Preparation method and application of sweat pore-imitating nanofiber membrane
Preparation of sweat-imitation nanofiber membranes through electrospinning technology solves the problem that traditional fabrics cannot effectively guide sweat removal by one-way, achieve efficient sweat removal and prevent reverse osmosis, and integrate biomarker detection functions in the fabric to improve the Heat comfort and health monitoring capabilities during exercise.
Patent Information
- Application Number
- CN202411075451.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-07
AI Technical Summary
Traditional fabrics and highly absorbent fabrics cannot effectively guide sweat away from each other during exercise, causing sweat to adhere to the skin surface, affecting thermal comfort and health monitoring, and it is difficult to have both fluid conductivity and anti-reverse osmosis.
Electrospinning technology is used to prepare sweat-imitation nanofiber membranes with array pore structures. The sweat-imitation array of nanofiber membranes is used to achieve one-way guidance of sweat, and biomarkers are integrated into the fabric to detect micro-regions through a smartphone. Detection of various biomarkers.
It realizes efficient single-guided sweat removal and prevents reverse osmosis, improves the wearer's thermal comfort, and can simultaneously detect biomarkers in sweat to provide health monitoring information.
Smart Images

Figure CN118957883A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-performance fiber and fiber fabric preparation, and specifically relates to a method for preparing a sweat pore-mimicking nanofiber membrane and application of the same in a unidirectional liquid-conducting fabric. Background Art
[0002] Sweating is a physiological function of the human body to regulate body temperature. During exercise, the sweat pores of the human skin will secrete sweat, and the evaporation of sweat will take away the heat and reduce the skin temperature. The sweat rate of an average person under moderate exercise conditions can reach 1000mL / h -1 m -2 . However, if clothing fabrics cannot effectively conduct sweat away from the skin surface, the excess sweat will exist in the form of attached sweat, which will soak the fabric surface to a certain extent and have a negative impact on the thermal comfort of the human body. Studies have found that different degrees of sweating will cause the thermal resistance of the fabric to decrease by 2%-8%. In a low temperature environment, the human body will feel damp and cold, and even cause hypothermia, resulting in risks such as hypothermia. Moreover, wet fabrics will adhere to the skin surface, reducing the comfort of the wearer. In recent years, the urgent need for fast moisture absorption and perspiration wicking materials has attracted people's attention to functional moisture-wicking fabrics.
[0003] Traditional fabrics and highly hygroscopic fabrics are committed to improving the hygroscopic properties of materials. However, sweat is transmitted bidirectionally in such fabrics. As the amount of sweat increases, sweat will adhere to the skin surface under the action of gravity. The design strategy of unidirectional moisture-conducting fabrics is to use the wettability gradient or pore gradient in the thickness direction to achieve unidirectional sweat conduction. However, the pores inside the hydrophobic layer must serve as sweat conduction channels and also have an anti-reverse osmosis effect. It is difficult to achieve both excellent liquid conduction and anti-reverse osmosis performance. Therefore, it is of great significance to develop new fiber materials that can solve the above problems.
[0004] As an important biological fluid closely related to human health, sweat contains a variety of biomarkers such as electrolytes, metabolites and proteins, providing a wealth of health information about physiological and metabolic status. For example, the concentration of chloride ions in sweat can be used as an indicator for the evaluation of cystic fibrosis, the pH level can be used as a basis for determining metabolic alkalosis, and excessive loss of calcium ions means the risk of hypocalcemia. Therefore, testing human sweat can monitor the health of the human body and provide early warning for diseases. In view of this, it is urgent to develop new functional fabrics that have both unidirectional sweat conduction and simultaneous detection of sweat biomarkers. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a sweat pore-mimicking nanofiber membrane and application of the same in a one-way liquid-conducting fabric.
[0006] The implementation process of the present invention is as follows:
[0007] A method for preparing a sweat pore-mimicking nanofiber membrane comprises the following steps: dispersing or dissolving a soluble hydrophobic polymer material and a micro-nano material in a solvent to obtain an electrostatic spinning solution; using a spinning collection device with an array pore structure and an electrostatic spinning device to perform electrospinning to obtain the sweat pore-mimicking nanofiber membrane.
[0008] Furthermore, the soluble hydrophobic polymer material is selected from any one or a combination of poly-ε-caprolactone, polyurethane, polylactic acid, poly(lactide-glycol), polysulfone, polymethyl methacrylate, polyvinyl butyral, and polyvinylidene fluoride.
[0009] Furthermore, the micro-nano material is selected from any one or a combination of SiO2, zinc oxide, titanium oxide, attapulgite, halloysite, graphene oxide, hydroxyapatite, polystyrene, and polymethyl methacrylate.
[0010] Furthermore, the solvent is selected from any one or a combination of tetrahydrofuran, N,N-dimethylformamide, dichloromethane, chloroform, hexafluoroisopropanol, and ethanol.
[0011] Furthermore, the mass concentration of the soluble polymer material in the electrospinning solution is 0.1-5.0 g / ml; the electrospinning parameters are voltage of 5 kv-20 kv, flow rate of 0.1-2.0 ml / h, and spinning distance of 5-20 cm.
[0012] Furthermore, the spinning collecting device with an array hole structure is any one or a combination of a spinning collecting device with a circular hole array structure, a spinning collecting device with a triangular hole array structure, a spinning collecting device with a polygonal hole array structure, a spinning collecting device with an irregular hole array structure, and a screen.
[0013] The sweat-pore-mimicking nanofiber membrane obtained by the above preparation method has sweat-conducting pores arranged in an array.
[0014] The application of the above-mentioned sweat pore-mimicking nanofiber membrane in fabrics, and the application of the above-mentioned sweat pore-mimicking nanofiber membrane in unidirectional liquid-conducting fabrics.
[0015] Furthermore, the sweat pore-mimicking nanofiber membrane is assembled with fabric to form a sweat pore-mimicking fabric; and the biomarkers in the sweat derived from the nanofiber membrane are detected by dropping an indicator on the sweat pore-mimicking fabric.
[0016] Furthermore, the indicator is an indicator used for detection that corresponds one-to-one to the biomarker in sweat.
[0017] The design concept of the present invention:
[0018] Inspired by the sweat pore array of human skin and drawing on the unilateral sweat conduction mode of human sweat pores from the inside to the outside, a sweat pore-mimicking nanofiber membrane is constructed. The sweat pore array inside the nanofiber membrane is used to unilaterally conduct a large amount of sweat, and the area around the sweat pores is used to prevent the conducted sweat from back-seeping. Furthermore, sweat component detection micro-areas are integrated into the sweat pore-mimicking nanofiber membrane, and based on colorimetry, intelligent detection of multiple biomarkers of sweat is achieved with the help of smartphones.
[0019] Positive effects of the present invention:
[0020] (1) Using electrospinning technology and a spinning collection device with an array pore structure, a controllable preparation of a sweat-like pore nanofiber membrane was achieved. The sweat-like pore nanofiber membrane was assembled with a fabric to form a fabric with a wettability gradient. The effect of the sweat-like pore size on the transport performance of a single droplet was studied, and it was found that the droplet transport rate increased with the increase of the pore size.
[0021] (2) The present invention investigates the effect of the pore spacing in the sweat-like pore nanofiber membrane on the bulk liquid transport performance. The results show that as the pore spacing increases, the liquid transport rate decreases, and the residual area of the liquid on the hydrophobic side decreases. The liquid conduction rate of the sweat-like pore fabric is as high as 240 g·s -1 ·m -2 The liquid residual area is only 16%, while the non-woven fabric without array pore structure is only 25g·s -1 ·m -2 , the liquid residual area of nonwoven fabrics without array pore structure is as high as 100%. In addition, it is found that the anti-reverse osmosis performance of liquid can be improved by increasing the hydrostatic pressure in the area around the pores, and the hydrostatic pressure increases with the increase of the area around the pores. COMSOL is used to simulate the liquid conduction process at the sweat-simulating pores and the area around the sweat pores, and the forces on the liquid in the two micro-areas are deeply analyzed, which clarifies the mechanism of sweat-simulating pore fabrics to both efficiently conduct liquid and prevent reverse osmosis.
