Method for rapidly detecting coating integrity rate of titanium dioxide

Through the complex color development reaction between indicator and titanium dioxide, the color difference value is detected by using a color difference instrument, which solves the problem of insufficient detection in the prior art, and achieves a rapid and accurate evaluation of the completeness of titanium dioxide coating, which is suitable for Industrial production and quality control ensure product quality and performance stability.

CN118961690APending Publication Date: 2024-11-15SICHUAN JINYAHUI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411143888.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art has problems in detecting the integrity of titanium dioxide surface coating, which is not fast, simple and accurate enough, especially because the color change reaction between 1,3-butanediol and nanotitanium dioxide mixture is slow and uneven, which affects the test results. There are abnormal phenomena in the evaluation of light stability in the alumina coating system.

Method used

After complexing with titanium dioxide, the color difference is developed by using an indicator to detect the color difference through a color difference meter and establish a reference value to quickly evaluate the coating integrity rate, simplify the calculation process, and improve the accuracy and repeatability of the detection.

Benefits of technology

It realizes rapid and accurate detection of the completeness of titanium dioxide coating, improves the accuracy and repeatability of measurement results, is suitable for modern industrial production and quality control, improves detection efficiency, and ensures product quality and performance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118961690A_ABST
    Figure CN118961690A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of inspection and detection, and particularly relates to a method for rapidly detecting the coating integrity rate of titanium dioxide, which comprises the following steps: S1, reference establishment: uniformly mixing uncoated titanium dioxide and completely coated titanium dioxide with an indicator respectively, detecting the color b values of the uncoated titanium dioxide and the completely coated titanium dioxide respectively by using a colorimeter, and calculating the color b value of the completely coated titanium dioxide; measuring the value b0 of the uncoated titanium dioxide and the value b1 of the completely coated titanium dioxide, and taking the measured value b0 and the measured value b1 as reference values of the coating integrity rate; and S2, sample testing: uniformly mixing the coated titanium dioxide sample with an indicator, testing the color b value of the mixture by using a colorimeter, and then comparing the color b value with the reference value in S1 to calculate the coating integrity rate. The method disclosed by the invention is simple, rapid and accurate, can realize rapid detection of the titanium dioxide coating integrity rate, and shows great application potential in the aspects of rapid evaluation and real-time monitoring of the titanium dioxide coating integrity rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of inspection and detection, and specifically relates to a method for quickly detecting the coating integrity rate of titanium dioxide. Background Art

[0002] Titanium dioxide is an important chemical raw material, which can be used in coatings, plastics, papermaking, rubber, ink, cosmetics and other fields. Titanium dioxide without surface treatment is easy to agglomerate, has poor dispersibility and high photochemical activity, so its particles need to be coated on the surface. The coating method usually used is inorganic coating, or organic coating on the outside of the inorganic coating layer.

[0003] There are many non-destructive detection methods for evaluating the surface coating effect of titanium dioxide in the prior art, including scanning electron microscopy (SEM) combined with X-ray energy spectrometer (EDS), X-ray fluorescence spectroscopy, infrared spectroscopy, electrochemical detection, etc. For example, patent document CN103411987A discloses a method for characterizing the uniformity and dispersion of titanium dioxide surface coating. The method uses a scanning electron microscope and an X-ray energy spectrometer combined with a scanning electron microscope to detect the chemical composition of different points on the titanium dioxide surface to judge the uniformity of its coating. The document "Preparation and Performance Study of Hydrated Alumina Coated on Titanium Dioxide Surface" (Zhou Wenjing, Xu Ran, Tang Chencheng, et al. Preparation and Performance Study of Hydrated Alumina Coated on Titanium Dioxide Surface [J]. Shanxi Metallurgy, 2023, 46(4):9-10.) discloses the use of an X-ray fluorescence spectrometer for testing. Patent document CN 116675248 A mixes the sample with 1,3-butanediol and tests the color difference value of the sample before and after illumination to make a judgment. In addition, the existing technology is also evaluated based on the results of application tests. For example, after the sample is prepared according to the formula, it is coated and the fineness of the particles in the film layer is observed; for example, the hydrophobic properties of the sample after organic coating are examined; for the sample coated with nano-silica, the dissolution rate of nano-titanium dioxide is tested after dissolving it in sulfuric acid to evaluate the integrity of the coating, etc.

