Healthy eye-protecting Mini LED backlight module and manufacturing method thereof

By using a modified hollow mesoporous silica-coated diffuser plate in the Mini LED backlight module, the problem of uneven light distribution was solved, resulting in a more uniform light distribution and eye-friendly effect, improving visual comfort and the lifespan of the backlight module.

CN118963025AActive Publication Date: 2024-11-15KUNSHAN DUMMEI ELECTRONIC IND CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411202336.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The uneven light distribution in existing Mini LED backlight modules leads to excessively high local light intensity, affecting visual comfort and potentially causing eye fatigue and vision loss.

Method used

A diffuser plate containing a modified hollow mesoporous silica coating is formed by coating a PET film with a coating liquid composed of a light diffusing agent, modified hollow mesoporous silica, a photoinitiator, a diluent, and polyurethane acrylate, resulting in a diffuser plate with high light transmittance and high haze, which is used in Mini LED backlight modules.

Benefits of technology

It achieves a more uniform light distribution, reduces "spots" or "hot spots" caused by excessive local light intensity, reduces eye fatigue and pressure from prolonged screen viewing, and improves the lifespan of the backlight module and eye protection effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118963025A_ABST
    Figure CN118963025A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of backlight modules, in particular to a healthy and eye-protecting Mini LED backlight module and a manufacturing method thereof. The invention discloses a healthy and eye-protecting Mini LED backlight module, the healthy and eye-protecting Mini LED backlight module comprises a Mini LED lamp panel and a diffusion plate arranged above the Mini LED lamp panel, and the diffusion plate comprises a base material and coatings coated on the two surfaces of the base material; the base material is a PET (Polyethylene Terephthalate) film; the coating is a coating containing modified hollow mesoporous silica. According to the healthy and eye-protecting Mini LED backlight module, the backlight plate which is high in light transmittance, high in haze and good in light diffusivity is prepared, the backlight module which is obvious in diffusion effect and good in light uniformity can be obtained, and the backlight module has the good healthy and eye-protecting effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of backlight modules, and more specifically, to a healthy and eye-protecting Mini LED backlight module and a method for manufacturing the same. Background Art

[0002] Liquid crystal display has become the mainstream flat panel display technology. Since liquid crystal does not emit light, a backlight is needed to provide illumination. The brightness, color, and volume of the backlight module largely determine the performance of the final display. Thinning display products has become a popular trend, which requires the backlight module to minimize thickness.

[0003] Light Emitting Diode (LED) is now the mainstream light source for LCD backlight modules. Direct-type backlight modules usually include multiple LEDs. As the size of LED chips increases, the power of a single LED continues to increase, and the spacing between LEDs becomes larger and larger. It is usually necessary to diffuse the light emitted by the LED through a secondary lens, and then further disperse the light through a diffusion film to form a uniform extended light source. The optical distance (OD) between the LED and the diffusion film is usually large, resulting in a large thickness of the backlight module. With the development of semiconductor technology, the size of LED light-emitting chips has been reduced to a few hundred microns, and Mini LED chips have emerged. Mini LED chips are small in size and low in heat generation, and can be densely arranged in a matrix in the backlight module. With the continuous development of display technology, consumers have increasing requirements for the visual effects and health performance of displays. The existing Mini LED backlight modules still need to be improved in terms of light uniformity and eye protection.

[0004] In the Mini LED backlight module, Mini LED chips can theoretically produce a more uniform light distribution due to their small size and high-density arrangement. However, when the diffusion film is too close to the chip, its diffusion effect is weakened, which may cause the local light intensity to be too high, forming a "light spot" or "hot spot". This uneven light distribution will directly affect the user's visual comfort, and long-term viewing may cause eye fatigue; and uneven light distribution not only affects the viewing experience, but may also cause additional pressure on the eyes. The eyes need to constantly adjust the focal length and pupil size to adapt to changes in light, which will increase the burden on the visual system, and in the long run may lead to decreased vision or other eye problems.

[0005] Therefore, it is necessary to provide a healthy and eye-protecting Mini LED backlight module and a manufacturing method. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the present invention provides a healthy eye protection Mini LED backlight module and a manufacturing method. By preparing a backlight plate with high light transmittance, high haze and good light diffusion, a backlight module with obvious diffusion effect and good light uniformity can be obtained. The backlight module has a good healthy eye protection effect.

[0007] The technical solution adopted by the present invention to solve its technical problem is:

[0008] The first purpose of the present application is to provide a healthy and eye-protecting Mini LED backlight module, including a Mini LED light board and a diffusion plate arranged above the Mini LED light board, the diffusion plate including a substrate and a coating coated on both sides of the substrate; the substrate is a PET film; the coating is a coating containing modified hollow mesoporous silica.

