Preparation method and application of cationic bio-based environment-friendly slurry for chinlon

The functional nylon fabric is sizing by chitosan-acrylamide-quaternary ammonium salt copolymer as an environmentally friendly slurry, which solves the problem of fabric surface permeation and color in inkjet printing, and improves printing accuracy and color fastness. It has achieved improvements in water, energy saving and antibacterial performance.

CN118958013AActive Publication Date: 2024-11-15SHAOXING QIANYONG TEXTILE CO LTD +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411199421.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

In the prior art In the inkjet printing process, functional nylon fabrics are prone to problems such as fabric surface seepage, low color brightness and uneven color, and traditionally the use of slurry will change the physical properties of the fabric and cause environmental pollution.

Method used

Chitosan is used as raw material, and chitosan-acrylamide-quaternary ammonium salt copolymer is prepared by grafting the amido group and introducing quaternary ammonium groups. As a cationic bio-based environmentally friendly slurry, the nylon fabric is slurryed and two-thick and two-rolled slurry Treatment, regulate the adsorption and fixation of dye molecules, and improve printing accuracy and color brightness.

Benefits of technology

It reduces the permeation of the fabric surface, improves printing accuracy and color fastness, reduces the number of washes, achieves the goal of water conservation and energy saving, and improves the antibacterial properties of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118958013A_ABST
    Figure CN118958013A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of cationic bio-based environment-friendly slurry for chinlon. The preparation method comprises the following steps: firstly, synthesizing a quaternary ammonium salt cationic modifier; then, the chinlon fabric is subjected to sizing treatment, positive groups such as quaternary ammonium salt groups are introduced, and electrostatic repulsion between fibers and dye molecules is reduced; and finally, applying to chinlon fabric ink-jet printing. By reasonably regulating and controlling the surface and interface properties among functional chinlon, slurry and ink droplets, ink permeation on the surface of the chinlon fabric is reduced, the color vividness and the pattern fineness are improved, the ink consumption in the digital printing ink jetting process is reduced, and the effects of energy conservation and emission reduction are achieved; the application of large-scale production of excellent chinlon and functional chinlon fabric products can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a cationic bio-based environmentally friendly slurry used for nylon and functional nylon. Background Art

[0002] Nylon is the second largest chemical fiber after polyester, and the textiles made from it have a wide range of demands and markets in daily clothing, sports and outdoor protection. Functional nylon is a graphene nylon composite fiber. In addition to excellent mechanical properties such as high strength, high modulus and wear resistance, it also has multifunctional properties such as far-infrared warming, antibacterial and anti-mite, antistatic and UV protection. As a functional material, it is widely used in sportswear, swimwear, down jackets, mountaineering clothing, and is the uniform equipment for Olympic and other events.

[0003] Compared with traditional printing and dyeing processes, textile inkjet printing technology has become increasingly common and important due to its lower resource consumption, higher image quality and less wastewater discharge. Inkjet printing is a technology that produces liquid ink droplets that are deposited on a substrate in a specific pattern. When the liquid contains a colorant, an image is generated. However, the porosity, roughness and thickness of the fabric greatly limit the quality of inkjet printing. For digital printing of functional nylon, which is gray in color, the color vividness after printing is insufficient. More importantly, the surface of functional nylon fiber is smooth and the fabric is relatively thin. If the fabric treatment and ink regulation are not relatively perfect, the fabric surface will be infiltrated or the color will not be bright after post-treatment such as steaming and washing. After digital printing, the fabric surface will be exposed to white and uneven color. Therefore, in order to reduce the infiltration of ink on the fabric surface and improve printing accuracy, color intensity and fixation rate, the fabric needs to be sized and cationic modified.

[0004] Conventional printing pretreatment agents currently used are mostly acrylate copolymers, sodium hydroxymethyl cellulose and sodium alginate. However, in the process of preparing the slurry, it is usually necessary to add auxiliaries such as urea, salt and alkali to help expand the fiber and help the dye to develop color or fix color. For the inkjet printing pretreatment process, traditional sizing has certain disadvantages. For example, the use of thickeners in the slurry will change the physical properties and feel of the fabric to a certain extent. At the same time, when the slurry is processed to the surface of the fabric by padding, a large amount of waste liquid will be generated, causing environmental pollution and waste of resources. Therefore, how to reduce the addition of salt and alkali auxiliaries, use clean production technology, and prepare environmentally friendly slurry for textile materials has become a research and development focus.