[0022] (3) The micro-nanoparticles in the method of the present invention can increase the roughness and hydrophobicity of the sweat-pore-mimicking nanofiber membrane, thereby improving the unidirectional sweat conduction speed and anti-reverse osmosis ability of the bionic nanofiber membrane.
[0023] (4) Application of the sweat pore-mimicking nanofiber membrane of the present invention in a one-way liquid-conducting fabric. The present invention provides a new application direction of the sweat pore-mimicking nanofiber membrane, which is used for the simultaneous detection of biomarkers in sweat.
[0024] (5) Based on the sweat pore-mimicking nanofiber membrane, multiple sweat detection areas are constructed for simultaneous detection of multiple biomarkers. This fabric can guide sweat to the detection area through unidirectional drainage and lateral drainage, and the amount of sweat collected in the detection area is controllable. In addition, different detection areas can be used to detect different biomarkers without interfering with each other. This fabric that integrates sweat conduction and sweat detection functions is expected to be used in the fields of textiles, medical treatment, medical beauty, sports medicine, aerospace, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a schematic diagram of the array hole structure template used as a collection device in Example 5;
[0026] Figure 2 Structural regulation of sweat pore-mimicking nanofiber membrane; (a) Schematic diagram of sweat pore-mimicking nanofiber membrane preparation; (b) Macroscopic digital photo of sweat pore-mimicking nanofiber membrane; (c) SEM photo of sweat pore-mimicking nanofiber membrane; (c1, c2) Enlarged SEM photos of the inner and surrounding areas of sweat pores, respectively; (d) Statistical distribution of fiber diameter; (e) High-magnification SEM photo of sweat pore-mimicking nanofiber membrane; (f) Mapping photo of sweat pore-mimicking nanofiber membrane; (g) FTIR spectrum of sweat pore-mimicking nanofiber membrane; (hj) Laser confocal microscopy CLSM photos of sweat pore-mimicking nanofiber membranes with different structures, (i) fiber pore size and (j) water contact angle statistics; (k) Water contact angle photo of sweat pore-mimicking nanofiber membrane, (l) breathability photo;
[0027] Figure 3 The wetting properties of sweat-pore-mimicking nanofiber membranes with different SiO2 contents; (a) photos of spinning solutions with different SiO2 contents; (b) low-magnification SEM photos of nanofiber membranes with three different SiO2 contents, (c) high-magnification SEM photos, (d) water contact angle statistics, (e) the wetting process of nanofiber membranes with different SiO2 loadings, and (f) statistics of the changes in the wetting area over time;
[0028] Figure 4 The transport performance diagram of sweat-like fabrics with different structures and non-woven fabrics in the control group for a large amount of liquid; (a) The liquid conduction process of sweat-like fabrics with different circular hole spacing and non-woven fabrics in the control group; (b) The statistics of the area of the droplet contacting the hydrophobic side before liquid conduction and the area of the hydrophobic side dyed after liquid conduction; (c) The liquid conduction rate of fabrics with different structures and (d) The percentage of the residual liquid area on the hydrophobic side to the liquid contact area;
[0029] Figure 5 The anti-reverse seepage performance diagram of the sweat pore-like fabric; (a) Liquid diffusion photo on the hydrophilic side of the sweat pore-like fabric; (b) Hydrostatic pressure test device diagram; (c) Relationship between the area around the circular hole of the sweat pore-like fabric and the hydrostatic pressure; (d) Linear fitting diagram between the area around the circular hole of the sweat pore-like fabric and the hydrostatic pressure;
[0030] Figure 6 The simulation diagram of the fluid transmission process in the sweat pore-like fabric; (a1-a4) from the hydrophobic side to the hydrophilic side; (b1-b4) from the hydrophilic side to the hydrophobic side; the flow velocity distribution and pressure distribution curve of the fluid passing through the double-layer contact interface (c) from the hydrophobic side to the hydrophilic side (d) from the hydrophilic side to the hydrophobic side;
[0031] Figure 7 Schematic diagram of nanofiber fabric for sweat biomarker detection; (a) Schematic diagram of the preparation of sweat pore-simulating fabric; (b) digital photo of the real object; (c) photos of contact angles of different areas of the sweat pore-simulating fabric; (d) photos of simulated sweat diffusion in cotton fabric and sweat detection micro-areas;
[0032] Figure 8 Biomarker colorimetric test; (a) sweat marker (Cl - , pH and Ca 2+ ) Schematic diagram of colorimetric detection; (b) Cl - , (c) pH, (d) Ca 2+ Colorimetric analysis optical photos and RGB analysis curves; (eg) R value, G value, B value and Cl - , pH, Ca 2+ Linear fit of . DETAILED DESCRIPTION
[0033] The present invention will be further described below in conjunction with the embodiments.
[0034] The sweat-pore-mimicking nanofiber membrane of the present invention is combined with fabric to form a new functional fabric material, which can combine the one-way sweat separation function with the synchronous sweat detection function, so that the wearer can keep the skin dry and comfortable during exercise, prevent sweat from reversely seeping back, and synchronously detect the components in sweat. The present invention will have important guiding significance for the development of the next generation of new functional fabrics.
[0035] It should be noted that the ratio of the soluble hydrophobic polymer material to the micro-nano material in the method of the present invention is not limited. In practical applications, those skilled in the art can select any ratio according to actual needs, as long as the obtained electrospinning solution can achieve electrospinning.
[0036] The ratio of the soluble hydrophobic polymer material to the solvent in the method of the present invention is not limited, as long as the mass concentration of the soluble hydrophobic polymer material in the electrospinning solution is 0.1-5.0 g / ml.
[0037] The type of solvent in the method of the present invention is not limited, as long as it can dissolve the soluble hydrophobic polymer material while not dissolving the micro-nano particles. The method of the present invention is preferably any one or a combination of tetrahydrofuran, N,N-dimethylformamide, dichloromethane, chloroform, hexafluoroisopropanol, and ethanol.
[0038] The deposition time of electrospinning in the method of the present invention is not limited, and those skilled in the art can select the deposition time according to experimental needs.
[0039] The fabric used in the application of the method of the present invention is not limited. Those skilled in the art can select fabrics of different materials according to actual needs. Cotton fabric is preferred in the method of the present invention.
[0040] The assembly described in the present invention is to stack the bionic nanofiber membrane and the fabric. The method of the present invention does not make too many restrictions on the assembly method. In the actual application process, those skilled in the art can choose a suitable assembly method according to the needs of the situation and other factors. In the present invention, the suturing method is preferred.
[0041] The sweat pore-simulating nanofiber membrane of the present invention is used in a one-way liquid conduction fabric. The sweat pore-simulating nanofiber membrane is assembled with a fabric to form a sweat pore-simulating fabric; an indicator is dripped onto the sweat pore-simulating fabric to detect biomarkers in sweat derived from the nanofiber membrane. The indicator used in the process can be various, and there is a one-to-one correspondence between the indicator and the target biomarker detected in sweat, such as sodium ions, potassium ions, uric acid, chloride ions, pH, calcium ions, etc.
[0042] Example 1 Preparation method of sweat pore-mimicking nanofiber membrane
[0043] Weigh 0.13g of hydrophobic SiO2 powder and add it to a mixed solution of 1mL tetrahydrofuran (THF) and 3mL N,N-dimethylformamide (DMF). After ultrasonic dispersion for 1h, add 0.65g of poly-ε-caprolactone particles (PCL) to the above dispersion and stir at room temperature for 12h until completely dissolved. The above solution was transferred to a glass syringe, and a spinning collection device with an array circular hole structure was used. The pore size-hole spacing parameter of the metal plate was 0.7-1.0mm. The sweat-like pore nanofiber membrane was obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage of 7.4kV, flow rate of 0.5mL / h, spinning distance of 10cm, and deposition time of 12min.
