Comprehensive utilization method of bauxite resources

Through acid decomposition and high-temperature thermal reduction, the low utilization rate of bauxite resources and solid waste problems were solved, and high-efficiency production of high-silicon aluminum alloys and aluminum alloys was achieved, reducing production costs and solid waste generation.

CN118957685APending Publication Date: 2024-11-15吴一峰
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411245019.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing bauxite resource utilization rate is low, and a large amount of industrial solid waste and red mud is generated when producing alumina, and low-grade ores are difficult to directly use in the production of alumina, resulting in waste of resources and high production costs.

Method used

The bauxite is decomposed by acid method, and saturated chloride salts are generated through concentrated acid dissolution reaction. The components are initially separated by crystallization, and the high-silicon aluminum alloy and aluminum alloy are further produced in high-temperature thermal reduction and aluminum electrolysis method to control the reaction Conditions are used to retain the alumina component and reduce impurities dissolution.

Benefits of technology

It improves the utilization rate of bauxite resources, reduces separation costs and production costs, realizes efficient production of high-silicon aluminum alloys and aluminum alloys, and reduces the generation of industrial solid waste.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a comprehensive utilization method of bauxite resources, and belongs to the technical field of light metal metallurgy. The method comprises the following steps: decomposing bauxite by using concentrated acid (hydrochloric acid or sulfuric acid) at high temperature and high pressure to obtain a soluble salt mixture solution and insoluble substances such as silicon oxide, titanium oxide and undissolved aluminum oxide; and crystallizing and separating out salt crystals with the concentration reaching a saturated state by using a crystallization method. After the formed co-crystallized composite salt is re-dissolved, carbonate, hydroxide or oxide of alkali metal (sodium and potassium) and alkaline earth metal (calcium and magnesium) are used as a neutralization reaction precipitator, and precipitation, separation and purification are carried out respectively. And the dissolved-out slag is mixed with carbon, high-temperature smelting reduction is conducted to generate aluminum-silicon alloy, the smelting slag serves as a raw material for aluminum electrolysis, and aluminum and aluminum alloy are generated through the aluminum electrolysis process.
Need to check novelty before this filing date? Find Prior Art

Description

1. Technical Field

[0001] The invention discloses a method for comprehensive utilization of bauxite resources, belonging to the technical field of light metal metallurgy. 2. Background Technology

[0002] Bauxite is the main raw material for the production of alumina and metallic aluminum, and is also its main use. It includes gibbsite and diaspore. It mainly contains aluminum oxide, silicon oxide, and iron oxide, accounting for more than 80% of the mineral composition, followed by calcium oxide, magnesium oxide, potassium oxide, sodium oxide, titanium oxide, etc., as well as lithium, gallium, sulfur and rare metal elements.

[0003] At present, my country's alumina plants use the Bayer process technology to produce alumina, which has relatively high requirements for the grade of bauxite, and the resource recovery rate is often less than 70%. From bauxite to product alumina, it needs to go through crushing, grinding, pre-desiliconization, evaporation, dissolution, refining, seed decomposition, filtration, washing, calcination and other processes, which consumes a lot of energy and has high costs. Every ton of alumina produced will produce more than two tons of industrial solid waste - red mud.

[0004] Low-grade bauxite cannot be directly used in the Bayer process to produce alumina. Even large amounts of high-silicon bauxite with an aluminum-silicon ratio below 5 are difficult to produce alumina using the Bayer process.

[0005] There are two methods to produce alumina from bauxite: sintering method, Bayer method, and the so-called combined method that uses both methods. The soda lime sintering method can produce alumina from low-grade bauxite, but it has high energy consumption and high production costs. The modern aluminum industry no longer uses the sintering method to produce alumina. The Bayer process is the main process technology for producing alumina at present. It uses high-aluminum-silicon ratio rich ores and gibbsite ores, as well as concentrates obtained by beneficiation of medium and low-grade ores as raw materials. The aluminosilicate structure in bauxite is a very stable mineral structure, especially for diaspore-type bauxite in my country. It is very difficult to dissolve and extract aluminum. The soda lime method (traditional sintering method, Bayer method) is to replace aluminum ions in minerals with sodium and calcium ions by strengthening the reaction conditions, selectively dissolve aluminum ions, and generate sodium aluminate solution, while the rest forms a mixed precipitate, i.e. red mud. The reaction conditions controlled by the Bayer process for producing alumina dissolution are: temperature 140-270°C, pressure 0.4-7.0MPa, Na2O concentration 140-220g / l, and dissolution reaction time of about 30min-1h.