[0009] In some embodiments, the pore size of the modified hollow mesoporous silica is 1-15 nm; the thickness of the PET film is 50-80 μm; and the thickness of the coating is 10-15 μm.

[0010] In some embodiments, the coating solution for forming the coating layer comprises the following raw materials in parts by weight:

[0011] 20-30 parts of light diffuser, 10-20 parts of modified hollow mesoporous silica, 0.5-0.8 parts of photoinitiator, 20-30 parts of diluent, 10-20 parts of polyurethane acrylate, and 5-8 parts of grafting agent.

[0012] In some embodiments, the photoinitiator is any one of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 4-methylphenylvinyldiphenyliodonium salt.

[0013] In some embodiments, the diluent is tripropylene glycol diacrylate.

[0014] In some embodiments, the grafting agent is any one of hydroxyethyl methacrylate and glycidyl methacrylate.

[0015] In some embodiments, the method for preparing the modified hollow mesoporous silica comprises the following steps:

[0016] Take 1g of nano-silica, add it to 90mL of water for dispersion, then add 20ml of 10-15mg / ml hexadecyltrimethylammonium bromide ethanol solution, stir at room temperature for 2-3h, add 5-6g of anhydrous sodium carbonate, stir at 35°C for 12h, then heat to 50°C, stir for another 24h, after the reaction is completed, post-treat to obtain hollow mesoporous nano-silica;

[0017] Take 0.5 g of hollow mesoporous nano-silica and 1 g of a coupling agent, mix them thoroughly, and stir them at room temperature for 24-36 hours to obtain modified hollow mesoporous silica.

[0018] In some embodiments, the coupling agent is any one of γ-methacryloxypropyltrimethoxysilane and aminopropyltriethoxysilane.

[0019] In some embodiments, the method for preparing the light diffuser comprises the following steps: fully mixing epoxy acrylate, allyl diglycol dicarbonate and a curing agent, and performing a curing reaction to obtain the light diffuser.

[0020] The second object of the present application is to provide a method for manufacturing the Mini LED backlight module, comprising the following steps:

[0021] S1. Preparation of diffusion plate

[0022] Prepare materials according to the weight composition of the coating liquid for forming the coating; mix and stir the photoinitiator, diluent, polyurethane acrylate, and grafting agent evenly under light-free conditions, and then add a light diffuser and modified hollow mesoporous silica to obtain a coating liquid;

[0023] The coating liquid is evenly applied on a PET film, and then cured under a 100W ultraviolet lamp for 10-15 minutes to form a film, and after being taken out, the other side of the PET film is also cured to form a film, thereby preparing a light diffusion film;

[0024] S2. Assemble the backlight module

[0025] The display screen, prism film, diffusion plate, LED lamp and reflective film are assembled from top to bottom to produce a backlight module.

[0026] The beneficial effects of this application are:

[0027] 1. The backlight module described in the present application is prepared by preparing a backlight plate with high light transmittance, high haze and good light diffusion. The backlight plate can provide more uniform light distribution, reduce "light spots" or "hot spots" caused by excessive local light intensity, thereby reducing eye fatigue and pressure caused by long-term viewing of the display screen, and has a better healthy eye protection effect.

[0028] 2. The backlight module described in the present application has a diffusion plate that exhibits good resistance to UV aging, which helps to increase the service life of the backlight module. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0030] Figure 1 This is a schematic diagram of the structure of the backlight module described in this application;

[0031] Among them: 1. Display screen; 2. Prism film; 3. Diffuser plate; 4. LED light; 5. Reflective film. DETAILED DESCRIPTION

[0032] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.

[0033] As used herein, "and / or" includes the term of any and all combinations of one or more associated listed items. The terms used herein are only used to describe specific embodiments and are not intended to limit the present invention. As used herein, the singular forms "a", "an", "an" and "the" are also intended to include the plural forms, unless the context clearly indicates otherwise. It is further understood that "including", when used in this specification, specifies the stated features, integers, steps, operations, elements and / or compositions, but does not exclude the existence or addition of one or more other features, integers, steps, operations, elements, compositions and / or combinations thereof.

[0034] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. It is further understood that terms, such as defined in commonly used dictionaries, are interpreted in accordance with their meanings in the context of the relevant art and are not in an idealized or overly formal sense unless explicitly so defined herein.