[0044] Comparative Example 1
[0045] The steps and methods are the same as those of Example 1, except that no hydrophobic SiO2 powder is added.
[0046] Comparative Example 2
[0047] The steps and methods are the same as those in Example 1, except that 0.26 g of hydrophobic SiO2 powder is added.
[0048] Comparative Example 3
[0049] The steps and methods are the same as those in Example 1, except that a spinning collection device without an array hole structure is used.
[0050] Example 2 Preparation method of sweat pore-mimicking nanofiber membrane
[0051] 0.13g of hydrophobic SiO2 powder was weighed and added to a mixed solution of 1mL of tetrahydrofuran (THF) and 3mL of N,N-dimethylformamide (DMF). After ultrasonic dispersion for 1h, 0.52g of poly-ε-caprolactone particles (PCL) were added to the above dispersion and stirred at room temperature for 12h until completely dissolved. The above solution was transferred to a glass syringe and electrospun to obtain a sweat-like pore nanofiber membrane using an electrospinning device. The electrospinning parameters were as follows: voltage of 7.4kV, flow rate of 0.5mL / h, and spinning distance of 10cm. A spinning collection device with an array circular hole structure was used, and the pore size-pore spacing parameters of the metal plate were 0.3-1.0mm, 0.7-0.8mm, 0.7-1.2mm, respectively. The deposition time was 12min, and sweat-like pore nanofiber membranes with different pore sizes-pore spacings were obtained.
[0052] Example 3 Preparation method of sweat pore-mimicking nanofiber membrane
[0053] 0.13g of hydrophobic SiO2 powder was weighed and added to a mixed solution of 1mL of tetrahydrofuran (THF) and 3mL of N,N-dimethylformamide (DMF). After ultrasonic dispersion for 1h, 0.78g of poly-ε-caprolactone particles (PCL) were added to the above dispersion and stirred at room temperature for 12h until completely dissolved. The above solution was transferred to a glass syringe and electrospun to obtain a sweat-like pore nanofiber membrane using an electrospinning device. The electrospinning parameters were as follows: voltage of 7.4kV, flow rate of 0.5mL / h, and spinning distance of 10cm. A spinning collection device with an array circular hole structure was used, and the pore size-pore spacing parameters of the metal plate were 0.3-1.0mm, 0.5-1.0mm, 0.7-0.8mm, 0.7-1.0mm, and 0.7-1.2mm, respectively. The deposition time was 12min, and a series of sweat-like pore nanofiber membranes with different pore sizes and pore spacings were obtained in turn.
[0054] Embodiment 4 imitation sweat hole fabric
[0055] The sweat pore-imitation nanofiber membrane is assembled with cotton fabric, the side in contact with the skin is the substrate, the substrate is the sweat pore-imitation nanofiber membrane, and the side exposed to the air is the cotton fabric, and the sweat pore-imitation fabric is assembled by stacking and sewing.
[0056] Example 5 Application of sweat pore-mimicking nanofiber membrane in liquid unidirectional conduction fabric for detecting biomarkers
[0057] Using the method and parameters described in Example 1, the collection device uses a metal plate with an aperture-hole spacing of 0.7-1.0 mm to construct three sweat detection areas with a radius of 5 mm. Figure 1 As shown, a sweat pore-mimicking nanofiber membrane with a structure similar to that of a metal plate is obtained by depositing on the metal plate for 12 minutes; the cotton fabric is cut into three discs with a radius of 5 mm using a hole puncher, 15 μL of chloride ion indicator, 15 μL of pH universal indicator, and 10 μL of calcium ion indicator solution are respectively dropped on the surfaces of the three circular cotton fabrics, and after drying at room temperature for 10 minutes, the three circular cotton fabrics are filled in the sweat detection area on the sweat pore-mimicking nanofiber membrane to assemble a sweat biomarker detection nanofiber fabric.
[0058] The performance characterization and testing of Examples 1-5 are as follows:
[0059] 1 Characterization of sweat-mimicking nanofiber membrane
[0060] (1) Morphological characterization: The structure of the sweat-like pore nanofiber membrane was observed using a confocal laser scanning microscopy (CLSM): 1% curcumin was added to the spinning solution as a fluorescent marker, and the prepared nanofiber membranes with different pore sizes and pore spacings were cut into 1 cm × 2 cm sizes, spread on a glass slide, and covered with a cover glass. The membranes were observed and images were taken at an excitation wavelength of 488 nm.
[0061] The morphology of the fiber membrane was observed using a scanning electron microscope (SEM): the sweat-like pore nanofiber membrane was cut into a size of 1cm×1cm, and the membrane was fixed flat on the surface of a hollow plastic ring with a radius of 7mm and a height of 3mm using double-sided tape, and then attached to a conductive tape. After gold spraying for 60s, it was observed using a SEM; the diameters of 100 fibers were measured using Photoshop software and the statistical distribution patterns were analyzed; the statistical distribution patterns of the pore sizes of 100 fibers were measured.
[0062] (2) Composition characterization: Mapping was used to observe the distribution of different elements on the sweat pore-mimicking nanofiber membrane, and Fourier transform infrared spectrometer (FTIR) was used to analyze the chemical composition of the sweat pore-mimicking nanofiber membrane.
[0063] (3) Hydrophilicity test: The hydrophilicity of the sample was measured by a static contact angle meter (WCA). The contact angle change process of 2 μL of water on the sample surface was recorded. Five different locations on the sample were randomly selected to repeat the test. The average value was measured and recorded as the contact angle of the sample.
[0064] Experimental results and discussion:
[0065] Using electrospinning technology combined with a customized template collection device, a sweat-like pore nanofiber membrane with a sweat-like pore array was obtained ( Figure 2 a). Its macroscopic digital photo is as follows Figure 2 b, the results show that the sweat-like pore nanofiber membrane can be prepared on a large area (25cm×15cm). The morphology of the sweat-like pore nanofiber membrane was observed using SEM, as shown in Figure 2 As shown in Figure c, it can be clearly seen that the prepared nanofiber membrane has a circular hole array structure similar to that of the collecting plate. Interestingly, the circular holes are not through-hole structures, but have a small amount of fiber deposition. The overall fiber distribution shows that the fibers inside the circular holes are sparse and the fibers around them are dense ( Figure 2 c1-c2), this is because during the electrospinning process, the electric potential inside the circular holes of the circular hole array metal template is different from that around the circular holes, resulting in differences in the electric field distribution. The nanofibers with positive charges applied by high voltage are selectively deposited on the surface of the metal template around the circular holes, thereby forming a nanofiber membrane with a similar morphology to the collection template. In addition, according to statistics, the fiber diameter of the sweat-like pore nanofiber membrane is about 600nm ( Figure 2 d).
[0066] from Figure 2 It can be clearly seen that there are many nanoparticles distributed on the fiber surface of the sweat-like pore nanofiber membrane. Mapping observation shows that in addition to the C and O elements contained in PCL, the Si element can also be clearly seen in the sweat-like pore nanofiber membrane, and the Si element distribution is arranged along the fiber direction, proving that the nanoparticle composition is SiO2 ( Figure 2 f) Analyze the fiber composition by FTIR. Figure 2 g, it can be seen that the nanofibers have a wavelength of 1729 cm -1 It shows a strong absorption band, which is attributed to the stretching vibration of C=O in PCL, and at 800cm -1 and 470cm -1 The absorption band corresponds to the stretching vibration peak of Si-O in SiO2, proving the successful composite of SiO2 nanoparticles and PCL nanofibers.
