Method for improving plastic deformation performance and current-carrying capacity of Bi2212 wire rod through low oxygen partial pressure post-heat treatment

Through low oxygen partial pressure post-heat treatment and drawing treatment, the lattice structure and deformation performance of Bi2212 wire is optimized, which solves the problem of insufficient current carrying performance of Bi2212 superconducting wire, which significantly improves its plastic deformation and current carrying performance. It is suitable for Application of high-performance superconducting magnets.

CN118969392APending Publication Date: 2024-11-15NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411038865.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the processing process, the current-carrying performance of Bi2212 superconducting wire is limited due to uneven deformation of the core wire, and the prior art is difficult to effectively improve its plastic deformation performance and current-carrying capacity.

Method used

By preparing Bi2212 precursor powder and performing preliminary sintering, followed by heat treatment after low oxygen partial pressure, optimizing the lattice structure, forming a composite blank for drawing treatment, and finally preparing Bi2212 wire with excellent plastic deformation performance and current carrying capacity.

Benefits of technology

It significantly improves the plastic deformation performance and current carrying capacity of Bi2212 wire, reduces the sliding resistance between grains, increases the contact area of ​​the silver superinterface, improves the interface combination quality, improves the superconducting performance and reduces hysteresis loss. Suitable for long-term and stable operation of large magnets.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for improving plastic deformation performance and current-carrying capacity of a Bi2212 wire rod through low oxygen partial pressure post-heat treatment. The method comprises the following steps: 1, preparing Bi2212 precursor powder; 2, primarily sintering the Bi2212 precursor powder; 3, performing low oxygen partial pressure post-heat treatment on the primarily sintered powder; 4, filling the powder subjected to low oxygen partial pressure and heat treatment into a silver tube; 5, the composite blank is subjected to drawing treatment; and 6, finally sintering the composite wire rod to obtain the Bi2212 wire rod with excellent plastic deformation performance and excellent current-carrying capacity. According to the preparation method, a Bi2212 lattice structure is optimized through heat treatment after low oxygen partial pressure, the sliding resistance between crystal grains is reduced, the plastic deformation performance of a core wire is improved, the current-carrying capacity and heat stability of the Bi2212 wire are improved, the Bi2212 wire texture is improved, superconducting crystal grains are arranged more orderly, the superconducting performance of the Bi2212 wire is improved, and magnetic hysteresis loss is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of Bi2212 high temperature superconducting wire preparation, and specifically relates to a method for improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment. Background Art

[0002] In the field of superconducting technology, Bi2212 (Bi2Sr2CaCu2O8) wire has always been the focus of research and application due to its excellent superconducting properties. However, the processing performance of this type of wire is significantly restricted by the inherent characteristics of the high-temperature superconducting ceramic powder inside it. These ceramic powders are carefully encapsulated in a metal sheath to form a composite wire structure to maximize superconducting performance. However, in the actual processing process, the deformation uniformity of the core wire (i.e., the high-temperature superconducting ceramic powder) becomes a key factor affecting the current-carrying performance of the wire.

[0003] The importance of core wire deformation uniformity is self-evident. Due to the inherent high hardness and low plasticity of ceramic powder, its deformation behavior in the metal sheath is difficult to accurately control, and local deformation is often too large or too small. This deformation unevenness will lead to an imbalance in the stress distribution inside the wire, which will in turn have an adverse effect on the microstructure and superconducting properties of the superconducting wire. Specifically, uneven deformation may induce defects such as fracture, interface delamination or microcracks in the superconducting wire, which will significantly reduce the current-carrying capacity of the wire and restrict its application in fields such as high-performance superconducting magnets.