[0005] At present, chitosan, as a high-tech green material, has been studied by many scholars because of its good biocompatibility, antibacterial and biodegradability. CN102409534A treated cotton fabric with chitosan solution under acidic conditions and found that chitosan molecules can be spontaneously transferred from the solution to the fiber, but it does not affect the internal structure of the fiber. The introduction of amino groups greatly improves the adsorption rate of the pigment. CN105178063A constructed a pure bio-based coating by depositing chitosan and ammonium phytate layer by layer, so that the fabric has certain antibacterial and flame retardant effects, and the tensile strength of cotton fabric is also improved. In recent years, some people have tried to apply chitosan to inkjet printing and have achieved certain results. CN108947346A used chitosan to prepare the slurry for inkjet printing fabric pretreatment. It was confirmed by experiments that chitosan can obtain better color performance when applied to fabric inkjet printing, but the use of chitosan will slightly reduce the tensile strength of the fabric. In existing studies, chitosan has made progress in dyeing, but there is still a lot of room for exploration in its application in dye inkjet printing. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing and applying a cationic bio-based environmentally friendly slurry for nylon, so as to improve the problems of fabric surface penetration and low color vividness during inkjet printing of nylon fabric. By using the slurry to size nylon fabric, the fabric surface penetration is reduced, the printing accuracy is improved, and the color fastness and color depth are improved.

[0007] For functional nylon fabrics, we research and develop a cationic bio-based environmentally friendly slurry system to regulate the interface relationship between nylon-slurry-ink droplets, promote the adsorption and fixation of dye molecules, ensure the color vividness and color uniformity of digitally printed functional nylon fabrics, improve the color fixation rate, reduce the number of washing times, and achieve the goal of saving water and energy.

[0008] The invention uses chitosan as a raw material, grafts amide groups, and then introduces quaternary ammonium groups on the grafted chitosan to prepare chitosan-acrylamide-quaternary ammonium salt copolymers with different grafting rates, performs double-dipping and double-rolling sizing treatment on nylon fabrics, and then uses them for inkjet printing of functional nylon fabrics.

[0009] The preparation and application of a functional nylon special environmentally friendly slurry comprises the following steps:

[0010] (1) Weigh a certain amount of chitosan into a flask, add an appropriate amount of acetic acid solution, stir mechanically and heat under a nitrogen atmosphere.

[0011] (2) Then, the oxidant solution, the reducing agent solution and the acrylamide monomer are added to the flask at the same time, and the reaction is stirred for 3-6 hours under nitrogen. Finally, the terminator is added and stirred for 20-30 minutes. The suspension is filtered, washed and filtered repeatedly with ethanol, and dried in a vacuum oven until the quality is stable to obtain grafted chitosan.

[0012] (3) Add the grafted chitosan to a flask and soak it in isopropyl ketone to fully swell it. Dissolve 3-chloro-2-hydroxypropyl dimethylbutane ammonium chloride in deionized water, slowly pour it into the flask and stir it continuously, and stir it at a constant speed at 80°C for 20-24 hours. After the reaction is completed, filter the liquid, soak the remaining solid in ethanol, wash it, filter it, and put it in a vacuum oven to dry it until the quality is stable, thereby obtaining chitosan quaternary ammonium salt.

[0013] (4) adding chitosan quaternary ammonium salt, acetic acid and urea into deionized water and stirring evenly to obtain a functional nylon special environmentally friendly slurry. The present invention first synthesizes a quaternary ammonium salt cationic modifier, then performs sizing treatment on nylon fabric, introduces positive groups such as quaternary ammonium salt groups, and reduces the electrostatic repulsion between the fiber and the dye molecules; and finally applies it to inkjet printing of nylon fabric.

[0014] The concentration of the acetic acid solution is 0.5-3%, the stirring speed of the mechanical stirring paddle is 600-1200 rpm, and the nitrogen introduction time is 15-30 min. More preferably, the concentration of the acetic acid solution is 1-2%, the stirring speed of the mechanical stirring paddle is 1000-1200 rpm, and the nitrogen introduction time is 30 min.