[0067] Furthermore, by controlling the parameters of the circular hole array template, sweat-like pore nanofiber membranes with pore sizes and pore spacings of 0.3-1.0, 0.5-1.0, 0.7-0.8, 0.7-1.0, and 0.7mm-1.2mm were obtained. Curcumin was added to the spinning solution to dye the fiber membrane, and five different circular hole array structures can be clearly seen through CLSM images ( Figure 2 h), achieving controllable preparation of structures with different circular hole diameters and circular hole spacing. In order to explore the influence of circular hole diameter and circular hole spacing on the fiber pore size inside the circular hole, the fiber pore size inside the circular hole was statistically analyzed ( Figure 2i) It was found that the fiber pore size inside the circular hole of the three groups of sweat-like pore nanofiber membranes increased from 1.8 to 2.7μm as the circular hole diameter increased, and the fiber pore size of the three groups of sweat-like pore nanofiber membranes increased from 2.4 to 2.9μm as the circular hole spacing increased. In addition, the fiber pore size around the circular hole was statistically analyzed and it was found that the fiber pore size was basically maintained at about 0.7μm, and was not greatly affected by the change of pore size. This shows that the fiber pore size inside the circular hole of the sweat-like pore nanofiber membrane can be regulated by regulating the circular hole diameter and the hole spacing, which provides the possibility for the subsequent regulation and optimization of liquid transport performance.
[0068] The water contact angle of the sweat-like pore nanofiber membrane was tested, and the water contact angles of different regions of the five sweat-like pore nanofiber membranes were statistically analyzed. They were all around 130°, and the five samples all showed that the contact angle at the circular hole was slightly smaller than the contact angle around the circular hole ( Figure 2 jk). This is because the fiber deposition density at the circular hole is small, while the fiber deposition density around the circular hole is large. At the same time, as a sweat-conducting layer, the sweat-like pore nanofiber membrane is required to have good air permeability, such as Figure 2 As shown in Figure 1, the sweat-like pore nanofiber membrane is fixed in the middle of the pipe, and water at a certain liquid level is injected above the membrane. It can be seen that the hydrophobicity of the sweat-like pore nanofiber membrane prevents water from penetrating downward. When air flow is input to the bottom of the pipe, a large number of bubbles appear in the water column above the fiber membrane, indicating that the sweat-like pore nanofiber membrane is both hydrophobic and breathable.
[0069] In summary, through the electrospinning technology combined with the template collection device, a structurally controllable array arrangement of sweat-like pore nanofiber membrane was successfully prepared. The sparse and dense fiber distribution structure in and around the circular holes made it possible to balance the liquid breakthrough pressure and anti-reverse osmosis performance during subsequent liquid transportation.
[0070] 2 Study on the wetting properties of sweat-mimicking nanofiber membrane
[0071] As a sweat-conducting layer close to the skin, it is necessary to ensure that the material is not wetted over a large area during the sweat-conducting process in order to keep the sweating skin surface dry and comfortable. This application introduces hydrophobic gas-phase SiO2 nanoparticles into PCL nanofibers to study the effect of SiO2 composite content on the wetting properties of sweat-like nanofiber membranes.
[0072] The electrospun fibers were collected with a 0.3-1.0 mm template, and three groups of sweat-like pore nanofiber membranes were obtained by controlling the composite ratio of SiO2 in the spinning solution, namely PCL, PCL / 20% SiO2 (mass percentage), and PCL / 40% SiO2 (mass percentage). The non-woven fabric saturated with methylene blue aqueous solution was placed in a culture dish, and the three groups of samples were laid flat on the surface of the non-woven fabric, and left to stand for 20 minutes. The infiltration process of the methylene blue aqueous solution in the three membranes was recorded by video, and the infiltration area of the three groups of samples at different time points and the total area of the samples were measured using Image J software. The percentage of the infiltration area to the sample area was used to evaluate the effect of different SiO2 composite amounts on the wetting properties of the sweat-like pore nanofiber membrane.
[0073] Experimental results and discussion:
[0074] like Figure 3 As shown in a, by controlling the SiO2 compounding amount in the spinning solution, PCL, PCL / 20%SiO2, and PCL / 40%SiO2 spinning solutions were obtained in turn. It can be seen that the PCL spinning solution is clear and transparent, and as the SiO2 compounding amount increases, the solution gradually becomes milky white. By observing the sweat-like pore nanofiber membranes with different SiO2 compounding amounts with the help of SEM, it can be seen that with the increase of the SiO2 compounding amount, the fiber deposition density inside the circular hole increases, and the patterning effect of the sweat-like pore nanofiber membrane obtained by electrospinning becomes weaker. It is basically difficult to observe the circular hole shape of the PCL / 40%SiO2 nanofiber membrane ( Figure 3 b), this may be because SiO2 itself is not conductive. As the addition of SiO2 reduces the conductivity of the spinning solution, the electric field force on the electrospun fiber in the electric field is reduced, which weakens the advantageous deposition effect of the fiber on the template, resulting in the fiber distribution being more inclined to a non-array pore structure. The morphology of the three groups of nanofiber membranes was observed using high-magnification SEM, and it was found that the surface of PCL fibers without SiO2 was smooth and flat; as the amount of SiO2 composite increased, more and more SiO2 nanoparticles were loaded on the fiber surface, and the fiber surface became rough ( Figure 3 c).
[0075] The water contact angles of the three groups of nanofiber membranes were tested using a static contact angle meter. When the SiO2 composite content was 20% and 40%, the corresponding contact angles increased from 132° to 136°, which were higher than the contact angle of pure PCL fiber membrane (122°) ( Figure 3d). Furthermore, the effect of SiO2 compounding amount on the wetting properties of sweat-like pore nanofiber membranes was studied. The three groups of membranes were laid flat on non-woven fabrics saturated with methylene blue aqueous solution. It can be seen that when the PCL membrane contacts the non-woven fabric, the blue solution quickly penetrates from the lower surface to the upper surface, and nearly 50% of the area of the PCL membrane is infiltrated. Within 6 seconds, the entire membrane is completely infiltrated; while the blue dye did not penetrate to the surface of the PCL / 20% SiO2 and PCL / 40% SiO2 membranes after 20 minutes ( Figure 3 ef); According to Wenzel theory, the surface microstructure can affect the wettability of the material. For a hydrophobic surface, the rougher the structure, the more hydrophobic it is. In the present invention, the introduction of SiO2 nanoparticles into PCL increases the roughness of the fiber surface, thereby successfully reducing the wettability of the nanofiber membrane.
[0076] In summary, when the SiO2 composite ratio is 20% by mass, the prepared nanofiber membrane has both a clear sweat-like pore array structure and low wetting properties.
[0077] 3 Study on the one-way liquid conduction and anti-reverse seepage performance of sweat pore-mimicking fabric
[0078] The sweat-pore-mimicking nanofiber membranes with pore sizes and pore spacings of 0.3-1.0mm, 0.5-1.0mm, 0.7-0.8mm, 0.7-1.0mm, and 0.7-1.2mm were assembled with cotton fabrics to form sweat-pore-mimicking fabrics. Non-woven fabrics composed of nanofiber membranes without array pore structure and cotton fabrics were used as controls to study the liquid transport properties of sweat-pore-mimicking fabrics with different structures.
[0079] 3.1 Study on the transport performance of large amounts of liquids by the spacing of circular holes in sweat-like fabrics
[0080] (1) Liquid transport rate test: Three groups of samples with pore sizes and pore spacings of 0.7-0.8, 0.7-1.0, and 0.7 mm-1.2 mm were selected, and a nanofiber fabric without an array pore structure was used as a control group. The samples were cut into fixed sizes according to the above method. A 100 μL (0.1 g) methylene blue aqueous solution was pipetted with a pipette to simulate sweat droplets on the hydrophobic side of the tetrahedral fabric, so that the liquid could cover multiple sweat pore structures of the sweat pore-simulating fabric. A mobile phone was used to record the entire process of spontaneous liquid transport to the hydrophilic layer, and the entire liquid transport time T was recorded. At the same time, the area of the liquid covering the hydrophobic layer was measured using Image J software, and the average transport rate of 100 μL (0.1 g) of liquid was calculated using formula (1):
[0081] V: V=0.1 / S×T (1)
[0082] Where: S1 is the area of the liquid covering the hydrophobic layer (m 2), T is the time (s) to transport 100 μL (0.1 g) of liquid, V is the average velocity (g·s -1 ·m -2 ), and each group of samples was measured three times to take the average value.