[0004] However, there are still some shortcomings in the existing test methods. For example, the color change reaction of the above-mentioned 1,3-butanediol and nano-titanium dioxide mixture is slow, and the color change is uneven, which will affect the test results. In the alumina coating system, there are abnormalities when using photostability to evaluate the coating integrity. The use of transmission electron microscopy or evaluation through application of test results has a long cycle or a limited detection range, and the detection is not fast and simple enough.

[0005] Therefore, developing a fast, simple and accurate method for detecting the surface coating integrity of titanium dioxide is of great significance for improving product quality and production efficiency. Summary of the invention

[0006] In view of this, the technical problem to be solved by the present invention is to use an indicator to complex with titanium dioxide and then develop color, thereby providing a method for quickly detecting the completeness of titanium dioxide coating. The method has the advantages of being simple, rapid and accurate. The method of the present invention is achieved by the following technical solutions: In one aspect, the present invention provides a method for rapidly detecting the titanium dioxide coating integrity rate, comprising the following steps: S1. Benchmark establishment: After uncoated titanium dioxide and completely coated titanium dioxide are mixed evenly with an indicator, the color b values ​​of the two are detected by a colorimeter. The uncoated titanium dioxide is measured as the b0 value, and the completely coated titanium dioxide is measured as the b1 value. The measured b0 value and b1 value are used as the benchmark values ​​of the coating completeness rate; S2. Sample testing: After the coated titanium dioxide sample and the indicator are evenly mixed, the color b value of the mixture is tested with a colorimeter, and then compared with the reference value in S1 to calculate the coating completeness rate.

[0007] In some embodiments, the uncoated titanium dioxide b0 has a coating completeness of 0%; the fully coated titanium dioxide b1 has a coating completeness of 100%, and the calculation method of the coating completeness in S2 is: (b0 value-b value) / (b0 value-b1 value)×100%.

[0008] In some embodiments, the completely coated titanium dioxide in S1 is prepared by calcination, and is coated after calcination, wherein the coating is inorganic coating.

[0009] In some embodiments, an inorganic coating layer is further included followed by an organic coating on the outside.

[0010] In some embodiments, the inorganic coating comprises aluminum hydroxide, silica or zirconium hydroxide; The organic coating adopts coating materials including: stearic acid, dimethyl silicone oil, and polymethylsiloxane.

[0011] In some embodiments, the indicator is dicaprylyl carbonate.

[0012] In some embodiments, the moisture content of the coated titanium dioxide sample is no greater than 3%.

[0013] In some embodiments, the inorganic coating includes a drying step, and the drying temperature can be selected to be 100-110°C.

[0014] In some embodiments, the uniform mixing step in S2 further includes adding zirconium beads and performing a dispersion step using a disperser, wherein the particle size of the zirconium beads is selected from 0.5 mm to 1.5 mm, and the dispersion time of the disperser is 5 min to 20 min.

[0015] In some embodiments, the inorganic coating amount is 2-19% based on titanium dioxide.

[0016] The beneficial effects of the present invention include: The present invention proposes a method for detecting the completeness of titanium dioxide coating, which uses a colorimeter as a detection tool, establishes a color reference value through a scientific method, and realizes a rapid and accurate evaluation of the integrity of the titanium dioxide coating layer. This method uses a colorimeter to detect through a complex color reaction between an indicator and titanium dioxide, and intuitively reflects the coating of titanium dioxide. It is applicable to various types of titanium dioxide coating materials, helps to ensure the quality and performance stability of the product, improves the accuracy and repeatability of the measurement results, and improves the detection efficiency. The method of the present invention is simple, rapid, and efficient, and meets the needs of modern industrial production and quality control, especially in the rapid evaluation and real-time monitoring of the completeness of titanium dioxide coating. It shows great application potential and is of great significance to promoting technological progress in related fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.

