, and drying to constant weight to obtain the sulfur-doped nanorod electrode material. According to the invention, the Bi2S3 nanorod is used as a catalyst, more defects are obtained by doping S in the nanorod electrode material, and more active reaction sites are provided for the electro-catalysis process by optimizing the surface of the Bi2S3 nanorod through the unique nanorod-shaped structure and sulfur doping; therefore, high selectivity and stability are realized in the electro-catalysis carbon dioxide reduction reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of CO2 electrocatalysis technology, and in particular to a preparation process and application of a sulfur-doped nanorod electrode material. Background Art

[0002] With the rapid growth of the world's population and the rapid development of global industrialization, the consumption of fossil fuels has increased dramatically, and a large amount of carbon dioxide (CO2) has been emitted into the air, leading to the global greenhouse effect. It is urgent to develop technologies for the effective utilization of CO2. Electrocatalytic CO2 reduction (CO2RR) is a new CO2 resource technology that involves mild reaction conditions, simple operation, and controllable reaction steps, and has therefore received widespread attention. However, due to its chemical inertness, electrocatalytic CO2 reduction technology still suffers from slow reaction kinetics and the existence of a competing reaction, the hydrogen evolution reaction (HER), which results in low selectivity and activity of the CO2 reduction products. Summary of the invention

[0003] In view of the above problems, the present invention provides a preparation process and application of sulfur-doped nanorod electrode materials. The prepared S-doped bismuth nanorods are catalysts that exhibit high selectivity and stability in the electrocatalytic carbon dioxide reduction reaction. Specifically, the technical solution of the present invention is as follows.

[0004] First, the present invention discloses a preparation process of a sulfur-doped nanorod electrode material, comprising the following steps: S1. Add bismuth chloride to hydrochloric acid and stir until completely dissolved to obtain solution A for later use.

[0005] S2. Add sodium sulfide to hydrochloric acid and stir until completely dissolved to obtain solution B for later use.

[0006] S3, adding the solution A dropwise into the solution B, stirring the mixed solution after the addition, and then separating the black solid product, washing and drying to constant weight to obtain the sulfur-doped nanorod electrode material.

[0007] Further, in step S1, the mass volume ratio of the bismuth chloride to the hydrochloric acid is 1.20-1.30 g: 25 mL. Optionally, the concentration of the hydrochloric acid is 1 mol / L.

[0008] Furthermore, in step S1, the stirring time is not less than 30 min.

[0009] Further, in step S2, the mass volume ratio of the sodium sulfide to the hydrochloric acid is 400-550 mg: 25 mL. Optionally, the concentration of the hydrochloric acid is 1 mol / L.

[0010] Furthermore, in step S2, the stirring time is 3 to 4 minutes.

[0011] Further, in step S3, the solution A is added dropwise to the solution B according to the mass ratio of bismuth chloride to sodium sulfide of 2.4 to 3.3:1. Optionally, the stirring time is 10 to 20 min.

[0012] Furthermore, in step S3, the black solid product is washed with anhydrous ethanol until it becomes neutral.

[0013] Furthermore, in step S3, the drying temperature is 80-90°C.

[0014] Secondly, the present invention discloses the application of the sulfur-doped nanorod electrode material prepared by the above process in the electrochemical reduction of carbon dioxide to prepare formic acid.

[0015] Furthermore, in the electrochemical reduction of carbon dioxide to prepare formic acid, the electrode loaded with the sulfur-doped nanorod electrode material is used as a cathode electrode.

[0016] Furthermore, the sulfur-doped nanorod electrode material, acetylene black and an ethanol solution containing Nafion are uniformly mixed to form a slurry, and the slurry is coated on the electrode surface and then dried to obtain the cathode electrode.