[0083] (2) Moisture residual area test: Based on the above experiments, Image J software was used to measure the blue dye residual area S of the above four groups of samples after liquid transportation. 2, Calculate the blue area percentage S using formula (2) w :
[0084] S w =S2 / S1×100% (2)
[0085] Where: S1 is the area of the liquid covering the hydrophobic layer (m 2 ), S2 is the blue dye area (m 2 ), S w The blue area percentage (%), each group of samples was measured three times and the average value was taken.
[0086] The effects of different fabric structures on the large-volume liquid transport performance were comprehensively evaluated by combining the liquid transport rate and the residual moisture area after transport.
[0087] Experimental results and discussion:
[0088] In order to study the transport performance of sweat-like pore fabrics for large amounts of liquid, based on the above experimental results, three groups of sweat-like pore fabrics with a circular hole diameter of 0.7 mm and hole spacing of 0.8, 1.0, and 1.2 mm were used to study the effect of circular hole spacing on the transport performance of large amounts of liquid, and non-woven fabrics were used as a control. Figure 4 a shows the transport process of 100μL liquid by fabrics with different structures. First, by observing the liquid transport of the sweat-like pore fabric, it can be found that the liquid covers multiple circular hole array structures before transportation, and as time goes on, the liquid tends to gather from the periphery of the circular holes to the circular holes, and finally penetrates vertically into the hydrophilic layer. By recording the liquid transport time of the three groups of sweat-like pore fabrics, it can be found that as the circular hole spacing increases from 0.8mm to 1.2mm, the liquid transport time increases from 3s to 10s, which is attributed to the decrease in the number of circular hole channels. When observing the liquid transport of the non-woven fabric in the control group, the liquid began to be transported at 23s, and the entire liquid transport process took 25s; by measuring the average liquid transport rate ( Figure 4 c) It can be found that as the spacing between the circular holes of the sweat-like fabric increases from 0.8, 1.0 to 1.2 mm, the liquid transport rate decreases from 240, 150 to 91 g·s -1 ·m -2However, the liquid transport rates of the three groups of sweat-like fabrics were all greater than those of nonwoven fabrics (25 g·s -1 ·m -2 ). This is because the hydrophobic layer of nonwoven fabric is composed of dense fibers. Compared with sweat-like pore fabrics, there is no dedicated liquid transport channel. The tightly packed fibers form a small fiber pore size, which means that the resistance to liquid transport increases, resulting in a longer time for liquid invasion.
[0089] In order to describe the residual water content of the hydrophobic layer during the liquid transportation process, the transported liquid was dyed and marked with methylene blue. It can be clearly seen that the residual area of blue dye on the hydrophobic side of fabrics with different structures is different after the liquid transportation process is completed ( Figure 4 ab). As the circular hole spacing of the three groups of sweat-like pore fabrics increases, the proportion of blue area becomes smaller and smaller. When the circular hole spacing is 0.8mm, the blue area accounts for nearly 40% of the liquid coverage area, while when the circular hole spacing is 1.0 and 1.2mm, the blue area is 16% and 12% respectively. Figure 4 d), and the blue imprint is distributed in a circular hole array: the color at the circular hole is dark, and there is almost no color residue around the circular hole, which can prove that in the process of transporting liquid, the circular hole array structure serves as a channel for liquid transportation. Although the liquid did not diffuse on the surface of the non-woven fabric in the control group, the residual area of the blue dye accounted for nearly 100% after the liquid transportation was completed. The results show that the design of the sweat-like pore structure can effectively reduce the residual water on the hydrophobic side during liquid transportation compared with the non-array pore structure, and the residual area decreases with the increase of the circular hole spacing, showing a high efficiency of liquid transportation. This is because in the process of liquid transportation, all the fiber pores of the non-woven fabric in contact with the liquid serve as liquid conduction channels. After the liquid conduction is completed, there is inevitably liquid residue between the fiber pores, and the residual area increases with the increase of the liquid conduction channels; the sweat-like pore fabric is designed with a special liquid conduction channel on the hydrophobic side, and the number of channels decreases with the increase of the circular hole spacing. Therefore, compared with the non-woven fabric, the residual water of the liquid in the hydrophobic layer is reduced, and the liquid transportation efficiency is improved.
[0090] In summary, when the circular hole spacing increases from 0.8 to 1.0 mm, the liquid transport rate decreases by 37.5%, but the moisture residual area decreases by nearly 60%. Therefore, considering the liquid transport rate and the moisture residue after transportation, the circular hole array structure with a circular hole diameter of 0.7 mm and a hole spacing of 1.0 mm is screened out to have the best liquid transport performance, showing the potential of sweat-like pore fabrics in sweat transport.
[0091] 3.2 Study on the anti-reverse seepage performance of sweat pore-like fabrics
[0092] (1) A self-made hydrostatic pressure test device was used to study the anti-reverse seepage performance of sweat pore-simulating fabrics: the bottoms of two plastic injection needles were removed and the tops were butted together. Three groups of sweat pore-simulating fabrics with different hole spacings of 0.7-0.8, 0.7-1.0, and 0.7 mm-1.2 mm were placed at the butt joint with the hydrophilic side facing upwards and fixed with a clip. The methylene blue aqueous solution was slowly dripped into the syringe on the hydrophilic side, and the critical liquid level h at which the liquid just broke through the sweat pore-simulating fabric was recorded. The hydrostatic pressure p corresponding to each group of samples was calculated according to formula (3):
[0093] p=ρ·g·h (3)
[0094] Where: ρ is the solution density (1kg / m 3 ), g is the acceleration due to gravity (9.8 N / kg), h is the height of the liquid level (m), and each set of experiments was performed three times to calculate the average value.
[0095] (2) Calculation of the area ratio of the area around the circular hole:
[0096] S A =(D 2 -πr 2 ) / D 2 ×100% (4)
[0097] Where D is the hole spacing (mm) and r is the hole radius (mm).
[0098] Experimental results and discussion:
[0099] In order to prove the contribution of the area around the circular hole to the liquid anti-reverse osmosis performance, three groups of sweat-like pore fabrics with structures of 0.7-0.8, 0.7-1.0, and 0.7-1.2 were used to study the effect of different circular hole spacing on the liquid anti-reverse osmosis performance. First, 100 μL of methylene blue aqueous solution was dropped on the hydrophilic side of the sweat-like pore fabric, and the blue liquid quickly diffused on the hydrophilic side surface ( Figure 5 a), and as time goes by, the diffusion area becomes larger and larger; at the same time, the use of Figure 5 The homemade hydrostatic pressure test device shown in b fixes the sweat-like pore fabric in the middle and drips liquid slowly to the hydrophilic side. It can be clearly seen that a high water column is formed on the hydrophilic side of the sweat-like pore fabric, and at a certain liquid level, the liquid does not penetrate through the hydrophobic layer, proving that the sweat-like pore fabric has anti-reverse osmosis performance. The hydrostatic pressure is used to evaluate the effect of different circular hole spacings on the anti-reverse osmosis performance of sweat-like pore fabrics ( Figure 5c), the results show that as the circular hole spacing increases from 0.8, 1.0 to 1.2 mm, the corresponding area around the circular hole accounts for 40%, 61.5%, and 73.3% respectively, and the hydrostatic pressure that the sweat-like pore fabric can withstand increases from 310, 370 to 410 Pa. By fitting the area ratio of the circular holes around the three groups of sweat-like pore fabrics and the hydrostatic pressure, it is found that there is a good linear relationship between the two, R 2 =0.9879( Figure 5 d).