[0018] Figure 1 A flow chart of the method steps for quickly detecting the titanium dioxide coating integrity rate provided in some embodiments of the present invention. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, one or more embodiments of the present invention will be described below in conjunction with the accompanying drawings. The flowchart illustrates the process performed by the system according to the present invention. It can be understood that the execution of the flowchart does not need to be performed in sequence, one or more steps can be omitted, one or more execution steps can be added, and one or more steps can be performed in sequence or in reverse order, and even in some embodiments, one or more steps can be performed simultaneously.

[0020] The % involved in the content in the present invention is mass percentage, for example, "the moisture content of the coated titanium dioxide sample is not higher than 3%" means "the moisture content of the coated titanium dioxide sample accounts for 3% of the total mass of the sample"; The 98% concentrated sulfuric acid in the present invention refers to a commercially available sulfuric acid solution with a mass fraction of 98%.

[0021] like Figure 1As shown, the present invention provides a method for quickly detecting the titanium dioxide coating integrity rate, comprising the following steps: S1. Benchmark establishment: After uncoated titanium dioxide and completely coated titanium dioxide are mixed evenly with an indicator, the color b values ​​of the two are detected by a colorimeter. The uncoated titanium dioxide is measured as the b0 value, and the completely coated titanium dioxide is measured as the b1 value. The measured b0 value and b1 value are used as the benchmark values ​​of the coating completeness rate; S2. Sample testing: After the coated titanium dioxide sample and the indicator are evenly mixed, the color b value of the mixture is tested with a colorimeter, and then compared with the reference value in S1 to calculate the coating completeness rate.

[0022] The present invention provides a method for detecting the completeness of titanium dioxide coating, which uses a colorimeter to detect the complex color reaction of titanium dioxide and an indicator, and quickly evaluates the integrity of the coating layer by establishing a color reference value. The method improves the measurement accuracy and repeatability, is applicable to various types of titanium dioxide coating materials, ensures stable product quality, and improves detection efficiency.

[0023] In some embodiments, the uncoated titanium dioxide b0 is a coating completeness of 0%; the fully coated titanium dioxide b1 is a coating completeness of 100%, and the coating completeness in S2 is calculated as: (b0 value-b value) / (b0 value-b1 value)×100%. The present invention further simplifies the calculation process of the coating completeness by defining the color values ​​of uncoated and fully coated titanium dioxide as a benchmark, making the results more intuitive and convenient for quantitative analysis.

[0024] In some embodiments, the preparation of the completely coated titanium dioxide in S1 is carried out by burning, and after burning, coating is performed, and the coating is inorganic coating. The present invention adopts the burning method to further eliminate the surface defects of the titanium dioxide particles and reduce the photoactivity, and the sufficient amount of inorganic coating after burning is to achieve complete coating and isolation of the titanium dioxide particles.

[0025] In some embodiments, an inorganic coating layer is further provided and then an organic coating is performed on the outside. Combining inorganic and organic coatings can provide dual protection and enhance the stability and application performance of titanium dioxide.

[0026] In some embodiments, the inorganic coating includes aluminum hydroxide, silica or zirconium hydroxide, and other white inorganic coating materials commonly used in the prior art may also be used.

[0027] The organic coating includes stearic acid, dimethyl silicone oil, polymethylsiloxane, and other white or colorless organic coating materials commonly used in the prior art.

[0028] In some embodiments, the indicator is dioctyl carbonate. Selecting a specific indicator can improve the sensitivity and selectivity of the detection, and ensure the direct relationship between the color change and the coating integrity rate. The dioctyl carbonate of the present invention is a colorless transparent liquid with low viscosity, strong permeability and dispersibility, and will immediately generate a yellow complex after contacting titanium dioxide, and will not change color when contacting with aluminum hydroxide, silica, zirconium hydroxide and commonly used organic matter as a surface coating. The complex generated is less, and the color of the mixture is light, and the complex generated is more, and the color of the mixture is dark.

[0029] In order to allow the indicator to further contact with titanium dioxide, in some embodiments, the moisture content of the coated titanium dioxide sample is not higher than 3%, because too much water molecules will form a film on the surface of the particles, preventing the indicator from contacting the titanium dioxide particles.