[0006] The modern aluminum industry still faces two thorny problems that are difficult to solve. The first is the low utilization and recovery rate of resources. Low-grade ores and beneficiation tailings are all waste resources. The second is that every ton of alumina produced will produce more than 2-3 tons of strongly alkaline red mud, which is still an industrial solid waste. Moreover, as the grade of bauxite is further reduced, a large amount of low-grade bauxite can no longer be used to produce alumina using the alkaline method.

[0007] Compared with the alkaline method which can only partially dissolve alumina, strong acids (concentrated hydrochloric acid, concentrated nitric acid, concentrated sulfuric acid) can completely dissolve aluminum in bauxite under high temperature and high pressure, and the aluminum exists in the solution in the form of aluminum salts. Compared with diaspore, which is more difficult to dissociate, gibbsite ore can be completely dissociated under high temperature and high pressure. When using concentrated hydrochloric acid and concentrated nitric acid, the insoluble matter includes silicon oxide; when using concentrated sulfuric acid, the insoluble matter includes silicon oxide, insoluble sulfates, etc. Considering the production cost and other factors, it is more advantageous to use hydrochloric acid or sulfuric acid.

[0008] The acid method for decomposing bauxite is not selective for aluminum. The aluminum, iron, sodium, potassium, calcium, magnesium, lithium, and rare earth elements in bauxite can all be dissolved into the solution and are difficult to separate and purify.

[0009] Under high temperature and high pressure, concentrated hydrochloric acid can basically dissolve all components in bauxite except silicon oxide to produce soluble chloride. The main chemical reaction formula is as follows:

[0010] Al2O3+6HCl=2AlCl3+3H2O

[0011] Fe2O3+6HCl=2FeCl3+3H2O

[0012] CaO+2HCl=CaCl2+H2O

[0013] MgO+2HCl=MgCl2+H2O

[0014] Li2O+2HCl=2LiCl+H2O

[0015] Na2O+2HCl=2NaCl+H2O

[0016] K2O+2HCl=2KCl+H2O

[0017] Re2O3+6HCl=2ReCl3+3H2O (Re is a rare earth element)

[0018] By controlling the dissolution reaction conditions, some easily soluble components in bauxite, such as iron, calcium, magnesium, lithium, etc., can be fully dissolved, while the more difficult to dissolve components, such as aluminum, titanium, etc., can only be partially dissolved and form slag together with silicon oxide, etc., which becomes the raw material for producing aluminum silicon alloy or aluminum silicon titanium alloy. Controlling the dissolution reaction conditions at a lower dissolution reaction temperature, lower acid concentration and longer dissolution reaction time is conducive to retaining more aluminum oxide components from being dissolved.

[0019] The chlorides that enter the solution can utilize the differences in solubility and concentration to precipitate the corresponding chloride salt crystals through crystallization of saturated solutions, so that various chlorides can be initially separated, creating conditions for further separation and purification.

[0020] Saturated solubility of main chlorides:

[0021] Ferrous chloride hexahydrate: 920 g / l (20°C);

[0022] Aluminum chloride hexahydrate: 700 g / l (20°C);

[0023] Calcium chloride: 740 g / l (20°C);

[0024] Magnesium chloride: 740 g / l (20°C);

[0025] Sodium chloride: 360 g / l (20°C);

[0026] Potassium chloride: 253 g / l (20°C);

[0027] Lithium chloride: 670 g / l (20°C);

[0028] Rare earth chloride: 500g / l (20℃).

[0029] Compounds with similar concentrations and saturated solubility will form co-crystals and co-precipitations, such as ferric chloride hexahydrate and aluminum chloride hexahydrate, calcium chloride and magnesium chloride, sodium chloride and potassium chloride, lithium chloride and rare earth chloride, etc. Therefore, for mixtures that form co-crystals and co-precipitations, other methods (such as precipitation method, extraction method, etc.) need to be used for further separation and purification.