[0100] This is because: if the sweat-like pore fabric is simplified into a series of vertically and parallel cylindrical nanopores, this phenomenon can be explained by the Laplace equation. When the liquid passes through the hydrophilic layer and reaches the interface of the hydrophobic layer bionic fiber membrane, it will be affected by the hydrophobic capillary force p provided by the nanopores of the hydrophobic layer. i , which will hinder the liquid from further passing through the hydrophobic layer. The hydrostatic pressure p can be understood as the sum of the Laplace pressures generated by a single hydrophobic nanopore. According to the Laplace equation:
[0101]
[0102] Where: γ is the surface tension of the fluid, θ i is the water contact angle at the hydrophobic nanofiber interface, R i is the radius of the ith nanopore. As the nanopore size decreases, the hydrophobic capillary force generated by a single pore increases. Since the fiber pore size around the circular pores of the sweat-like pore nanofiber membrane is much smaller than the fiber pore size inside the circular pores, the hydrostatic pressure of the sweat-like pore fabric is mainly provided by the area around the circular pores and increases with the increase of the spacing between the circular pores. This is also the reason why the area around the circular pores and the hydrostatic pressure are linearly related. The intercept of the fitting line is not zero because the fibers inside the circular pores also provide a small amount of hydrostatic pressure. It should be noted that under actual conditions, sweat will be transported to the hydrophilic layer and will immediately diffuse in the hydrophilic layer without forming a high liquid surface. Therefore, the above results show that the three groups of sweat-like pore fabrics can effectively prevent sweat back osmosis.
[0103] In summary, when the liquid is transported from the hydrophilic side to the hydrophobic side in the sweat pore-like fabric, the hydrophobic side with the bionic structure mainly uses the area around the circular holes to hinder the further transmission of the liquid, and it is proved that the anti-reverse osmosis performance increases with the increase of the circular hole spacing, which is consistent with the design strategy of this article.
[0104] 3.3 One-way liquid conduction and anti-perspiration reverse osmosis mechanism of sweat-like fabrics
[0105] The volume distribution of fluid in sweat-like pore fabrics was simulated by COMSOL software, and the fluid conduction mechanism of sweat-like pore fabrics was explained in combination with force analysis. Figure 6As shown in ab, each small circle represents an aggregate of 50μm thick hydrophobic fibers, and the large circle represents an aggregate of 80μm thick hydrophilic fibers. When liquid is transported in the fiber membrane, it will be affected by capillary force, and the magnitude of the capillary force can be calculated using the Laplace equation:
[0106] P = 4γcosθ / d (6)
[0107] Where: γ is the surface tension of the liquid, θ is the contact angle of the liquid on the fiber membrane, and d represents the pore size between the fibers of the fiber membrane. When the liquid is transported in the hydrophobic membrane, since the contact angle θ>0, cosθ<0, the capillary force on the liquid is negative, recorded as the hydrophobic capillary force P S , used to describe the repulsive force on the liquid; when the liquid is transported in the hydrophilic membrane, θ < 0, and the capillary force is positive when it is substituted into the above formula, indicating that the liquid is subjected to the hydrophilic capillary force P in the same direction as the transport direction. C .
[0108] When the liquid contacts the hydrophobic layer ( Figure 6 a1), the liquid is subjected to gravity P G and hydrophobic capillary force P S Since the fiber pore size at the circular hole of the hydrophobic layer is much smaller than the fiber pore size around the circular hole, the liquid has a smaller invasion pressure at the circular hole, and the liquid tends to penetrate the hydrophobic layer from the circular hole. When the liquid passes through the hydrophobic layer and contacts the hydrophilic layer ( Figure 6 a2), hydrophilic capillary force direction P C Same as liquid transport direction, at P C Under the action of Figure 6 a3), liquid in P C With P S The transport speed is further accelerated by the combined effect of the push-pull effect. This phenomenon is also called the "push-pull effect". Figure 6 a4), subjected to P from all directions of the hydrophilic layer C and downward P S , the liquid diffuses in the hydrophilic layer and maintains a steady state. When the liquid is transported from the hydrophilic side to the hydrophobic side, C Under the action of Figure 6 b1-b3), when the liquid contacts the hydrophobic layer ( Figure 6 b4), subject to the upward P S and P C , the combined force is upward, eventually overcoming gravity P G , stable in the hydrophilic layer and cannot penetrate further downward. The above analysis explains the unidirectional liquid-conducting principle of sweat-like pore fabrics, and the simulation results are consistent with the experimental results.
[0109] In order to conduct qualitative and quantitative analysis of fluid distribution, the liquid flow rate and pressure at the hydrophobic-hydrophilic layer interface were calculated, such as Figure 6 As shown in Figure c, when the liquid passes through the hydrophobic layer to the hydrophilic layer, the liquid flow rate is significantly accelerated under the negative pressure of nearly -600Pa, and the negative pressure area is located at the circular hole (area 1), which once again verifies that the circular hole is a channel for transporting liquid during the liquid conduction process. At the same time, when the liquid reaches the hydrophobic layer from the hydrophilic layer, the positive pressure at the interface hinders the downward transport of the liquid. In addition, Figure 6 d It can be observed that the pressure around the circular hole (region 2, region 3) is close to 300 Pa, which is much higher than the pressure in the middle area, indicating that the area around the circular hole plays a major role in preventing the liquid from transporting in the reverse direction.
[0110] 4 Preparation and assembly of biomarker detection micro-areas of sweat pore-mimicking nanofiber fabrics
[0111] The electrospun fibers were collected by electrospinning technology combined with a customized template to obtain a PCL / SiO2 nanofiber membrane, which retained the sweat pore array structure and preset three sweat detection areas. Figure 7 b. If Figure 7 As shown in a, a sweat biomarker detection nanofiber fabric that can detect sweat is formed by assembling with cotton fabric loaded with three indicators. Figure 7 As shown in Figure c, in terms of wettability, cotton fabric exhibits superhydrophilicity with a contact angle of about 0°, while the PCL / SiO2 nanofiber membrane combined with it has a contact angle of about 130° and is hydrophobic, which is due to the combined effect of hydrophobic PCL and hydrophobic SiO2 nanoparticles.
[0112] In order to detect three sweat components at the same time, the sweat biomarker detection nanofiber fabric is required to effectively manage the collected sweat in different zones to prevent sweat or indicators from interfering with each other, thus ensuring that the indicator colors will not bleed during the detection process. Figure 7 d shows the sweat management performance of the sweat biomarker detection nanofiber fabric, and a cotton fabric disc is placed on the cotton fabric as a control. A methylene blue aqueous solution is used to simulate sweat, and it is continuously dripped on the sweat detection area of the sweat biomarker detection nanofiber fabric. It can be found that sweat spreads rapidly on the surface of the latter, and the diffusion area gradually increases with the increase in the amount of dripping liquid. The former shows excellent sweat management performance. When the sweat volume increases from 10μL to 70μL, the liquid still gathers firmly in the sweat detection area, forming an increasingly high liquid surface without spreading to the surroundings.
[0113] 5 Sweat biomarker detection Colorimetric detection of different chloride ions, pH, and calcium ions in nanofiber fabrics
[0114] Chloride ion colorimetric detection: Prepare NaCl solutions with chloride ion concentrations of 0, 20, 40, 60, 80, and 100 mM, respectively. Use a pipette to draw 20 μL of the above NaCl solutions of different concentrations and drop them on the cotton fabric disc loaded with the chloride ion indicator. After reacting for 2 minutes, use a mobile phone (Huawei nova 7) to take pictures and record the color image. Use the "Color Recognition" application (downloadable from the Android store) to give the RGB value of the color of the target area to quantify the color change. In order to ensure that the ambient light causes errors in the color results, the entire shooting process is carried out under a 40W LED light, with a uniform blue cardboard as the shooting background, and the shooting distance of the mobile phone is fixed at 20 cm. Each group is measured three times and the average value is taken.