[0017] Compared with the prior art, the present invention has the following beneficial technical effects: the present invention uses Bi2S3 nanorods as catalysts, and obtains more defects and active sites in the nanorod electrode material by S doping, and its unique nanorod structure and trace sulfur elements in situ doped into the surface of Bi2S3 nanorods during electrolysis form more sulfur defects for enhancing CO2RR activity, providing more active reaction sites for the electrocatalytic process, thereby achieving high selectivity and stability in the electrocatalytic carbon dioxide reduction reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein: Figure 1 The following is a scanning electron microscope image of the sulfur-doped nanorod electrode material prepared in Example 1 before and after the electro-reduction reaction; Figure 2 The X-ray diffraction pattern of the sulfur-doped nanorod electrode material prepared in the following Example 1 before and after the electro-reduction reaction; Figure 3 The following are X-ray photoelectron spectra of Bi and S elements of the cathode electrodes of Example 1 and Example 2; Figure 4 The Faraday efficiency diagram and LSV curve diagram of the electrode of the sulfur-doped nanorod electrode material prepared in the following Example 1; Figure 5 The current density curves and Faraday efficiency diagrams of the following Examples 6 and 7 are shown; Figure 6 The CV curves and electrochemical active area (ECSA) curves of the cathode electrode prepared in the following Example 5 at different scan rates. DETAILED DESCRIPTION

[0019] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0020] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. If not otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the described content can be applied to the method of the present invention. Now, the present invention is further described in conjunction with the accompanying drawings and specific embodiments of the present invention, and the preferred implementation methods and materials described in the present invention are only for demonstration purposes.

[0021] Embodiment 1: A preparation process of a sulfur-doped nanorod electrode material comprises the following steps: S1. Add 1.26 g of bismuth chloride to 25 mL of 1 mol / L hydrochloric acid and stir for 30 min to completely dissolve the bismuth chloride to obtain a transparent solution A for later use.

[0022] S2. Add 435 mg of sodium sulfide to 25 mL of 1 mol / L hydrochloric acid and stir for 4 min to completely dissolve the sodium sulfide to obtain a transparent solution B for later use.

[0023] S3. Add the solution A dropwise into the solution B, stir for 10 min after the solution is added, then collect the black solid product by centrifugation, wash the solid product by centrifugation four times with anhydrous ethanol, then dry the solid product in an oven at 85°C to constant weight, and grind it into powder to obtain sulfur-doped nanorod electrode material.

[0024] Performance test: 4 mg of the sulfur-doped nanorod electrode material prepared in this example and 2 mg of acetylene black were dispersed in 400 µL of ethanol solution (containing 25 µL of Nafion, the ethanol solution was a mixture of anhydrous ethanol and water in equal volumes), and then ultrasonicated for 30 min and drop-coated on the front and back surfaces of a carbon paper electrode (HCP030P). The single-side coating area was 1 cm 2 , the coating amount is 1.0 mg, and the cathode electrode is obtained after drying by irradiation with a baking lamp. The cathode electrode is used as the working electrode, the platinum sheet is used as the counter electrode, and the Ag / AgCl electrode is used as the reference electrode. The three-electrode electrochemical performance test is carried out on a Shanghai Chenhua electrochemical workstation (model CHI660E) using an H-type electrolytic cell filled with 0.5 M KHCO3 solution. Before the test, CO2 gas is introduced for 0.5 h to saturate the solution, and the constant gas flow rate is 20 mL / min. The bismuth sulfide nanorod electrode material is converted into sulfur-doped bismuth nanorods rich in sulfur defects by electroreduction at a potential of -1.0 V vs. RHE for 1 h.

[0025] Figure 1 Figure a in the middle is a scanning electron microscope image of the sulfur-doped nanorod electrode material prepared in this example, and it can be seen that its microscopic morphology is a nanorod structure. Figure 1 Figure b is a scanning electron microscope image of the sulfur-doped nanorod electrode material after the above-mentioned electro-reduction. It can be seen that the sulfur-doped nanorod electrode material still maintains the nanorod structure after electro-reduction, indicating that the sulfur-doped nanorod electrode material prepared in this embodiment has good structural stability.

[0026] Figure 2 Figure a is the XRD spectrum of the sulfur-doped nanorod electrode material prepared in this embodiment, and Figure b is the XRD spectrum of the doped nanorod electrode material after the above-mentioned electro-reduction. It can be seen that the composition before and after electro-reduction is consistent, indicating that the sulfur-doped nanorod electrode material prepared in this embodiment has good structural stability.