[0030] For example, the co-crystals and co-precipitates formed by ferric chloride hexahydrate and aluminum chloride hexahydrate can be redissolved and the pH value of the solution can be adjusted through a neutralization reaction to precipitate ferric hydroxide and aluminum hydroxide, respectively, so that aluminum and iron can be separated and purified.

[0031] The components that have not reached the saturated concentration in the dissolution mother liquor will enter the next dissolution reaction with the mother liquor until they reach the saturated concentration, so that they can be separated from the mother liquor by crystallization.

[0032] The acid method can be used to treat bauxite, which can not only separate the main components, such as aluminum oxide, silicon oxide and iron oxide, but also separate the medium and trace elements, so that the bauxite resources can be comprehensively utilized.

[0033] The mother liquor and washing liquid of each stage can be combined together, supplemented with hydrochloric acid, and then used to decompose bauxite.

[0034] It should be pointed out that unlike alkaline decomposition of bauxite, which is aimed at achieving a higher aluminum dissolution rate, acid decomposition of bauxite should be aimed at fully removing impurity elements such as iron and retaining more aluminum components without being dissolved. The acid slag with silicon oxide and aluminum oxide as the main components can be used to directly produce aluminum silicon alloy, aluminum and aluminum alloy.

[0035] 90% of alumina production is used to produce metallic aluminum, and most of the metallic aluminum is used to produce aluminum alloys.

[0036] Silicon aluminum alloy and high silicon aluminum alloy, which account for about 30% of the aluminum alloy market, are binary alloys composed of Si and Al. High silicon aluminum alloy materials can maintain the excellent properties of silicon and aluminum, and the content of Si and Al is quite rich. The alloy density is 2.4-2.7g / cm3, and the thermal expansion coefficient is between 7-20ppm / ℃. Increasing the silicon content can significantly reduce the density and thermal expansion coefficient of the alloy material. At the same time, high silicon aluminum alloy also has good thermal conductivity, high specific strength and rigidity, good plating performance with gold, silver, copper and nickel, can be welded with the substrate, and is easy to process with precision. It is used for electronic packaging materials, especially in high-tech fields such as aerospace, space technology and portable electronic devices.

[0037] In addition to low-silicon aluminum alloys, there are hypoeutectic silicon aluminum alloys, which contain 9-12% silicon; eutectic silicon aluminum alloys, which contain 11-13% silicon; hypereutectic silicon aluminum alloys have a silicon content of more than 12%, mainly 15-20%; and those with a silicon content of more than 22% are called high-silicon aluminum alloys, of which 25-70% is the main content. Internationally, the highest silicon alloy can reach 80%.

[0038] The acid slag obtained from acid-soluble bauxite mainly contains silicon oxide, aluminum oxide and titanium oxide, etc., and can be directly reduced to obtain aluminum and aluminum alloys. The main reduction methods include high-temperature thermal reduction and aluminum electrolysis.

[0039] The high-temperature thermal reduction method is to reduce oxides to metals using suitable reducing agents such as carbon, hydrogen or coal gas at a suitable temperature (1800-2400℃); the aluminum electrolysis method is to use an aluminum electrolytic cell to reduce oxides to metals, mainly reducing aluminum oxide to metallic aluminum.

[0040] Aluminum is produced industrially by electrolysis. The Hall-Heroult cryolite-alumina molten salt electrolysis method is used in aluminum electrolysis industry, that is, fluoride salts mainly composed of cryolite are used as flux, and alumina is used as the melt to form a multi-electrolyte system. Among them, the Na2AlF6-Al2O3 binary system and the Na3AlF6-AlF3-Al2O3 ternary system are the basis of industrial electrolytes.