[0115] pH colorimetric detection: Similar to the calcium ion colorimetric detection and chloride ion detection methods, the pH detection range is 4, 5, 6, 7, 8;
[0116] Calcium ion colorimetric detection: Prepare CaCl2 solutions with concentrations ranging from 0, 2, 4, 6, 10, and 15 mM, and the remaining detection steps are the same as the above method. Each group is measured three times and the average value is taken. All experiments were carried out at room temperature of 25°C.
[0117] Experimental results and discussion:
[0118] Smartphones can analyze and record the captured images through mobile phone software, and convert the color changes of sweat biomarker detection nanofiber fabrics into semi-quantitative data. Therefore, it is only necessary to build a correlation between the data and the concentration of related markers to obtain the concentration information of each component of the sweat to be tested. In this study, the three biomarkers Cl in sweat were analyzed. - , pH and Ca 2+ Conduct testing. Figure 8 a is a schematic diagram of the detection of different components. - Detection, we can see Cl - When the concentration increases from 0, 20, 40, 60, 80 to 100 mM, the indicator changes from colorless to yellow, and the color (yellow) gradually deepens ( Figure 8 b), its RGB percentage curve shows that as Cl - With the increase of concentration, the proportion of R value increased from 32.7% to 43%, the proportion of G value remained stable at about 34%, and the proportion of B value decreased from 33% to 22%. - The concentration was linearly fitted and it was found that the R value was - There is a good linear correlation in the concentration range of 5mM-100mM, R 2 =0.9650( Figure 8e). For pH detection, within the physiologically relevant range (pH 4-8), the indicator color tends to gradually change from deep red to green ( Figure 8 c), its RGB percentage curve shows that the R value dropped from 44.1% to 39.1%, the G value increased from 29.2% to 33.7%, and the B value remained at around 27%. The R, G, and B values were linearly fitted with pH, and the G value change had a good linear correlation with pH. 2 =0.9986( Figure 8 f). With the increase of Ca 2+ When the concentration increases from 0, 2, 4, 6, 10 to 15 mM, the indicator color changes from light purple to dark purple ( Figure 8 d), according to the color conversion RGB value display, the R value ratio is basically maintained at around 31%, the G value is reduced from 30.5% to 26.3%, and the B value is increased from 38.7% to 42.2%. 2+ The concentration linear fitting showed that the B value was related to Ca 2+ The concentration linear correlation is good, R 2 =0.9829( Figure 8 g).
[0119] Example 6 Preparation method of sweat pore-mimicking nanofiber membrane
[0120] Weigh 0.4g zinc oxide powder and add it to a mixed solution of 2mL tetrahydrofuran (THF) and 2mL N,N-dimethylformamide (DMF). After ultrasonic dispersion for 1h, add 7.2g polyurethane (PU) to the above dispersion and stir at room temperature for 15h until completely dissolved. The above solution was transferred to a glass syringe, and a spinning collection device with an array circular hole structure was used. The pore size-hole spacing parameter of the metal plate was 0.7-1.0mm. The sweat-like pore nanofiber membrane was obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage of 5kV, flow rate of 0.1mL / h, spinning distance of 5cm, and deposition time of 20min.
[0121] Example 7 Preparation method of sweat pore-mimicking nanofiber membrane
[0122] Weigh 0.13g of hydrophobic SiO2 powder and add it to a mixed solution of 3mL of tetrahydrofuran (THF) and 1mL of N,N-dimethylformamide (DMF). After ultrasonic dispersion for 2h, add 1.2g of polyurethane (PU) to the above dispersion and stir at room temperature for 15h until completely dissolved. The above solution was transferred to a glass syringe, and a spinning collection device with an array circular hole structure was used. The pore size-hole spacing parameter of the metal plate was 0.7-1.0mm. The sweat-like pore nanofiber membrane was obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage of 20kV, flow rate of 2.0mL / h, spinning distance of 15cm, and deposition time of 20min.
[0123] Example 8 Preparation method of sweat pore-mimicking nanofiber membrane
[0124] Weigh 0.3g of titanium oxide powder and add it to a mixed solution of 2mL of tetrahydrofuran (THF) and 2mL of N,N-dimethylformamide (DMF). After ultrasonic dispersion for 1h, add 4g of polylactic acid (PLA) to the above dispersion and stir at room temperature for 15h until completely dissolved. The above solution was transferred to a glass syringe, and a spinning collection device with an array circular hole structure was used. The pore size-hole spacing parameter of the metal plate was 0.7-1.0mm. The sweat-like pore nanofiber membrane was obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage of 15kV, flow rate of 0.8mL / h, spinning distance of 20cm, and deposition time of 15min.
[0125] Example 9 Preparation method of sweat pore-mimicking nanofiber membrane
[0126] Weigh 0.23g of attapulgite powder and add it to a mixed solution of 3mL tetrahydrofuran (THF) and 1mL N,N-dimethylformamide (DMF). After ultrasonic dispersion for 1h, add 0.4g of polylactic acid (PLA) to the above dispersion and stir at room temperature for 15h until completely dissolved. The above solution was transferred to a glass syringe, and a spinning collection device with an array circular hole structure was used. The pore size-hole spacing parameter of the metal plate was 0.7-1.0mm. The sweat-like pore nanofiber membrane was obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage of 15kV, flow rate of 0.8mL / h, spinning distance of 15cm, and deposition time of 15min.
[0127] Example 10 Preparation method of sweat pore-mimicking nanofiber membrane
[0128] Weigh 0.3g of attapulgite powder and add it to 4mL of tetrahydrofuran (THF). After ultrasonic dispersion for 3h, add 5.6g of poly(lactide-glycolide) (PLGA) to the above dispersion and stir at room temperature for 15h until completely dissolved. The above solution is transferred to a glass syringe, and a spinning collection device with an array circular hole structure is used. The pore size-hole spacing parameter of the metal plate is 0.7-1.0mm. The sweat-like pore nanofiber membrane is obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage is 15kV, flow rate is 0.8mL / h, spinning distance is 15cm, and deposition time is 15min.
[0129] Example 11 Preparation method of sweat pore-mimicking nanofiber membrane
[0130] Weigh 0.5g of halloysite powder and add it to a mixed solution of 3mL tetrahydrofuran (THF) and 1mL N,N-dimethylformamide (DMF). After ultrasonic dispersion for 1h, add 0.8g of poly(lactide-glycolide) (PLGA) to the above dispersion and stir at room temperature for 12h until completely dissolved. The above solution was transferred to a glass syringe, and a spinning collection device with an array circular hole structure was used. The pore size-hole spacing parameter of the metal plate was 0.7-1.0mm. The sweat-like pore nanofiber membrane was obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage of 15kV, flow rate of 0.8mL / h, spinning distance of 15cm, and deposition time of 15min.
[0131] Example 12 Preparation method of sweat pore-mimicking nanofiber membrane
[0132] Weigh 2g of graphene oxide powder and add it to 4mL of N,N-dimethylformamide (DMF). After ultrasonic dispersion for 1h, add 6g of polysulfone (PSF) to the above dispersion and stir at room temperature for 12h until completely dissolved. The above solution is transferred to a glass syringe, and a spinning collection device with an array circular hole structure is used. The pore size-hole spacing parameter of the metal plate is: 0.7-1.0mm. The sweat-like pore nanofiber membrane is obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage is 15kV, flow rate is 0.8mL / h, spinning distance is 15cm, and deposition time is 15min.