[0035] The exemplary invention described herein may appropriately lack any one or more element limitations that are not specifically disclosed herein. Therefore, the terms "comprise", "include", "contain", etc. should be understood broadly and non-restrictively. In addition, the terminology used herein is used as a description, not a limitation, and it is unintentional to use these terminology expressions that do not include any equivalent characteristics, but only describe some of their characteristics, but various modifications are possible within the scope of the present invention according to the rights. Therefore, although the present invention has been specifically disclosed by preferred embodiments and optional features, the modifications disclosed herein to embody the changes of the present invention may be recorded by those skilled in the art, and such modifications and changes will be considered to be within the scope of the present invention.

[0036] The raw materials or reagents used in the embodiments of the present invention and the comparative examples are all purchased from mainstream manufacturers in the market. The manufacturer or concentration is not specified, and they are all analytically pure raw materials or reagents that can be routinely obtained. As long as the expected effect can be achieved, there is no particular restriction. The instruments and equipment used in the present embodiment are all purchased from major manufacturers in the market. As long as the expected effect can be achieved, there is no particular restriction. If specific techniques or conditions are not specified in the present embodiment, the techniques or conditions described in the literature in this area or according to the product specification are carried out.

[0037] Terminology explanation:

[0038] Display screen, the display screen is the key part of the display device, responsible for converting electrical signals or digital signals into visible images. In the backlight module, the display screen (such as LCD liquid crystal display screen) does not emit light itself, but relies on the light provided by the backlight module to display images. Working process: When the electrical signal is input to the display screen, the liquid crystal molecules will adjust their arrangement according to the signal, thereby allowing or blocking the light emitted by the backlight module to pass through and form an image.

[0039] Prism film is an optical film that is mainly used to enhance the directionality of light and improve brightness. Working process: In the backlight module, the prism film is usually placed on the diffusion film to further converge the diffused light and direct it to the display screen to improve the brightness and contrast of the picture.

[0040] The diffuser is located above the LED lamp. When the light from the LED lamp hits the diffuser, the tiny particles or structures in the coating will scatter the light in all directions, thereby enhancing the uniformity and softness of the light. At the same time, the diffuser can also play a certain role in heat insulation and protection, reducing the impact of the heat generated by the LED lamp on surrounding components.

[0041] LED lamp, LED (light emitting diode) is a semiconductor device that can convert electrical energy into light energy, with the advantages of high efficiency, energy saving, and environmental protection. In the backlight module, LED lamp is used as a light source to provide lighting. Working process: When current passes through the PN junction of the LED chip, electrons and holes recombine to release energy and emit light in the form of photons. In the Mini LED backlight module, multiple Mini LED chips are densely arranged to emit light together, and are diffused and homogenized through components such as diffusion films.

[0042] The reflective film is usually located at the bottom of the backlight module, close to the LED light board. It is used to reflect the part of the light emitted by the LED lamp that is not directly used back upward, so that it can be diffused and uniformed again through components such as the diffuser plate, and finally irradiate the display screen.

[0043] Polyurethane acrylate 5320, analytical grade, was obtained from Jiangmen Hengguang New Materials Co., Ltd.

[0044] Traditional Mini LED backlight modules may have the problem of uneven light distribution, resulting in excessive local light intensity, affecting visual comfort; when the backlight module needs to be exposed or work for a long time, the diffusion plate may age, affecting the performance and life of the backlight module. In order to solve the above problems, this application provides the following Figure 1The healthy eye-protecting Mini LED backlight module shown includes a Mini LED light board and a diffusion plate 3 arranged above the Mini LED light board, wherein the diffusion plate 3 includes a substrate and a coating coated on both sides of the substrate; the substrate is a PET film; and the coating is a coating containing modified hollow mesoporous silica.

[0045] Specifically, the Mini LED backlight module is provided with a display screen 1, a prism film 2, a diffusion plate 3, an LED lamp 4, and a reflective film 5 assembled together from top to bottom.

[0046] In some embodiments, the coating solution for forming the coating layer comprises the following raw materials in parts by weight:

[0047] 20-30 parts of light diffuser, 10-20 parts of modified hollow mesoporous silica, 0.5-0.8 parts of photoinitiator, 20-30 parts of diluent, 10-20 parts of polyurethane acrylate, and 5-8 parts of grafting agent.

[0048] The pore size of the modified hollow mesoporous silica is 1-15 nm; the photoinitiator is any one of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 4-methylstyryl diphenyl iodonium salt; the diluent is tripropylene glycol diacrylate; and the grafting agent is any one of hydroxyethyl methacrylate and glycidyl methacrylate.