[0015] The oxidant is any one of potassium persulfate, sodium persulfate, ammonium persulfate, hydrogen peroxide, permanganate and sodium perborate. The oxidant is any one of potassium persulfate, sodium persulfate, ammonium persulfate, hydrogen peroxide, permanganate and sodium perborate. The terminator is any one of hydroquinone and p-tert-butylcatechol. More preferably, the oxidant is any one of potassium persulfate, sodium persulfate and sodium perborate; the reducing agent is any one of sodium bisulfite and sodium sulfite; and the terminator is hydroquinone.

[0016] More preferably, the acrylamide accounts for 10%-50% of the chitosan.

[0017] More preferably, the dosage of the oxidant is 0.02-0.05 mol / L, the molar ratio of the oxidant to the reductant is 1:1.5-3 (most preferably 1:1.5), and the mass percentage of the terminator to the chitosan is 2-5% (most preferably 3%).

[0018] The isopropyl acetone soaking time is 20-24h, the ethanol washing number is 2-6 times, and the chitosan quaternary ammonium salt is placed in a vacuum oven at 75-85°C and dried until the mass is constant. Further preferably, the isopropyl acetone soaking time is 24h, the ethanol washing number is 3 times, and the chitosan quaternary ammonium salt is placed in a vacuum oven and dried at 80°C until the mass is constant.

[0019] Further preferably, in the functional nylon special environmentally friendly slurry, chitosan quaternary ammonium salt accounts for 1-5%, acetic acid accounts for 1-3%, urea accounts for 2-5%, deionized water accounts for 87-96%, and the bath ratio of fabric to aqueous solution is 1:30-50.

[0020] The nylon fabric is subjected to a two-immersion and two-roll sizing treatment, the bath ratio of the nylon fabric to the cationic bio-based environmentally friendly slurry is 1:15-50, the immersion time is 20-30 minutes each time, and the liquid rate is 70%-80%. Then it is dried at 70-80°C for 5-10 minutes. Further preferably, the nylon fabric needs to be subjected to a two-immersion and two-roll sizing treatment, the immersion time is 20 minutes, and the rolling rate is ensured to be 70%-80%. Then it is dried at 70°C for 10 minutes.

[0021] The obtained functional nylon fabric was then subjected to inkjet printing.

[0022] Compared with the prior art, the beneficial effects of the present invention are:

[0023] (1) The preparation and application of a functional nylon special environmentally friendly slurry of the present invention promotes the adsorption and fixation of anionic dye molecules, reduces the amount of ink used in the digital printing inkjet process, ensures the color vividness and color uniformity of the digital printed functional nylon fabric, improves the color fixation rate, reduces the number of water washings, and achieves the goal of saving water and energy.

[0024] (2) The raw material chitosan used in the present invention is a green and environmentally friendly material with good biocompatibility, biodegradability and antibacterial properties. Not only is the raw material easily available, but the prepared nylon-specific environmentally friendly slurry is durable and durable when coated on the surface of the fabric, thereby improving the inkjet printing performance of the dye and the antibacterial properties of the fabric. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the infrared spectrum of the chitosan-acrylamide-quaternary ammonium salt copolymer prepared in Example 1. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is further described in detail below through specific embodiments.

[0027] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the following embodiments, unless otherwise specified, are all conventional methods in the art.

[0028] Embodiment 1:

[0029] A method for preparing a slurry suitable for functional nylon fabrics comprises the following steps:

[0030] (1) Weigh 20 g of chitosan and place it in a flask. Add 40 ml of 1% acetic acid solution, stir evenly with a mechanical stirring paddle and heat at a stirring speed of 1100 rpm. Pass nitrogen into the flask for 30 minutes to exhaust the air.

[0031] (2) When the temperature in the flask reaches 60°C, 5 ml of 0.045 mol / L oxidizing agent potassium persulfate solution, 5 ml of 0.0657 mol / L reducing agent sodium bisulfite solution and 5 g of acrylamide monomer are added to the flask at the same time, and the mass ratio of acrylamide to chitosan is 25%. Stir the reaction for 4 hours while keeping nitrogen flowing, add 0.06 g of terminator hydroquinone, turn off nitrogen, continue stirring for 30 minutes, and the reaction ends. Filter the suspension, wash and filter it repeatedly with ethanol, and dry it in a vacuum oven until the mass is stable to obtain grafted chitosan.