[0030] In some embodiments, the inorganic coating includes a drying step, and the drying temperature can be determined according to the coating material so as not to change the coating state, structure and color. In the present invention, the drying temperature of the inorganic coating can be selected to be 100-110°C, including but not limited to 100°C, 105°C or 110°C. If the coating layer is an organic matter, the drying temperature can be appropriately lowered to ensure that the organic matter does not deteriorate.

[0031] In order to ensure that the sample and the indicator are fully mixed, a small amount of zirconium beads can be added and dispersed by a disperser. In some embodiments of the present invention, the mixing step in S2 also includes adding zirconium beads and dispersing them by a disperser. The particle size of the zirconium beads is selected from 0.5mm~1.5mm, and the dispersion time of the disperser is 5min~20min, including but not limited to 5min, 10min, 15min or 20min.

[0032] In some embodiments, the inorganic coating amount, based on titanium dioxide, is 2-19%, including but not limited to 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18% or 19%.

[0033] The scheme of the present invention will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the embodiments, conventional technical schemes in the art are used. Where the reagents or instruments are not indicated by the manufacturer, they are all conventional products that can be obtained commercially.

[0034] Example 1 Nano titanium dioxide is coated with aluminum hydroxide, the coating amount is 2% of the mass of TiO2, and the moisture content of the sample is 1.1%. Weigh 15g of the sample, 5g of dioctyl carbonate, and 10g of zirconium beads with a particle size of 0.5~1.5mm, disperse them for 5 minutes using a rapid dispersion tester, and the b value of the mixture is 15.2 measured by a colorimeter. The color b0 value of the mixture of uncoated nano titanium dioxide and dioctyl carbonate is 17.5, and the color b1 value of the mixture of nano titanium dioxide completely coated with aluminum hydroxide and dioctyl carbonate is 1.0. The calculation shows that the coating completeness of the sample is 13.9%.

[0035] Example 2 Nano titanium dioxide is coated with aluminum hydroxide, the coating amount is 10% of the mass of TiO2, and the moisture content of the sample is 3%. Weigh 15g of the sample, 5g of dioctyl carbonate, and 10g of zirconium beads with a particle size of 0.5~1.5mm, disperse them for 20 minutes using a rapid dispersion tester, and the b value of the mixture is 7.9 measured by a colorimeter. The color b0 value of the mixture of uncoated nano titanium dioxide and dioctyl carbonate is 17.5, and the color b1 value of the mixture of nano titanium dioxide completely coated with aluminum hydroxide and dioctyl carbonate is 1.0. The calculation shows that the coating completeness of the sample is 58.2%.

[0036] Example 3 Nano titanium dioxide is coated with aluminum hydroxide, the coating amount is 19% of the mass of TiO2, and the moisture content of the sample is 1.35%. Weigh 15g of the sample, 5g of dioctyl carbonate, and 10g of zirconium beads with a particle size of 0.5~1.5mm, disperse them for 10 minutes using a rapid dispersion tester, and the b value of the mixture is 2.1 measured by a colorimeter. The color b0 value of the mixture of uncoated nano titanium dioxide and dioctyl carbonate is 17.5, and the color b1 value of the mixture of nano titanium dioxide and dioctyl carbonate that is completely coated with aluminum hydroxide is 1.0. The calculation shows that the coating completeness of the sample is 93.3%.

[0037] Example 4 Nano titanium dioxide is coated with silica, the coating amount is 11.0% of the mass of TiO2, and the moisture content of the sample is 1.0%. Weigh 15g of the sample, 5g of dioctyl carbonate, and 10g of zirconium beads with a particle size of 0.5~1.5mm, disperse them for 10 minutes using a rapid dispersion tester, and the b value of the mixture is 7.5 measured by a colorimeter. The color b0 value of the mixture of uncoated nano titanium dioxide and dioctyl carbonate is 17.5, and the color b1 value of the mixture of nano titanium dioxide and dioctyl carbonate completely coated with silica is 0.9. The calculation shows that the coating completeness of the sample is 60.2%.