[0049] Specifically, the weight of the light diffuser is 20-30 parts, for example, the weight of the light diffuser is any value among 20 parts, 21 parts, 23 parts, 25 parts, 26 parts, 28 parts, and 30 parts, within the range of 20-30 parts (including the endpoint values).

[0050] Specifically, the weight of the modified hollow mesoporous silica is 10-20 parts, for example, the weight of the modified hollow mesoporous silica is any value among 10 parts, 11 parts, 13 parts, 15 parts, 16 parts, 18 parts, and 20 parts, within 10-20 parts (including the endpoint values).

[0051] Specifically, the weight portion of the photoinitiator is 0.5-0.8 parts, for example, the weight portion of the photoinitiator is any value among 0.5 parts, 0.6 parts, 0.7 parts, and 0.8 parts, and it is within the range of 0.5-0.8 parts (including the endpoint values).

[0052] Specifically, the weight of the diluent is 20-30 parts, for example, the weight of the diluent is any value among 20 parts, 21 parts, 23 parts, 25 parts, 26 parts, 28 parts, and 30 parts, within the range of 20-30 parts (including the endpoint values).

[0053] Specifically, the weight of polyurethane acrylate is 10-20 parts, for example, the weight of polyurethane acrylate is any value among 10 parts, 11 parts, 13 parts, 15 parts, 16 parts, 18 parts, and 20 parts, within the range of 10-20 parts (including the endpoint values).

[0054] Specifically, the weight of the grafting agent is 5-8 parts, for example, the weight of the grafting agent is any value among 20 parts, 21 parts, 23 parts, 25 parts, 26 parts, 28 parts, and 30 parts, within the range of 5-8 parts (including the endpoint values).

[0055] Specifically, the weight of the light diffusing agent is 20-30 parts, for example, the weight of the light diffusing agent is any value among 5 parts, 6 parts, 7 parts, and 8 parts, within the range of 20-30 parts (including the endpoint values).

[0056] In the present application, the addition of grafting agents such as hydroxyethyl methacrylate and glycidyl methacrylate helps to improve the overall transparency of the coating, thereby maintaining a high light transmittance. The grafting agent can form a stable cross-linked structure during the curing process of the coating, reduce light scattering, and help light to pass through. At the same time, the grafting agent can improve the interfacial bonding between the coating and the PET film substrate, making the coating more firmly attached to the PET film. The grafting agent prevents the coating from falling off or peeling off during use, thereby improving the overall durability and stability of the backlight module.

[0057] In this application, the modified hollow mesoporous silica (pore size of 1-15nm) can significantly increase the haze of the coating while ensuring a certain transmittance due to its unique mesoporous structure and surface modification. These tiny hole structures can effectively scatter light, making the light more evenly distributed, avoiding "light spots" or "hot spots" caused by excessive local light intensity; the hollow mesoporous structure enables the silica particles to scatter light more effectively, and has better light diffusion performance than traditional solid particles. In addition, surface modification (such as the use of γ-methacryloxypropyltrimethoxysilane and aminopropyltriethoxysilane) enhances the compatibility of silica with the coating, further improving the light diffusion effect.

[0058] In the present application, the light diffuser can form multiple tiny scattering centers in the coating, which can effectively disperse the light so that the light is evenly distributed in the backlight module. The addition of the light diffuser significantly improves the light diffusion effect of the backlight module and reduces the local concentration of light.

[0059] In some embodiments, the method for preparing the modified hollow mesoporous silica comprises the following steps:

[0060] Take 1g of nano-silica, add it to 90mL of water for dispersion, then add 20ml of 10-15mg / ml hexadecyltrimethylammonium bromide ethanol solution, stir at room temperature for 2-3h, add 5-6g of anhydrous sodium carbonate, stir at 35°C for 12h, then heat to 50°C, stir for another 24h, after the reaction is completed, post-treat to obtain hollow mesoporous nano-silica;

[0061] 0.5 g of hollow mesoporous nano-silica and 1 g of a coupling agent are mixed thoroughly and stirred at room temperature for 24-36 hours to obtain modified hollow mesoporous silica. The coupling agent is any one of γ-methacryloxypropyltrimethoxysilane and aminopropyltriethoxysilane.

[0062] Specifically, hexadecyltrimethylammonium bromide is added to the nano-silicon dioxide dispersion as a template to help form a hollow mesoporous structure.

[0063] The prepared hollow mesoporous nano-silica has a large specific surface area and pore volume, which makes them have excellent scattering properties in light diffusers, which helps to improve the light uniformity of the backlight module; the hollow mesoporous structure can effectively scatter light and reduce the direct penetration of light, thereby improving the light diffusion effect of the backlight module and avoiding "light spots" or "hot spots" caused by excessive local light intensity; the hollow mesoporous nano-silica has better chemical stability, which helps to improve the service life of the backlight module.