[0032] (3) Add the grafted chitosan to a flask, pour in 50 ml of isopropyl ketone and soak for 24 hours to allow it to fully swell. Dissolve 23.32 g of 3-chloro-2-hydroxypropyldimethylbutane ammonium chloride in deionized water, slowly pour into the flask and stir continuously, and stir the reaction at a constant speed of 80°C for 24 hours. After the reaction is completed, filter the liquid, soak the remaining solid in ethanol, wash, and filter, repeat three times, and place in a vacuum oven at 80°C to dry until the quality is stable to obtain chitosan quaternary ammonium salt, which is chitosan-acrylamide-quaternary ammonium salt copolymer. The infrared spectrum of the chitosan-acrylamide-quaternary ammonium salt copolymer prepared in Example 1 is shown in FIG. Figure 1 As shown, at 3406cm -1 The broad peaks at 1657 cm-1 are the stretching vibration peaks of -COOH, -CONH-, and -CONH2. -1 The absorption peak intensity at 1380-1430cm -1 The bending vibration peak intensity of the -NH- group increased, indicating that acrylamide has been connected to the chitosan main chain to form a graft copolymer. -1 A strong absorption peak of CH bending vibration of -CH3 appeared, which indicated that quaternary ammonium salt side chains were introduced into the copolymer.

[0033] (4) Add 2.554 g of chitosan quaternary ammonium salt, 1.276 g of acetic acid and 3.83 g of urea into 120 ml of deionized water and stir evenly to obtain a functional nylon special environmentally friendly slurry.

[0034] Weigh 6g of nylon fabric (the ratio of fabric to functional nylon special environmentally friendly slurry water bath is 1:20) and perform two-immersion and two-rolling sizing treatments, each immersion time is 20 minutes, and the rolling rate is guaranteed to be 70%-80%. Then place the fabric in an oven for drying at a temperature of 70°C for 10 minutes.

[0035] The fabric after sizing is ready for subsequent inkjet printing.

[0036] Embodiment 2:

[0037] A method for preparing a slurry suitable for functional nylon fabrics comprises the following steps:

[0038] (1) Weigh 20 g of chitosan and place it in a flask. Add 40 ml of 1% acetic acid solution, stir evenly with a mechanical stirring paddle and heat at a stirring speed of 1100 rpm. Pass nitrogen into the flask for 30 minutes to exhaust the air.

[0039] (2) When the temperature in the flask reaches 60°C, 5 ml of 0.045 mol / L oxidizing agent potassium persulfate solution, 5 ml of 0.0657 mol / L reducing agent sodium bisulfite solution and 5 g of acrylamide monomer are added to the flask at the same time, and the mass ratio of acrylamide to chitosan is 25%. Stir the reaction for 4 hours while keeping nitrogen flowing, add 0.06 g of terminator hydroquinone, turn off nitrogen, continue stirring for 30 minutes, and the reaction ends. Filter the suspension, wash and filter it repeatedly with ethanol, and dry it in a vacuum oven until the mass is stable to obtain grafted chitosan.

[0040] (3) Add the grafted chitosan to a flask, pour in 50 ml of isopropyl ketone and soak for 24 hours to fully swell it. Dissolve 23.32 g of 3-chloro-2-hydroxypropyl dimethylbutane ammonium chloride in deionized water, slowly pour into the flask and stir continuously, and stir at a constant speed at 80°C for 24 hours. After the reaction is completed, filter the liquid, soak the remaining solid in ethanol, wash, and filter, repeat three times, and place in a vacuum oven at 80°C to dry until the quality is stable, to obtain chitosan quaternary ammonium salt.

[0041] (4) Add 3.831 g of chitosan quaternary ammonium salt, 1.914 g of acetic acid and 5.745 g of urea into 180 ml of deionized water and stir evenly to obtain a functional nylon special environmentally friendly slurry.

[0042] Weigh 6g of nylon fabric (the ratio of fabric to functional nylon special environmentally friendly slurry water bath is 1:30) and perform two-immersion and two-rolling sizing treatments, each immersion time is 20 minutes, and the rolling rate is guaranteed to be 70%-80%. Then place the fabric in an oven for drying at a temperature of 70°C for 10 minutes.