[0041] Aluminum electrolysis process: Modern aluminum industry production adopts cryolite-alumina molten salt electrolysis method. Molten cryolite It is a solvent, with alumina as the solute, carbonite as the anode, and aluminum liquid as the cathode. After a strong direct current is passed through, an electrochemical reaction, namely electrolysis, takes place at the two electrodes in the electrolytic cell at 950℃-970℃. Chemical reactions Mainly through this equation: 2 Al2O3 + 3C = =4 Al+3CO2. Anode: 2O2 - +C-4e - =CO2↑Cathode: Al3+3e - =Al. The anode products are mainly carbon dioxide and Carbon monoxide Gas, which contains a certain amount of Hydrogen fluoride The cathode product is aluminum liquid, which is extracted from the tank by vacuum ladle and sent to the foundry. After purification and clarification in the holding furnace, it is cast into aluminum ingots or directly processed into wire billets, profiles, etc.

[0042] Aluminum electrolysis cells can also be used to produce aluminum alloys. The aluminum content in aluminum alloys can be increased through the aluminum electrolysis process, and impurities in aluminum alloys can be purified and removed through the aluminum electrolysis process. It should be pointed out that it is convenient and effective to increase the beneficial trace elements in aluminum alloys through the aluminum electrolysis process, but the concentration limit of electrolytes on metal oxides and the adverse effects of some metal oxides on electrolytes should be taken into account.

[0043] According to the basic principles of chemical thermodynamics, the relationship between the standard free energy change and temperature of the carbon reduction reaction and the equilibrium constant K of the reactions at 1800K can be obtained by calculating the basic thermodynamic data of the relevant oxides and related reactions:

[0044] 1 / 2SiO2+C=1 / 2Si+CO, ΔG°=356100-183.85T(KJ) (T=1883~2000K),

[0045] K(1800K)=0.19;

[0046] 1 / 3Al2O3+C=2 / 3Al+CO, ΔG°=442270-191.76T(KJ) (T=1500~2000K),

[0047] K(1800K)=0.0016.

[0048] Under standard conditions, the starting temperatures of the reduction reaction of silicon oxide, aluminum oxide and carbon are:

[0049] Si≈1740℃

[0050] Al≈2000℃

[0051] But in fact, when Al.Si forms an alloy, the ΔG value of reduction can be reduced, and the temperature at which the reduction reaction starts can be reduced accordingly. A mixture of Al2O3 and SiO2 can react with carbon to form an aluminum-silicon alloy in the temperature range of 1800-2400℃.

[0052] Considering that the carbon thermal reduction method is difficult to reduce alumina, it is difficult to obtain high aluminum alloys through the carbon thermal reduction method. Therefore, the carbon thermal reduction method is mainly used to obtain high silicon aluminum alloys. After the carbon thermal reduction reaction is completed, the slag and the alloy liquid can be separated by static separation, centrifugal separation and other methods. The slag mainly contains alumina and can be used as an aluminum electrolysis raw material to produce aluminum and aluminum alloys. Considering the requirements and restrictions of the aluminum electrolytic cell on the raw material composition, the lower the silicon oxide content in the slag, the better, and should be less than 8%. If the content of impurities such as silicon oxide in the separated slag in the carbon thermal reduction process is high, it should be considered to return the ingredients. It should be pointed out that the aluminum silicon alloy obtained from the carbon thermal reduction method can also be injected into the aluminum electrolytic cell in an appropriate manner (for example: the amount of metal liquid extracted from the aluminum electrolytic cell should be approximately the same as the amount of metal liquid added, and the melting point of the added metal liquid should be lower than 900°C, etc.), and the aluminum content and the quality of the alloy can be increased through the aluminum electrolysis process. The low silicon oxide melt (alloy liquid and slag) with relatively sufficient silicon oxide reduction can also be directly injected into the aluminum electrolytic cell for aluminum addition and purification. III. Summary of the invention

[0053] The main contents of the present invention include: crushing and grinding the ore to 100-300 meshes, analyzing the content of soluble components such as iron oxide, calcium oxide, magnesium oxide, aluminum oxide, potassium oxide, sodium oxide, etc. in the ore by chemical analysis method, and decomposing bauxite with concentrated acid (hydrochloric acid or sulfuric acid). If hydrochloric acid is used, the amount of hydrochloric acid required for complete reaction is calculated according to chemical reaction formulas such as Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O, and then an excess of 20% is used. Concentrated hydrochloric acid (10-30%) is used to react for 10min-4h at high temperature (100-220℃) and high pressure (0.1-2.35MPa) to leach out soluble components such as ferric chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, lithium chloride, and rare earth chloride. Chloride salts reaching saturation concentration are precipitated by crystallization. For salts that reach saturation concentration at the same time, co-crystals and co-precipitations are formed. For salts that do not reach saturation concentration, new ore will be decomposed along with the mother liquor until it reaches saturation concentration, and can be separated from the mother liquor by crystallization.