[0064] In some embodiments, the method for preparing the light diffuser comprises the following steps: fully mixing epoxy acrylate, allyl diglycol dicarbonate and a curing agent, and performing a curing reaction to obtain the light diffuser.

[0065] Specifically, the preparation method of the light diffuser includes the following steps: 1g of epoxy acrylate, 6g of allyl diglycol dicarbonate and 0.1g of benzoyl peroxide curing agent are fully mixed, and a curing reaction is carried out at 60 for 2h, and then cooled to room temperature to obtain a light diffuser.

[0066] In the present application, the light diffuser is a microsphere mother solution, epoxy acrylate (epoxy acrylate) is used as a reactive component, triethylenetetramine (triethylenetetramine) is used as a curing agent, and allyl diglycol dicarbonate (allyl diglycol dicarbonate) is used as a solvent phase. As the curing reaction begins, a chemical reaction occurs between epoxy acrylate and triethylenetetramine, resulting in changes in the chemical and physical properties of the system. The curing reaction causes the network structure formed by epoxy acrylate and triethylenetetramine to be incompatible with allyl diglycol dicarbonate, thereby inducing phase separation;

[0067] The phase separation process can follow two mechanisms: spinodal separation (SD) and nucleation and growth (NG). When the mass ratio of allyl diglycol dicarbonate to epoxy acrylate is 6:1 or below, the phase separation follows the SD mechanism to form a micro-bicontinuous phase structure, and then the bicontinuous phase breaks to form dispersed microspheres.

[0068] When the mass ratio of allyl diglycol dicarbonate to epoxy acrylate is 8:1 or above, the phase separation follows the NG mechanism, and the primary nucleus gradually grows and disperses in the solvent phase to form microspheres. Therefore, through the above preparation method, a diffusing agent of a microsphere mother solution is prepared, which is added to the coating liquid to form multiple tiny scattering centers in the coating and prevent the coating liquid from agglomerating.

[0069] A method for manufacturing the above-mentioned Mini LED backlight module is provided, comprising the following steps:

[0070] S1. Preparation of diffusion plate

[0071] Prepare materials according to the weight composition of the coating liquid for forming the coating; mix and stir the photoinitiator, diluent, polyurethane acrylate, and grafting agent evenly under light-free conditions, and then add a light diffuser and modified hollow mesoporous silica to obtain a coating liquid;

[0072] The coating liquid is evenly applied on a PET film, and then cured under a 100W ultraviolet lamp for 10-15 minutes to form a film, and after being taken out, the other side of the PET film is also cured to form a film, thereby preparing a light diffusion film;

[0073] S2. Assemble the backlight module

[0074] The display screen, prism film, diffusion plate, LED lamp and reflective film are assembled from top to bottom to produce a backlight module.

[0075] The specific assembly and matching method can be carried out in the same way as the conventional mini LED backlight module.

[0076] The backlight module and the diffuser plate described in the present application are further described through the following preparation examples, embodiments and comparative examples.

[0077] Preparation Example 1

[0078] The preparation method of hollow mesoporous nano-silica comprises the following steps:

[0079] 10 ml of tetraethoxysilane was quickly added to a mixture of 100 ml of ethanol, 15 ml of deionized water and 4 ml of ammonia solution (25%), and then stirred for 12 hours, centrifuged to obtain a separated solid, and then the separated solid was washed with deionized water and ethanol, and dried at 150° C. for 10 hours to obtain nano-silica.

[0080] Take 1g of nano-silica, add it to 90mL of water to disperse, then add 20ml of 10mg / ml hexadecyltrimethylammonium bromide ethanol solution, stir at room temperature for 2h, add 5g of anhydrous sodium carbonate, stir at 35℃ for 12h, then heat to 50℃, and stir for another 24h. After the reaction is completed, centrifuge, wash the separated solid with deionized water and ethanol, and dry at 120℃ for 12h to obtain hollow mesoporous nano-silica.

[0081] Preparation Example 2

[0082] The preparation method of the light diffuser comprises the following steps: 1g of epoxy acrylate, 6g of allyl diglycol dicarbonate and 0.1g of benzoyl peroxide curing agent are fully mixed, a curing reaction is carried out at 60°C for 2h, and the temperature is cooled to room temperature to obtain the light diffuser.