[0027] Figure 3 Figures a and b are the X-ray photoelectron spectra of the Bi element and the S element of the sulfur-doped nanorod electrode material prepared in this example, respectively. It can be seen that an obvious S 2s peak appears in Figure b, proving that the sulfur-doped nanorod electrode material is doped with sulfur.

[0028] Embodiment 2: 4 mg of the sulfur-doped nanorod electrode material prepared in Example 1 was dispersed in 400 mL of ethanol solution (containing 25 μL of Nafion, the ethanol solution was a mixture of anhydrous ethanol and water in equal volumes), and then ultrasonicated for 30 min and drop-coated on the front and back surfaces of a carbon paper electrode (HCP030P), with a single-side coating area of ​​1 cm2 The coating amount was 1.0 mg, and the cathode electrode was obtained after drying by irradiation with a baking lamp.

[0029] Figure 3 Figures c and d are the X-ray photoelectron spectra of the Bi element and the S element of the sulfur-doped nanorod electrode material prepared in this embodiment, respectively. As can be seen from the figure, there is a weak S2s peak, proving that part of the sulfur element is in-situ doped into the Bi nanorods during the electroreduction process of the sulfur-doped nanorod electrode material.

[0030] Embodiment 3: The cathode electrode prepared in Example 1 was used as the working electrode, the platinum sheet was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode. A three-electrode electrochemical performance test was performed on a Shanghai Chenhua electrochemical workstation (model CHI660E) using an H-type electrolytic cell filled with 0.5 M KHCO3 solution. Before the test, the CO2 gas was pre-bubbled for 20 min to saturate the solution, and the constant gas flow rate was 20 mL / min. The electrolysis was performed at a potential of -0.7 ~-1.2 V vs. RHE for 20 min each, and the gas after the electrolysis reaction was passed into a gas chromatograph for detection. Part of the electrolyte after the reaction was taken for nuclear magnetic resonance detection.

[0031] Test results such as Figure 4 As shown in a, the sulfur-doped nanorod electrode material maintains a high formic acid Faradaic efficiency (FE) over a wide potential. formate ≥90%), especially at a potential of -1.0 V vs. RHE, the FE of formic acid is 95.6%, which proves that sulfur doping in the sulfur-doped nanorod electrode material can effectively enhance the production of formic acid.

[0032] Embodiment 4: The cathode electrode prepared in Example 1 was used as the working electrode, the platinum sheet was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode. The three-electrode electrochemical performance test was performed on a Shanghai Chenhua electrochemical workstation (model CHI660E) using an H-type electrolytic cell filled with 0.5 M KHCO3 solution. The CO2 gas was pre-bubbled for 30 min to saturate the solution. The gas constant flow rate was 20 mL / min, and the scanning speed when testing the LSV curve was 20 mV·s -1 .

[0033] Test results such as Figure 4 As shown in Figure b, by comparing the saturated CO2 and saturated N2 electrolytes, it is shown that the sulfur-doped nanorod electrode material has a higher current density in the electrochemical CO2 reduction and indeed has excellent electrochemical performance, proving that the sulfur defects on the surface of the bismuth nanorods promote the catalytic activity of CO2 reduction.

[0034] Embodiment 5: The cathode electrode prepared in Example 1 was used as the working electrode, the platinum sheet was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode. The three-electrode electrochemical performance test was performed in a Shanghai Chenhua electrochemical workstation (model CHI660E) using an H-type electrolytic cell filled with 0.5 M KHCO3 solution. Before the test, CO2 gas was pre-bubbled for 30 min to saturate the solution. After CO2 was saturated, the CO2 gas was stopped and the stirring was turned off, and the CV curve was tested immediately.