[0054] The mother liquor components can be initially separated by the method of precipitation crystallization, which can reduce the separation cost and create conditions for further separation and purification.

[0055] By controlling the lower reaction temperature, acid concentration and longer dissolution reaction time, impurity elements such as iron can be fully dissolved, while retaining more alumina components in the acid slag, providing high-aluminum raw materials for the next step of direct reduction to produce aluminum-silicon alloy.

[0056] The slag after acid dissolution mainly contains silicon oxide, aluminum oxide, titanium oxide, etc. Using carbon as a reducing agent, the amount of carbon required for complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 0-50% is added to this amount. Smelting is carried out at a temperature of 1800-2400℃ for 1-4h to generate high silicon aluminum alloy.

[0057] Static and centrifugal separation methods can be used to fully separate the slag from the melt. If the slag contains a high content of impurities such as silicon oxide (such as silicon oxide content ≥ 8%), it should be returned to the batching for carbon thermal reduction reaction again.

[0058] The slag (mainly containing alumina) after the carbon thermal reduction reaction is used as the raw material for aluminum electrolysis to produce aluminum and aluminum alloys through the aluminum electrolysis process.

[0059] The aluminum-silicon alloy obtained by the carbon thermal reduction method can be injected into the aluminum electrolytic cell in an appropriate manner (for example, the amount of molten metal extracted from the aluminum electrolytic cell should be approximately equal to the amount of molten metal added, and the melting point of the added molten metal should be lower than 900°C, etc.) to increase the metallic aluminum content and improve the quality of the alloy through the aluminum electrolysis process.

[0060] The low silicon oxide melt (alloy liquid and slag) with relatively sufficient silicon oxide reduction can be directly injected into the aluminum electrolytic cell for aluminum addition and purification.

[0061] The positive beneficial effects of the present invention are:

[0062] 1. It can make full use of various bauxite resources;

[0063] 2. Through the crystallization separation of saturated solution, the separation cost of acid-soluble components can be effectively reduced, creating conditions for further separation and purification;

[0064] 3. Through high-temperature thermal reduction and aluminum electrolysis, the aluminum-silicon oxide mixture is directly reduced to generate high-silicon aluminum alloy, aluminum and aluminum alloy in two steps;

[0065] 4. It can reduce the production cost of aluminum and aluminum alloy by more than 30%. 4. Specific implementation methods

[0066] The following examples are only intended to further illustrate the present invention and are not intended to limit the present invention.

[0067] Embodiment 1,

[0068] The bauxite ore is crushed and ground to 200 mesh;

[0069] Use chemical analysis methods to analyze the content of iron oxide, calcium oxide, magnesium oxide, aluminum oxide, potassium oxide, sodium oxide and other substances in the ore;

[0070] Decompose bauxite with concentrated hydrochloric acid.

[0071] According to Fe2O3+6HCl=2FeCl3+3H2O

[0072] CaO+2HCl=CaCl2+H2O

[0073] MgO+2HCl=MgCl2+H2O

[0074] Li2O+2HCl=2LiCl+H2O

[0075] Na2O+2HCl=2NaCl+H2O

[0076] K2O+2HCl=2KCl+H2O

[0077] Re2O3+6HCl=2ReCl3+3H2O (Re is a rare earth element)

[0078] The amount of hydrochloric acid required for the complete reaction is calculated according to the chemical reaction formula, and a 20% excess of concentrated hydrochloric acid (10%) is used at high temperature (110°C) and high pressure (0.2MPa) in a pressure-resistant enamel reactor. The reaction is stirred for 3 hours to leach out soluble components such as ferric chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, lithium chloride, and rare earth chloride. Chloride salts with a saturated concentration are crystallized and precipitated. For salts that reach the saturated concentration at the same time, co-crystals and co-precipitations are formed. For salts that do not reach the saturated concentration, new ore is decomposed again with the mother liquor until crystals can be precipitated and separated by precipitation.