[0133] Example 13 Preparation method of sweat pore-mimicking nanofiber membrane
[0134] Weigh 1g of hydroxyapatite powder and add it to a mixed solution of 1mL hexafluoroisopropanol and 3mL N,N-dimethylformamide (DMF). After ultrasonic dispersion for 2h, add 0.8g of polysulfone (PSF) to the above dispersion and stir at room temperature for 12h until it is completely dissolved. The above solution is transferred to a glass syringe, and a spinning collection device with an array triangular pore structure is used. The hole spacing parameter of the metal plate is: 1.0mm. The sweat-like pore nanofiber membrane is obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage is 15kV, flow rate is 0.8mL / h, spinning distance is 15cm, and deposition time is 15min.
[0135] Example 14 Preparation method of sweat pore-mimicking nanofiber membrane
[0136] Weigh 1g of titanium oxide powder and add it to a mixed solution of 1mL of tetrahydrofuran (THF) and 3mL of chloroform. After ultrasonic dispersion for 2h, add 0.4g of polymethyl methacrylate (PMMA) to the above dispersion and stir at room temperature for 12h until it is completely dissolved. The above solution is transferred to a glass syringe, and a spinning collection device with an array hexagonal pore structure is used. The pore spacing parameter of the metal plate is: 1.0mm. The sweat-like pore nanofiber membrane is obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage is 15kV, flow rate is 0.8mL / h, spinning distance is 15cm, and deposition time is 15min.
[0137] Example 15 Preparation method of sweat pore-mimicking nanofiber membrane
[0138] Weigh 4g of halloysite powder and add it to a mixed solution of 1mL of dichloromethane and 3mL of N,N-dimethylformamide (DMF). After ultrasonic dispersion for 2h, add 7.2g of polymethyl methacrylate (PMMA) to the above dispersion and stir at room temperature for 12h until it is completely dissolved. The above solution is transferred to a glass syringe, and a spinning collection device with an array rectangular hole structure is used. The hole spacing parameter of the metal plate is: 1.0mm. The sweat-like pore nanofiber membrane is obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage is 15kV, flow rate is 0.8mL / h, spinning distance is 15cm, and deposition time is 15min.
[0139] Example 16 Preparation method of sweat pore-mimicking nanofiber membrane
[0140] Weigh 1g of polystyrene powder and add it to 4mL of ethanol. After ultrasonic dispersion for 2h, add 2.4g of polyvinyl butyral (PVB) to the above dispersion and stir at room temperature for 12h until completely dissolved. The above solution was transferred to a glass syringe, and a spinning collection device with an array triangular pore structure was used. The hole spacing parameter of the metal plate was 1.0mm. The sweat-like pore nanofiber membrane was obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage of 15kV, flow rate of 0.8mL / h, spinning distance of 15cm, and deposition time of 15min.
[0141] Example 17 Preparation method of sweat pore-mimicking nanofiber membrane
[0142] Weigh 1g of polymethyl methacrylate and add it to 4mL of ethanol. After ultrasonic dispersion for 2h, add 0.4g of polyvinyl butyral (PVB) to the above dispersion and stir at room temperature for 12h until completely dissolved. The above solution was transferred to a glass syringe, and a spinning collection device with an array square hole structure was used. The hole spacing parameter of the metal plate was 1.0mm. The sweat-like pore nanofiber membrane was obtained by electrospinning with the help of an electrospinning device. The electrospinning parameters are as follows: voltage of 15kV, flow rate of 0.8mL / h, spinning distance of 15cm, and deposition time of 15min.
[0143] Example 18 Preparation method of sweat pore-mimicking nanofiber membrane
[0144] Weigh 0.8g of hydrophobic SiO2 powder and add it to a mixed solution of 1mL tetrahydrofuran (THF) and 3mL N,N-dimethylformamide (DMF). After ultrasonic dispersion for 4h, add 3.6g of polyvinylidene fluoride (PVDF) to the above dispersion and stir at room temperature for 12h until completely dissolved. The above solution was transferred to a glass syringe and electrospun to obtain a sweat-like pore nanofiber membrane using an electrospinning device. The electrospinning parameters are as follows: voltage of 10kV, flow rate of 1.5mL / h, and spinning distance of 15cm. A spinning collection device with an array irregular pore structure was used, the pore spacing parameter of the metal plate was: 1.0mm, and the deposition time was 12min.
[0145] Example 19 Preparation method of sweat pore-mimicking nanofiber membrane
[0146] Weigh 0.8g of hydrophobic SiO2 powder and add it to 4mL of N,N-dimethylformamide (DMF). After ultrasonic dispersion for 4h, add 0.8g of polyvinylidene fluoride (PVDF) to the above dispersion and stir at room temperature for 12h until completely dissolved. The above solution was transferred to a glass syringe and electrospun to obtain a sweat pore-mimicking nanofiber membrane using an electrospinning device. The electrospinning parameters are as follows: voltage of 7.4kV, flow rate of 0.5mL / h, and spinning distance of 10cm. A screen with an array hole structure is used as the spinning collection device. The hole spacing parameter of the screen is: 1.0mm, and the deposition time is 12min.
[0147] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and the specific implementation of the present invention cannot be limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing a sweat pore-mimicking nanofiber membrane, characterized in that: The method comprises the following steps: dispersing or dissolving soluble hydrophobic polymer materials and micro-nano materials in a solvent to obtain an electrostatic spinning solution; using a spinning collection device with an array pore structure and an electrostatic spinning device to perform electrospinning to obtain a sweat pore-mimicking nanofiber membrane.
2. The preparation method according to claim 1, characterized in that: The soluble hydrophobic polymer material is selected from any one or a combination of poly-ε-caprolactone, polyurethane, polylactic acid, poly(lactide-glycol), polysulfone, polymethyl methacrylate, polyvinyl butyral, and polyvinylidene fluoride.
3. The preparation method according to claim 1, characterized in that: The micro-nano material is selected from any one or a combination of SiO2, zinc oxide, titanium oxide, attapulgite, halloysite, graphene oxide, hydroxyapatite, polystyrene, and polymethyl methacrylate.
4. The preparation method according to claim 1, characterized in that: The solvent is selected from any one or a combination of tetrahydrofuran, N,N-dimethylformamide, dichloromethane, chloroform, hexafluoroisopropanol, and ethanol.
5. The preparation method according to claim 1, characterized in that: The mass concentration of the soluble polymer material in the electrospinning solution is 0.1-5.0 g / ml; the electrospinning parameters are voltage of 5 kv-20 kv, flow rate of 0.1-2.0 ml / h, and spinning distance of 5-20 cm.
6. The preparation method according to claim 1, characterized in that: The spinning collection device with an array hole structure is any one or a combination of a spinning collection device with a circular hole array structure, a spinning collection device with a triangular hole array structure, a spinning collection device with a polygonal hole array structure, a spinning collection device with an irregular hole array structure, and a screen.
7. The sweat pore-mimicking nanofiber membrane obtained by the preparation method according to claim 1, characterized in that: The sweat-conducting pores are arranged in an array on the sweat-pore-mimicking nanofiber membrane.
8. The use of the sweat pore-mimicking nanofiber membrane in fabrics according to claim 7, characterized in that: Application of the sweat pore-mimicking nanofiber membrane in unidirectional liquid-conducting fabrics.
9. The use according to claim 8, characterized in that: The sweat pore-mimicking nanofiber membrane and fabric are assembled into sweat pore-mimicking fabric; and the biomarkers in the sweat derived from the nanofiber membrane are detected by dropping an indicator on the sweat pore-mimicking fabric.
10. The use according to claim 9, characterized in that: The indicator is an indicator used for detection in a one-to-one correspondence with the biomarkers in sweat.
Citation Information
Patent Citations
Method for preparing high-hydrophobicity film by electrostatic spinning
CN110820172A
Preparation method of fabric-based sensing patch for sweat colorimetric analysis
CN113916871A
Preparation method of temperature-sensitive moisture-permeable composite coated fabric with super-hydrophobicity
CN114622422A
Preparation method and application of nano film with directional moisture transport and efficient antibacterial functions
CN115198442A
Porous scaffold with multi-scale structure design and preparation method and application thereof
CN117379594A