[0035] The results are as follows Figure 6 As shown in a, a central potential is selected at different scanning speeds, and the double layer current corresponding to the potential is taken as the vertical axis and the potential is taken as the horizontal axis. The slope is the double layer capacitance C dl ,pass Figure 6 a That is, the CV curve represents the electrochemical active area of ​​the electrode material. Figure 6 As shown in b, the sulfur-doped nanorod electrode material has a higher electrochemically active area (ECSA). Its larger electrochemically active area is mainly attributed to its unique nanorod-like structure and the optimization of the Bi2S3 nanorod surface by sulfur doping, which provides more active reaction sites for the electrocatalytic process.

[0036] Embodiment 6: 4 mg of the sulfur-doped nanorod electrode material prepared in Example 1 and 2 mg of acetylene black were dispersed in 400 μL of ethanol solution (containing 25 μL of Nafion, the ethanol solution was a mixture of anhydrous ethanol and water in equal volumes), and then ultrasonicated for 30 min and drop-coated on the front and back surfaces of a carbon paper electrode (HCP030P), with a single-side coating area of ​​1.5 cm 2 The coating amount was 2.0 mg, and the cathode electrode was obtained after drying by irradiation with a baking lamp.

[0037] The cathode electrode of this embodiment was used as the working electrode, the platinum sheet was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode. The 1.0 M KOH electrolyte was flowed in the flow cell by a peristaltic pump (400 rpm), and the electrochemical performance test was performed on a Shanghai Chenhua electrochemical workstation (model CHI660E). During the test, CO2 gas was continuously introduced at a constant flow rate of 20 mL / min. The electrolysis was performed at a potential of -0.7~-1.4 V vs. RHE for 20 min each, and the gas after the electrolysis reaction was passed into a gas chromatograph for detection.

[0038] Test results such as Figure 5 As shown in b, the sulfur-doped nanorod electrode material exhibits a high FE in a wide potential range (-0.5~-1.4 V vs. RHE).formate (≥93%).

[0039] Embodiment 7: 4 mg of the sulfur-doped nanorod electrode material prepared in Example 1 and 2 mg of acetylene black were dispersed in 400 μL of ethanol solution (containing 25 μL of Nafion, the ethanol solution was a mixture of anhydrous ethanol and water in equal volumes), and then ultrasonicated for 30 min and drop-coated on the front and back surfaces of a carbon paper electrode (HCP030P), with a single-side coating area of ​​1.5 cm 2 The coating amount was 2.0 mg, and the cathode electrode was obtained after drying by irradiation with a baking lamp.

[0040] The cathode electrode of this embodiment was used as the working electrode, the platinum sheet was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode. The 1.0 M KHCO3 electrolyte was flowed in the flow cell by a peristaltic pump (400 rpm), and the electrochemical performance test was performed on a Shanghai Chenhua electrochemical workstation (model CHI660E). During the test, CO2 gas was continuously introduced at a constant flow rate of 20 mL / min. The electrolysis was performed for 20 min at a potential of -0.6~-1.3 V vs. RHE, and the gas after the electrolysis reaction was passed into a gas chromatograph for detection.

[0041] Test results such as Figure 5 As shown in c, the sulfur-doped nanorod electrode material exhibits a high formic acid Faradaic efficiency (≥92%) under a wide potential range (-0.7~-1.3Vvs. RHE). Comparative Example 6, when the electrolytes in the flow cell are KOH and KHCO3, respectively, Figure 5 As shown in a, when the electrolyte is KOH, the formic acid separation current density of the sulfur-doped nanorod electrode material is relatively large, that is, the electrode material exhibits excellent catalytic activity and selectivity in the synthesis of formic acid from CO2 under alkaline conditions.

[0042] Embodiment 8: A preparation process of a sulfur-doped nanorod electrode material comprises the following steps: S1. Add 1.2 g of bismuth chloride to 25 mL of 1 mol / L hydrochloric acid and stir for 30 min to completely dissolve the bismuth chloride to obtain a transparent solution A for later use.

[0043] S2. Add 400 mg of sodium sulfide to 25 mL of 1 mol / L hydrochloric acid and stir for 4 min to completely dissolve the sodium sulfide to obtain a transparent solution B for later use.