[0083] The reaction processes involved are:

[0084]

[0085] Example 1

[0086] The method for manufacturing a diffusion plate comprises the following steps:

[0087] Prepare materials according to the weight composition of the coating liquid for forming a coating; 0.5 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 20 parts of tripropylene glycol diacrylate, 10 parts of polyurethane acrylate, and 5 parts of hydroxyethyl methacrylate are mixed and stirred evenly under lightless conditions; then 20 parts of a light diffusing agent (Preparation Example 2) and 10 parts of modified hollow mesoporous silica are added and mixed thoroughly to obtain a coating liquid;

[0088] The coating liquid is evenly applied on the PET film, and then cured under a 100W ultraviolet lamp for 10 minutes to form a film. After being taken out, the other side of the PET film is also cured to form a film, thereby preparing a light diffusion film; the thickness of the PET film is controlled at 50μm, and after the coating liquid on one side is cured, the thickness is 10-11μm.

[0089] The method for preparing the modified hollow mesoporous silica comprises the following steps:

[0090] Take 0.5 g of hollow mesoporous nano-silica (Preparation Example 1), add it to 50 ml of anhydrous ethanol, ultrasonically disperse it for 30 minutes, add 1 g of γ-methacryloxypropyltrimethoxysilane and mix it thoroughly, stir it at room temperature for 24 hours, centrifuge it, wash the separated solid with deionized water and ethanol, and dry it at 80°C for 20 hours to obtain hollow mesoporous nano-silica.

[0091] Example 2

[0092] The method for manufacturing a diffusion plate comprises the following steps:

[0093] Prepare materials according to the weight composition of the coating liquid for forming a coating; 0.8 parts of 4-methylstyryl diphenyl iodonium salt, 30 parts of tripropylene glycol diacrylate, 20 parts of polyurethane acrylate, and 8 parts of glycidyl methacrylate are mixed and stirred evenly under lightless conditions; then 30 parts of a light diffusing agent (Preparation Example 2) and 20 parts of modified hollow mesoporous silica are added and mixed thoroughly to obtain a coating liquid;

[0094] The coating liquid is evenly applied on the PET film, and then cured under a 100W ultraviolet lamp for 15 minutes to form a film. After being taken out, the other side of the PET film is also cured to form a film, thereby preparing a light diffusion film; the thickness of the PET film is controlled at 50μm, and after the coating liquid on one side is cured, the thickness is 10-11μm.

[0095] The method for preparing the modified hollow mesoporous silica comprises the following steps:

[0096] Take 0.5g of hollow mesoporous nano-silica (Preparation Example 1), add it to 50ml of anhydrous ethanol, ultrasonically disperse it for 30min, add 1g of aminopropyltriethoxysilane and mix it thoroughly, stir it at room temperature for 36h, centrifuge it, wash the separated solid with deionized water and ethanol, and dry it at 80°C for 20h to obtain hollow mesoporous nano-silica.

[0097] Example 3

[0098] The method for manufacturing a diffusion plate comprises the following steps:

[0099] Prepare materials according to the weight composition of the coating liquid for forming a coating; 0.6 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 25 parts of tripropylene glycol diacrylate, 15 parts of polyurethane acrylate, and 7 parts of glycidyl methacrylate are mixed and stirred evenly under lightless conditions; then 25 parts of a light diffusing agent (Preparation Example 2) and 15 parts of modified hollow mesoporous silica are added and mixed thoroughly to obtain a coating liquid;

[0100] The coating liquid is evenly applied on the PET film, and then cured under a 100W ultraviolet lamp for 13 minutes to form a film. After being taken out, the other side of the PET film is also cured to form a film, thereby preparing a light diffusion film; the thickness of the PET film is controlled at 50μm, and after the coating liquid on one side is cured, the thickness is 10-11μm.

[0101] The method for preparing the modified hollow mesoporous silica comprises the following steps:

[0102] Take 0.5 g of hollow mesoporous nano-silica (Preparation Example 1), add it to 50 ml of anhydrous ethanol, ultrasonically disperse it for 30 minutes, add 1 g of aminopropyltriethoxysilane and mix it thoroughly, stir it at room temperature for 30 hours, centrifuge it, wash the separated solid with deionized water and ethanol, and dry it at 80°C for 20 hours to obtain hollow mesoporous nano-silica.