[0038] Example 5 Pigment-grade titanium dioxide is coated with silica, and the coating amount is 3.0% of the mass of TiO2. The moisture content of the sample is 1.0%. Weigh 15g of the sample, 15g of dioctyl carbonate, and 10g of zirconium beads with a particle size of 0.5~1.5mm. Use a fast dispersion tester to disperse for 10 minutes. Use a colorimeter to measure the b value of the mixture to be 2.6. The color b0 value of the mixture of uncoated nano titanium dioxide and dioctyl carbonate is 5.6, and the color b1 value of the mixture of nano titanium dioxide and dioctyl carbonate completely coated with silica is 2.5. Calculation shows that the coating completeness of the sample is 96.8%.

[0039] Example 6 Nano titanium dioxide is coated with aluminum hydroxide and then surface treated with stearic acid. The amount of aluminum hydroxide coated is 7.0% of the mass of TiO2, and the amount of stearic acid used is 5.0% of the mass of TiO2. The moisture content of the sample is 1.4%. Weigh 15g of the sample, 5g of dioctyl carbonate, and 10g of zirconium beads with a particle size of 0.5~1.5mm. Disperse them for 10 minutes using a rapid dispersion tester, and the b value of the mixture is 8.3 measured by a colorimeter. The color b0 value of the mixture of uncoated nano titanium dioxide and dioctyl carbonate is 17.5, and the color b1 value of the mixture of nano titanium dioxide completely coated with aluminum hydroxide and dioctyl carbonate is 1.0. It is calculated that the coating completeness of the sample is 55.8%.

[0040] Comparative Example 1 Nano-titanium dioxide was coated with aluminum hydroxide and then surface treated with stearic acid. The amount of aluminum hydroxide coated was 7.0% of the mass of TiO2, and the amount of stearic acid used was 5.0% of the mass of TiO2. The moisture content of the sample was 1.4%. Weigh 2g of the sample, add 100mL of deionized water, and stir with an electric stirrer for 30min at a stirring speed of 200rpm. The transmittance of the supernatant was tested with a UV spectrophotometer, and the result was 88.3%, that is, the organic coating integrity of the sample was close to 88.3%.

[0041] Comparative Example 2 Nano-titanium dioxide was coated with aluminum hydroxide, with a coating amount of 10% of the mass of TiO2 and a water content of 1.2%. The sample was mixed with 1,3-butanediol at a ratio of 1:1 and its light stability was tested. The color difference value ΔE was 2.3, and the light stability (color difference value ΔE) of the uncoated nano-titanium dioxide was 19.8. The coating completeness was calculated to be 58.2%.

[0042] Comparative Example 3 Pigment-grade titanium dioxide was coated with silica, with a coating amount of 3.0% of the mass of TiO2 and a water content of 1.0%. After mixing with 98% concentrated sulfuric acid, it was gently stirred at 120°C for 2 hours. The TiO2 content in the filtrate was tested, and the coating completeness of the sample was calculated to be 80.5%.

[0043] Table 1 is a comparison of the test conditions and parameters of the method of the present invention and comparative examples 1 to 3, and the results are as follows: Table 1 Examples and Comparative Examples Results

[0044] As can be seen from Table 1, the titanium dioxide coating process of Comparative Example 1 and Example 6 is exactly the same (inorganic coating is coated with organic coating outside), the only difference is that the technical means of detection are different. Comparative Example 1 adopts the ultraviolet spectrophotometer method, and Example 6 adopts the method of the present invention. It can be seen from the results that the result of Comparative Example 1 is higher than that of Example 6. The reason is that Comparative Example 1 adopts ultraviolet spectrophotometer detection, adds 100mL of deionized water, and stirs with an electric stirrer for 30min at a stirring speed of 200rpm. The transmittance of the supernatant was tested with an ultraviolet spectrophotometer, and the color was developed after stirring with water. Although the titanium dioxide surface of Comparative Example 1 is coated with stearic acid, there will be gaps in the organic coating layer of some titanium dioxide, and water penetrates into the gaps. At this time, part of the organic coating layer will fall off in the water, resulting in a high measurement result; Comparative Example 2 was evaluated by the color difference method, and the results were compared with those of Example 4. Since the color change reaction of the mixture of 1,3-butanediol and nano-titanium dioxide was slow and the color change was uneven, it would affect the test results. When the detection environment was dark or the light was dim, the color change of the mixture of 1,3-butanediol and nano-titanium dioxide would be affected. However, the method of the present invention was not affected by the lighting conditions of the detection environment.