[0044] S3. Add the solution A dropwise into the solution B, stir for 20 min after the solution is added, then collect the black solid product by centrifugation, wash the solid product by centrifugation four times with anhydrous ethanol, then dry the solid product in an oven at 80°C to constant weight, and grind it into powder to obtain sulfur-doped nanorod electrode material.

[0045] Embodiment 9: A preparation process of a sulfur-doped nanorod electrode material comprises the following steps: S1. Add 1.3 g of bismuth chloride to 25 mL of 1 mol / L hydrochloric acid and stir for 30 min to completely dissolve the bismuth chloride to obtain a transparent solution A for later use.

[0046] S2. Add 550 mg of sodium sulfide to 25 mL of 1 mol / L hydrochloric acid and stir for 4 min to completely dissolve the sodium sulfide to obtain a transparent solution B for later use.

[0047] S3. Add the solution A dropwise into the solution B, stir for 20 min after the solution is added, then collect the black solid product by centrifugation, wash the solid product by centrifugation four times with anhydrous ethanol, then dry the solid product in an oven at 90° C. to constant weight, and grind it into powder to obtain sulfur-doped nanorod electrode material.

[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A process for preparing a sulfur-doped nanorod electrode material, characterized in that: The steps include: S1, add bismuth chloride to hydrochloric acid and stir until completely dissolved to obtain solution A, which is set aside; S2, adding sodium sulfide to hydrochloric acid and stirring until completely dissolved to obtain solution B, which is set aside; S3, adding the solution A dropwise into the solution B, stirring the mixed solution after the addition, and then separating the black solid product, washing and drying to constant weight to obtain the sulfur-doped nanorod electrode material.

2. The process for preparing the sulfur-doped nanorod electrode material according to claim 1, characterized in that: In step S1, the mass volume ratio of the bismuth chloride to the hydrochloric acid is 1.20-1.30 g:25 mL; optionally, the concentration of the hydrochloric acid is 1 mol / L.

3. The process for preparing the sulfur-doped nanorod electrode material according to claim 1, characterized in that: In step S1, the stirring time is not less than 30 min.

4. The process for preparing the sulfur-doped nanorod electrode material according to claim 1, characterized in that: In step S2, the mass volume ratio of the sodium sulfide to the hydrochloric acid is 400-550 mg:25 mL; optionally, the concentration of the hydrochloric acid is 1 mol / L.

5. The process for preparing the sulfur-doped nanorod electrode material according to claim 1, characterized in that: In step S2, the stirring time is 3 to 4 minutes.

6. The process for preparing the sulfur-doped nanorod electrode material according to claim 1, characterized in that: In step S3, the solution A is added dropwise to the solution B according to a mass ratio of bismuth chloride to sodium sulfide of 2.4-3.3:1; optionally, the stirring time is 10-20 min.

7. The process for preparing the sulfur-doped nanorod electrode material according to any one of claims 1 to 6, characterized in that: In step S3, the black solid product is washed with anhydrous ethanol until it becomes neutral; optionally, in step S3, the drying temperature is 80-90°C.

8. Use of the sulfur-doped nanorod electrode material obtained by the preparation process according to any one of claims 1 to 7 in the preparation of formic acid by electrochemical reduction of carbon dioxide.

9. The use according to claim 8, characterized in that: In the electrochemical reduction of carbon dioxide to prepare formic acid, the electrode loaded with the sulfur-doped nanorod electrode material is used as the cathode electrode.

10. The use according to claim 9, characterized in that: The sulfur-doped nanorod electrode material, acetylene black and ethanol solution containing Nafion are uniformly mixed to form a slurry, and the slurry is coated on the electrode surface and then dried to obtain the cathode electrode.

Citation Information

Patent Citations

  • Chemical preparation method of graphene-bismuth sulfide nanocomposite material

    CN102910617A

  • Method for preparing bismuth oxychloride / bismuth sulfide nanoflower heterojunction at room temperature in one step

    CN110227502A

  • Bismuth-based nano material as well as preparation method and application thereof

    CN111604046A

  • Bismuth sulfide-carbon nanomaterial as well as preparation method and application thereof

    CN115896857A