[0103] Example 4

[0104] The method for manufacturing a diffusion plate comprises the following steps:

[0105] Prepare materials according to the weight composition of the coating liquid for forming a coating; 0.6 parts of 4-methylstyryl diphenyl iodonium salt, 22 parts of tripropylene glycol diacrylate, 12 parts of polyurethane acrylate, and 6 parts of hydroxyethyl methacrylate are mixed and stirred evenly under lightless conditions; then 21 parts of a light diffusing agent (Preparation Example 2) and 12 parts of modified hollow mesoporous silica are added and mixed thoroughly to obtain a coating liquid;

[0106] The coating liquid is evenly applied on the PET film, and then cured under a 100W ultraviolet lamp for 11 minutes to form a film. After being taken out, the other side of the PET film is also cured to form a film, thereby preparing a light diffusion film; the thickness of the PET film is controlled at 50μm, and after the coating liquid on one side is cured, the thickness is 10-11μm.

[0107] The method for preparing the modified hollow mesoporous silica comprises the following steps:

[0108] Take 0.5g of hollow mesoporous nano-silica (Preparation Example 1), add it to 50ml of anhydrous ethanol, ultrasonically disperse it for 30min, add 1g of aminopropyltriethoxysilane and mix it thoroughly, stir it at room temperature for 26h, centrifuge it, wash the separated solid with deionized water and ethanol, and dry it at 80°C for 20h to obtain hollow mesoporous nano-silica.

[0109] Example 5

[0110] The method for manufacturing a diffusion plate comprises the following steps:

[0111] Prepare materials according to the weight composition of the coating liquid for forming a coating; 0.7 parts of 4-methylstyryl diphenyl iodonium salt, 29 parts of tripropylene glycol diacrylate, 18 parts of polyurethane acrylate, and 7 parts of glycidyl methacrylate are mixed and stirred evenly under lightless conditions; then 28 parts of a light diffusing agent (Preparation Example 2) and 18 parts of modified hollow mesoporous silica are added and mixed thoroughly to obtain a coating liquid;

[0112] The coating liquid is evenly applied on the PET film, and then cured under a 100W ultraviolet lamp for 14 minutes to form a film. After being taken out, the other side of the PET film is also cured to form a film, thereby preparing a light diffusion film; the thickness of the PET film is controlled at 50μm, and after the coating liquid on one side is cured, the thickness is 10-11μm.

[0113] The method for preparing the modified hollow mesoporous silica comprises the following steps:

[0114] Take 0.5 g of hollow mesoporous nano-silica (Preparation Example 1), add it to 50 ml of anhydrous ethanol, ultrasonically disperse it for 30 minutes, add 1 g of γ-methacryloxypropyltrimethoxysilane and mix it thoroughly, stir it at room temperature for 33 hours, centrifuge it, wash the separated solid with deionized water and ethanol, and dry it at 80°C for 20 hours to obtain hollow mesoporous nano-silica.

[0115] Comparative Example 1

[0116] The method for manufacturing a diffusion plate comprises the following steps: no grafting agent is added to the coating liquid, and the other conditions are the same as those in Example 1.

[0117] Comparative Example 2

[0118] The method for manufacturing a diffusion plate comprises the following steps: no modified hollow mesoporous nano-silica is added to the coating liquid, and the other conditions are the same as those in Example 1.

[0119] Comparative Example 3

[0120] The method for manufacturing a diffusion plate comprises the following steps: no light diffusing agent is added to the coating liquid, and the other conditions are the same as those in Example 1.

[0121] The diffuser plates prepared in the above Examples 1-5 and Comparative Examples 1-3 were subjected to the following performance tests, and the test results are summarized in Table 2;

[0122] Light transmittance and haze: Sampling is carried out according to 4.2 of GB / T 2410-2008 "Determination of light transmittance and haze of transparent plastics", and the light transmittance and haze of the light diffusion film are tested using the spectrophotometer method in 7.2 Method B;

[0123] UV aging test chamber test: aging time is 0 to 240 hours, sampling and observation are performed every 24 hours; a colorimeter is used to test the change in the color difference value (ΔE) of the film material during the aging process, and it is evaluated according to the color change degree and color change grade evaluation standards specified in GB / T 1766-1995 (Table 1);

[0124] Table 1

[0125] Color change level Color difference value (△E) Discoloration degree 0 ≤1.5 No discoloration 1 1.6~3.0 Very slight discoloration 2 3.1~6.0 Slight discoloration 3 6.1~9.0 Obvious discoloration 4 9.1~12.0 Larger discoloration 5 >12.0 Severe discoloration

[0126] Light uniformity test: Use a color analyzer to perform uniformity index test; the uniformity index indicates the consistency of color distribution. The lower the value, the more uniform the color distribution.