[0079] The separated ferric chloride hexahydrate and aluminum chloride hexahydrate are co-crystallized and co-precipitated, and after redissolved, the pH value of the solution is adjusted by neutralization reaction. When the pH value reaches 3.8, ferric hydroxide is completely precipitated, and when the pH value reaches 3.8, aluminum hydroxide begins to precipitate, so that ferric hydroxide and aluminum hydroxide are precipitated separately, and aluminum and iron are separated and purified.

[0080] The co-crystals and co-precipitates formed by lithium chloride and rare earth chloride are redissolved, and the pH value of the solution is adjusted with sodium carbonate to precipitate rare earth oxide first, which is filtered and washed to obtain mixed rare earth oxide; the pH value of the filtrate is further adjusted with sodium carbonate to precipitate lithium carbonate, which is filtered and washed to obtain lithium carbonate precipitate.

[0081] The slag after acid dissolution, which mainly contains silicon oxide, aluminum oxide, titanium oxide, etc., is treated with carbon as a reducing agent. The amount of carbon required for complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 10% of the ingredients are added on this basis. A mineral thermal reduction furnace is used with slag-free submerged arc high-temperature smelting technology. The smelting reaction is continued at a temperature of 2000°C for 1 hour to separate the slag and the alloy liquid.

[0082] The slag is used as raw material for aluminum electrolysis to produce aluminum and aluminum alloys through the aluminum electrolysis process.

[0083] Embodiment 2,

[0084] The bauxite ore is crushed and ground to 200 mesh;

[0085] Use chemical analysis methods to analyze the content of iron oxide, calcium oxide, magnesium oxide, aluminum oxide, potassium oxide, sodium oxide and other substances in the ore;

[0086] Decompose bauxite with concentrated hydrochloric acid.

[0087] According to Fe2O3+6HCl=2FeCl3+3H2O

[0088] CaO+2HCl=CaCl2+H2O

[0089] MgO+2HCl=MgCl2+H2O

[0090] Li2O+2HCl=2LiCl+H2O

[0091] Na2O+2HCl=2NaCl+H2O

[0092] K2O+2HCl=2KCl+H2O

[0093] Re2O3+6HCl=2ReCl3+3H2O (Re is a rare earth element)

[0094] The amount of hydrochloric acid required for the complete reaction is calculated according to the chemical reaction formula, and then a 20% excess of concentrated hydrochloric acid (20%) is used at high temperature (150°C) and high pressure (0.78MPa) in a pressure-resistant enamel reactor. The reaction is stirred for 0.5h to leach out soluble components such as ferric chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, lithium chloride, and rare earth chloride. Chloride salts with saturated concentration are crystallized and precipitated. For salts that reach saturated concentration at the same time, co-crystals and co-precipitations are formed. For salts that do not reach saturated concentration, new ore is decomposed again with the mother liquor until crystals can be precipitated and separated by precipitation.

[0095] The separated ferric chloride hexahydrate and aluminum chloride hexahydrate can be co-crystallized and co-precipitated, and then the pH value of the solution can be adjusted by neutralization reaction after being redissolved. When the pH value reaches 3.8, ferric hydroxide is completely precipitated, and when the pH value reaches 3.8, aluminum hydroxide begins to precipitate, so that ferric hydroxide and aluminum hydroxide are precipitated separately, and aluminum and iron are separated and purified.

[0096] The co-crystals and co-precipitates formed by lithium chloride and rare earth chloride are redissolved, and the pH value of the solution is adjusted with sodium carbonate to precipitate rare earth oxide first, which is filtered and washed to obtain mixed rare earth oxide; the pH value of the filtrate is further adjusted with sodium carbonate to precipitate lithium carbonate, which is filtered and washed to obtain lithium carbonate precipitate.

[0097] The acid-dissolved slag, which mainly contains silicon oxide, aluminum oxide, titanium oxide, etc., uses carbon as a reducing agent. The amount of carbon required for complete reaction is calculated according to the reaction formula Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2. The smelting reaction is continued at a temperature of 2200°C for 1 hour.