[0043] Embodiment 3:

[0044] A method for preparing a slurry suitable for functional nylon fabrics comprises the following steps:

[0045] (1) Weigh 20 g of chitosan and place it in a flask. Add 40 ml of 1% acetic acid solution, stir evenly with a mechanical stirring paddle and heat at a stirring speed of 1100 rpm. Pass nitrogen into the flask for 30 minutes to exhaust the air.

[0046] (2) When the temperature in the flask reaches 60°C, 5 ml of 0.045 mol / L oxidizing agent potassium persulfate solution, 5 ml of 0.0657 mol / L reducing agent sodium bisulfite solution and 5 g of acrylamide monomer are added to the flask at the same time, and the mass ratio of acrylamide to chitosan is 25%. Stir the reaction for 4 hours while keeping nitrogen flowing, add 0.06 g of terminator hydroquinone, turn off nitrogen, continue stirring for 30 minutes, and the reaction ends. Filter the suspension, wash and filter it repeatedly with ethanol, and dry it in a vacuum oven until the mass is stable to obtain grafted chitosan.

[0047] (3) Add the grafted chitosan to a flask, pour in 50 ml of isopropyl ketone and soak for 24 hours to fully swell it. Dissolve 23.32 g of 3-chloro-2-hydroxypropyl dimethylbutane ammonium chloride in deionized water, slowly pour into the flask and stir continuously, and stir at a constant speed at 80°C for 24 hours. After the reaction is completed, filter the liquid, soak the remaining solid in ethanol, wash, and filter, repeat three times, and place in a vacuum oven at 80°C to dry until the quality is stable, to obtain chitosan quaternary ammonium salt.

[0048] (4) Add 6.39 g of chitosan quaternary ammonium salt, 3.18 g of acetic acid and 9.57 g of urea into 300 ml of deionized water and stir evenly to obtain a functional nylon special environmentally friendly slurry.

[0049] Weigh 6g of nylon fabric (the ratio of fabric to functional nylon special environmentally friendly sizing agent bath is 1:50) and perform two-immersion and two-rolling sizing treatments, each immersion time is 20 minutes, and the rolling rate is guaranteed to be 70%-80%. Then place the fabric in an oven for drying at a temperature of 70°C for 10 minutes.

[0050] Comparative Example 1

[0051] The commercially available polyvinyl alcohol sizing agent, acetic acid and urea were added into 300 ml of deionized water and stirred evenly to obtain a sizing solution.

[0052] 6 g of fabric was weighed and subjected to double-immersion and double-rolling sizing treatment (the ratio of fabric to deionized water bath was 1:50). The immersion time was 20 min and the rolling rate was 70%-80%.

[0053] After the nylon fabric was subjected to double dipping and double rolling sizing treatment, the fabric was then placed in an oven for drying at a temperature of 70°C for 10 minutes.

[0054] The fabric after sizing is ready for subsequent inkjet printing.

[0055] Comparative Example 2

[0056] (1) Weigh 10.1 g of N,N-dimethylbutylamine and add it to 45 ml of 15% hydrochloric acid solution. Deoxygenate for 20 min and stir evenly at 60°C for 2 h.

[0057] (2) The obtained solution was injected into 20.35 g of epichlorohydrin at a rate of 36 ml / h at 25°C, and the reaction was allowed to proceed for 2 h. 5 g of acrylamide monomer was added to the flask, and the reaction was continued for 4 h at 80°C with constant stirring while nitrogen was maintained. After the reaction was completed, the liquid was filtered, and the remaining solid was soaked, washed, and filtered with ethanol, and the process was repeated three times, and the solid was placed in a vacuum oven and dried at 80°C until the quality was stable.

[0058] (3) Add 6.39 g of sizing agent, 3.18 g of acetic acid and 9.57 g of urea to 300 ml of deionized water and stir well to obtain a sizing solution.

[0059] Weigh 6g of fabric and perform two-immersion and two-rolling sizing treatment (fabric to deionized water bath ratio 1:50), each immersion time is 20min, and the rolling rate is guaranteed to be 70%-80%. Then place the fabric in an oven for drying at 70°C for 10min.

[0060] The fabric after sizing is ready for subsequent inkjet printing.