[0127] Table 2

[0128]

[0129]

[0130] As can be seen from Table 2, the diffusers prepared in Examples 1-5 of the present application have a transmittance of more than 90%, which indicates that these diffusers have high light transmittance, which is conducive to maintaining the brightness and clarity of the display device; the diffusers prepared in Examples 1-5 of the present application have a haze of more than 90%, indicating that the coating design effectively improves the scattering effect of light; the diffusers prepared in Examples 1-5 of the present application have a uniformity index of less than 1.0, showing very excellent light uniformity. The diffusers prepared in Examples 1-5 of the present application show "no discoloration", indicating that these diffusers have excellent aging resistance.

[0131] The diffuser plate of Comparative Example 1, in the absence of a grafting agent, obviously changes color in an aging test, and the diffuser plate, haze, and light uniformity of the diffuser plate decrease.

[0132] The diffuser plate of Comparative Example 2 has a significantly reduced light transmittance in the absence of the modified hollow mesoporous nano-silica.

[0133] The diffuser plate, light diffuser, haze and light uniformity of Comparative Example 3 were significantly reduced.

[0134] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A healthy eye protection Mini LED backlight module, comprising a Mini LED light board and a diffusion plate arranged above the Mini LED light board, characterized in that: The diffusion plate comprises a substrate and a coating layer coated on both sides of the substrate; the substrate is a PET film; and the coating layer is a coating layer containing modified hollow mesoporous silica.

2. The Mini LED backlight module according to claim 1, characterized in that: The pore size of the modified hollow mesoporous silica is 1-15 nm; the thickness of the PET film is 50-80 μm; and the thickness of the coating is 10-15 μm.

3. The Mini LED backlight module according to claim 1 or 2, characterized in that: The coating liquid for forming the coating layer comprises the following raw materials in parts by weight: 20-30 parts of light diffuser, 10-20 parts of modified hollow mesoporous silica, 0.5-0.8 parts of photoinitiator, 20-30 parts of diluent, 10-20 parts of polyurethane acrylate, and 5-8 parts of grafting agent.

4. The Mini LED backlight module according to claim 3, characterized in that: The photoinitiator is any one of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 4-methylphenylvinyl diphenyl iodonium salt.

5. The Mini LED backlight module according to claim 3, characterized in that: The diluent is tripropylene glycol diacrylate.

6. The Mini LED backlight module according to claim 3, characterized in that: The grafting agent is any one of hydroxyethyl methacrylate and glycidyl methacrylate.

7. The Mini LED backlight module according to claim 1, characterized in that: The preparation method of the modified hollow mesoporous silica comprises the following steps: Take 1g of nano-silica, add it to 90mL of water for dispersion, then add 20ml of 10-15mg / ml hexadecyltrimethylammonium bromide ethanol solution, stir at room temperature for 2-3h, add 5-6g of anhydrous sodium carbonate, stir at 35°C for 12h, then heat to 50°C, stir for another 24h, after the reaction is completed, post-treat to obtain hollow mesoporous nano-silica; Take 0.5 g of hollow mesoporous nano-silica and 1 g of a coupling agent, mix them thoroughly, and stir them at room temperature for 24-36 hours to obtain modified hollow mesoporous silica.

8. The Mini LED backlight module according to claim 7, characterized in that: The coupling agent is any one of γ-methacryloxypropyltrimethoxysilane and aminopropyltriethoxysilane.

9. The Mini LED backlight module according to claim 3, characterized in that: The preparation method of the light diffuser comprises the following steps: fully mixing epoxy acrylate, allyl diglycol dicarbonate and a curing agent, and performing a curing reaction to obtain the light diffuser.

10. The method for manufacturing a Mini LED backlight module according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Preparation of diffusion plate Prepare materials according to the weight composition of the coating liquid for forming the coating; mix and stir the photoinitiator, diluent, polyurethane acrylate, and grafting agent evenly under light-free conditions, and then add a light diffuser and modified hollow mesoporous silica to obtain a coating liquid; The coating liquid is evenly applied on a PET film, and then cured under a 100W ultraviolet lamp for 10-15 minutes to form a film, and after being taken out, the other side of the PET film is also cured to form a film, thereby preparing a light diffusion film; S2. Assemble the backlight module The display screen, prism film, diffusion plate, LED lamp and reflective film are assembled from top to bottom to produce a backlight module.

Citation Information

Patent Citations

  • Method for preparing ordered mesoporous hollow silica spheres

    CN102153094A

  • Preparation method of light diffusion film

    CN112433279A

  • Composition, film, display panel and display device

    CN118271831A

  • Minled direct type glass diffusion plate capable of improving edge brightness

    CN220691122U

  • Mesoporous silica nanoparticle dispersion solution, manufacturing method therefor, coating liquid, and mesoporous silica film