[0098] An appropriate amount of melt is injected into the aluminum electrolysis cell to produce aluminum and aluminum alloys through the aluminum electrolysis process.

Claims

1. A method for comprehensive utilization of bauxite resources, characterized by comprising the following contents and steps: a. Crushing and grinding the bauxite ore to 100-300 mesh; b. Use chemical analysis methods to analyze the content of iron oxide, calcium oxide, magnesium oxide, aluminum oxide, potassium oxide, sodium oxide and other substances in the ore; c. Use concentrated acid (hydrochloric acid or sulfuric acid) to decompose bauxite; if hydrochloric acid is used, press Al2O3+6HCl=2AlCl3+3H2O Fe2O3+6HCl=2FeCl3+3H2O CaO+2HCl=CaCl2+H2O MgO+2HCl=MgCl2+H2O Li2O+2HCl=2LiCl+H2O Na2O+2HCl=2NaCl+H2O K2O+2HCl=2KCl+H2O Re2O3+6HCl=2ReCl3+3H2O (Re is a rare earth element) The amount of hydrochloric acid required for the complete reaction is calculated according to the chemical reaction formula, and concentrated hydrochloric acid (10-30%) is used to react for 10 minutes to 4 hours at high temperature (100-220°C) and high pressure (0.1-2.56MPa) to leach out soluble components such as ferric chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, lithium chloride, and rare earth chloride. Chloride salts reaching saturated concentration are precipitated by crystallization. For salts reaching saturated concentration at the same time, co-crystals and co-precipitations are formed. For salts that have not reached saturated concentration, they are used again with the mother liquor to decompose new ore until crystals can be precipitated and separated by precipitation; d. The separated ferric chloride hexahydrate and aluminum chloride hexahydrate are co-crystallized and co-precipitated. After redissolving, the pH value of the solution is adjusted by neutralization reaction with carbonate or hydroxide of alkali metal (sodium, potassium) or alkaline earth metal (calcium, magnesium). When the pH value reaches 3.8, ferric hydroxide is completely precipitated, and when the pH value reaches 3.8, aluminum hydroxide begins to precipitate, so that ferric hydroxide and aluminum hydroxide are precipitated respectively, and aluminum and iron are separated and purified; the co-crystallization and co-precipitation formed by lithium chloride and rare earth chloride can be adjusted with sodium carbonate after redissolving, and rare earth oxide precipitation is first precipitated, and mixed rare earth oxide is obtained after filtering and washing; the pH value of the solution is adjusted with sodium carbonate continuously, lithium carbonate precipitation is precipitated, and lithium carbonate precipitation is obtained after filtering and washing; e. The slag after acid dissolution mainly contains silicon oxide, aluminum oxide, titanium oxide, etc. Carbon is used as a reducing agent. The amount of carbon required for complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 0-20% is added to this amount. The slag is smelted at a temperature of 1800-2400℃ for 1-4h, and the slag is separated statically or by centrifugation; or an appropriate amount of melt (slag and alloy liquid) is directly injected into the aluminum electrolytic cell; f. Use the slag as the raw material for aluminum electrolysis to generate aluminum and aluminum alloys through the aluminum electrolysis process.

2. According to claim 1, It is characterized by The chloride salts reaching the saturated concentration are precipitated by the crystallization method. For the salts reaching the saturated concentration at the same time, co-crystals and co-precipitations are formed. For the salts that have not reached the saturated concentration, they are used again with the mother liquor to decompose new ores until crystals can be precipitated and separated by precipitation.

3. According to claim 1, Features It is to redissolve the salt crystals and further separate and purify them through neutralization precipitation.

4. According to claim 1, Features The acid-dissolved slag is mixed with carbon, smelted at 1800-2400°C for 1-4 hours, and the slag is separated from the melt by static or centrifugal separation.

5. According to claims 1 and 4, Features The slag after carbon thermal reduction reaction is used as the raw material for aluminum electrolysis to produce aluminum and aluminum alloy through the aluminum electrolysis process.

6. According to claim 1, Features The method is to directly inject an appropriate amount of melt (slag and alloy liquid) into the aluminum electrolysis cell, increase the aluminum content of the alloy through the aluminum electrolysis process, and purify, remove impurities and optimize the alloy in the process.