[0045] The titanium dioxide coating processes of Comparative Example 3 and Example 5 are exactly the same, and the only difference is that Comparative Example 3 is tested by the sulfuric acid dissolution method. Compared with the results of Example 5, the coating integrity rate of the sample in Comparative Example 3 is lower. This is because the inorganic oxide layer coated with the titanium dioxide particles is mixed with 98% concentrated sulfuric acid and then gently stirred at 120°C for 2 hours. There is a gap between the titanium dioxide particles and the coating layer. Sulfuric acid reacts with titanium dioxide through the gap, and the coating layer will fall off. At this time, the TiO2 content in the test filtrate is TiO2 formed after the silica falls off after TiO2 is coated with silica. Therefore, it is inevitable that the coating integrity rate is lower than the actual coating integrity rate, resulting in a deviation in the measurement result.

[0046] In summary, the method of the present invention is simple, rapid and accurate, and can realize rapid detection of the titanium dioxide coating completeness rate.

[0047] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0048] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for rapidly detecting the completeness of titanium dioxide coating, characterized in that: The steps include: S1. Benchmark establishment: After uncoated titanium dioxide and completely coated titanium dioxide are mixed evenly with an indicator, the color b values ​​of the two are detected by a colorimeter. The uncoated titanium dioxide is measured as the b0 value, and the completely coated titanium dioxide is measured as the b1 value. The measured b0 value and b1 value are used as the benchmark values ​​of the coating completeness rate; S2. Sample testing: After the coated titanium dioxide sample and the indicator are evenly mixed, the color b value of the mixture is tested with a colorimeter, and then compared with the reference value in S1 to calculate the coating completeness rate.

2. The method for rapidly detecting the titanium dioxide coating integrity rate according to claim 1, characterized in that: The uncoated titanium dioxide b0 has a coating completeness rate of 0%; the fully coated titanium dioxide b1 has a coating completeness rate of 100%. The calculation method of the coating completeness rate in S2 is: (b0 value-b value) / (b0 value-b1 value)×100%.

3. The method for rapidly detecting the titanium dioxide coating integrity rate according to claim 1, characterized in that: The completely coated titanium dioxide in S1 is prepared by burning, and after burning, it is coated, and the coating is inorganic coating.

4. The method for rapidly detecting the titanium dioxide coating integrity rate according to claim 3, characterized in that: It also includes an inorganic coating layer followed by an organic coating on the outside.

5. The method for rapidly detecting the titanium dioxide coating integrity rate according to claim 4, characterized in that: The inorganic coating adopts a coating material including aluminum hydroxide, silica or zirconium hydroxide; The organic coating adopts coating materials including: stearic acid, dimethyl silicone oil, and polymethylsiloxane.

6. The method for rapidly detecting the titanium dioxide coating integrity rate according to claim 1, characterized in that: The indicator is dicaprylyl carbonate.

7. The method for rapidly detecting the titanium dioxide coating integrity rate according to claim 1, characterized in that: The moisture content of the coated titanium dioxide sample is not higher than 3%.

8. The method for rapidly detecting the titanium dioxide coating integrity rate according to claim 3, characterized in that: The inorganic coating includes a drying step, and the drying temperature can be selected to be 100-110°C.

9. The method for rapidly detecting the titanium dioxide coating integrity rate according to claim 3, characterized in that: The uniform mixing step in S2 also includes adding zirconium beads and performing a dispersion step using a disperser, wherein the particle size of the zirconium beads is selected from 0.5 mm to 1.5 mm, and the dispersion time of the disperser is 5 min to 20 min.

10. The method for rapidly detecting the titanium dioxide coating integrity rate according to claim 3, characterized in that: The inorganic coating amount is 2-19% based on titanium dioxide.