[0061] Table 1 Properties of various slurries and inkjet printed fabrics

[0062]

[0063] It can be seen from Table 1 that the slurry prepared in Implementation Case 1 is used for functional nylon inkjet printing, and its performance is better than other comparison groups. The slurry viscosity is moderate, and the inkjet printed fabric has high color brightness, good color fastness, good washing and abrasion fastness, and good anti-seepage effect.

[0064] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0065] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a cationic bio-based environmentally friendly slurry for nylon, characterized in that: The following steps are involved: (1) weighing chitosan and acetic acid, mixing them, mechanically stirring and heating under a nitrogen atmosphere to obtain an acetic acid solution of chitosan; (2) then adding an oxidant, a reducing agent and acrylamide monomer to the acetic acid solution of chitosan, stirring the reaction for 3-6 hours under nitrogen, finally adding a terminator and stirring for 20-30 minutes, filtering the suspension, washing and filtering with ethanol repeatedly, and drying in a vacuum oven to obtain grafted chitosan; (3) adding the grafted chitosan to the reactor, pouring isopropyl ketone into the reactor to soak it and fully swell it, dissolving 3-chloro-2-hydroxypropyl dimethylbutane ammonium chloride with deionized water, pouring it into the reactor and stirring it continuously, stirring and reacting at 70-90° C. for 20-24 hours, filtering the liquid after the reaction is completed, soaking the remaining solid with ethanol, washing, filtering it, and drying it in a vacuum oven to obtain chitosan quaternary ammonium salt; (4) Chitosan quaternary ammonium salt, acetic acid and urea are added into deionized water and stirred evenly to obtain a cationic bio-based environmentally friendly slurry used for nylon.

2. The method for preparing a cationic bio-based environmentally friendly slurry for nylon according to claim 1, characterized in that: In step (1), the stirring speed of the mechanical stirring paddle is 600-1200 rpm.

3. The method for preparing a cationic bio-based environmentally friendly slurry for nylon according to claim 1, characterized in that: In step (2), the oxidant is any one of potassium persulfate, sodium persulfate, ammonium persulfate, hydrogen peroxide, permanganate, and sodium perborate.

4. The method for preparing a cationic bio-based environmentally friendly slurry for nylon according to claim 1, characterized in that: In step (2), the reducing agent is any one of ferrous sulfate, sodium hypophosphite, oxalic acid, sodium thiosulfate, sodium bisulfite, and sodium sulfite.

5. The method for preparing a cationic bio-based environmentally friendly slurry for nylon according to claim 1, characterized in that: In step (2), the terminator is any one of hydroquinone and p-tert-butylcatechol.

6. The method for preparing a cationic bio-based environmentally friendly slurry for nylon according to claim 1, characterized in that: In step (2), the molar ratio of the oxidant to the reductant is 1:1.5-3, the amount of acrylamide added is 10%-50% of the mass of chitosan, and the amount of the terminator added is 0.2-0.5% of the mass of chitosan.

7. The method for preparing a cationic bio-based environmentally friendly slurry for nylon according to claim 1, characterized in that: In step (3), the soaking time of isopropyl tone is 20-24h.

8. The method for preparing a cationic bio-based environmentally friendly slurry for nylon according to claim 1, characterized in that: In step (4), the cationic bio-based environmentally friendly slurry used for nylon adopts the following raw materials in percentage by weight:

9. Use of the cationic bio-based environmentally friendly slurry for nylon prepared by the preparation method according to any one of claims 1 to 8 in inkjet printing of nylon fabric.

10. The use according to claim 9, characterized in that: include: The nylon fabric is subjected to double-immersion and double-rolling sizing treatment, the bath ratio of the nylon fabric to the cationic bio-based environmentally friendly sizing agent is 1:15-50, the immersion time each time is 20-30 minutes, the liquid carrying rate is 70%-80%, and then it is dried at 70-80°C for 5-10 minutes.

Citation Information

Patent Citations

  • Method for improving fabric ink-jet printing performance by using quaternary ammonium chitosan

    CN102071574A

  • Chitosan modified nylon fabric and manufacturing method thereof

    CN102199876A

  • Preparation method for modified cation retention and filter aid

    CN103819612A

  • Ultraviolet-resistant sun-proof garment

    CN109082882A

  • Active digital printing base pulp and preparation method thereof

    CN110409199A