[0004] Although the processing performance of Bi2212 superconducting wires has been improved to a certain extent by optimizing processing technology, improving metal sheath materials and structural design, these traditional methods are still insufficient in the face of growing performance requirements. Therefore, the development of new processing technologies, especially optimization technologies for the uniformity of core wire deformation, has become the key to promoting the performance improvement of Bi2212 superconducting wires. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment in view of the deficiencies of the above-mentioned prior art. The present invention first prepares Bi2212 precursor powder, and then performs preliminary sintering to lay the foundation for subsequent processing. Through low oxygen partial pressure post-heat treatment, the Bi2212 lattice structure is optimized, and the plastic deformation performance and superconducting performance are significantly enhanced. The low oxygen partial pressure post-heat treatment powder is loaded into a silver tube to form a composite blank composed of Ag and low oxygen partial pressure post-heat treatment powder, in preparation for the drawing of the wire, and the composite blank is drawn into a composite wire through a drawing process, and finally sintered to obtain a Bi2212 wire with excellent plastic deformation performance and excellent current carrying capacity.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment, characterized in that the method comprises the following steps:

[0007] Step 1, preparing Bi2212 precursor powder;

[0008] Step 2: Preliminarily sintering the Bi2212 precursor powder prepared in step 1 to obtain a preliminary sintered powder;

[0009] Step 3: subjecting the preliminary sintered powder obtained in step 2 to low oxygen partial pressure post-heat treatment to obtain low oxygen partial pressure post-heat treatment powder; the oxygen partial pressure in the low oxygen partial pressure post-heat treatment is 10Pa-1000Pa, the temperature is 520°C-580°C, and the time is 6h-12h;

[0010] Step 4: putting the low oxygen partial pressure heat-treated powder obtained in step 3 into a silver tube to obtain a composite blank;

[0011] Step 5: Drawing the composite blank obtained in step 4 to obtain a composite wire;

[0012] Step 6: finally sintering the composite wire obtained in step 5 to obtain a Bi2212 wire with excellent plastic deformation performance and excellent current carrying capacity.

[0013] The present invention first prepares Bi2212 precursor powder, and then performs preliminary sintering to lay a foundation for subsequent processing. Through low oxygen partial pressure heat treatment, the Bi2212 lattice structure is optimized, the plastic deformation performance and superconducting performance are significantly enhanced, the low oxygen partial pressure heat treatment powder is loaded into a silver tube to form a composite blank composed of Ag and the low oxygen partial pressure heat treatment powder, in preparation for wire drawing, the composite blank is drawn into a composite wire through a drawing process, and finally sintering is performed to obtain a Bi2212 wire with excellent plastic deformation performance and excellent current carrying capacity.

[0014] The present invention optimizes the Bi2212 lattice structure through low oxygen partial pressure post-heat treatment, reduces the sliding resistance between grains, and makes it easier for the ceramic core wire formed by the Bi2212 precursor powder to form uniform deformation in the silver tube sheath. The optimization of the lattice structure and the reduction of defects such as oxygen vacancies greatly improve the plastic deformation performance of the ceramic core wire, making the composite blank easier to deform during processing, thereby preparing a thinner and more uniform Bi2212 wire. In addition, the refined core wire increases the contact area of ​​the silver superinterface, improves the interface bonding quality, reduces the interface resistance and thermal resistance, and improves the current carrying capacity and thermal stability of the Bi2212 wire. In addition, the texture of the Bi2212 wire is improved, the superconducting grains are arranged more orderly, the superconducting performance of the Bi2212 wire is improved, and the hysteresis loss is reduced, which is of great significance to the long-term stable operation of large magnets.

[0015] The present invention controls the parameters of the heat treatment after low oxygen partial pressure, thereby avoiding the problem that the superconducting transition temperature of the powder is tilted when the oxygen partial pressure is lower than 10Pa, preventing the superconducting powder from having a relatively obvious impurity phase, and avoiding the situation that when the oxygen partial pressure is higher than 1000Pa, the lattice constant c is less than 3.08, and this lattice structure is not conducive to the deformation of the ceramic superconducting core wire, and excessive oxygen can serve as an effective pinning center, resulting in dislocations not being easy to slip. However, when the oxygen partial pressure is 10Pa-1000Pa, the lattice constant c is greater than 3.08, and this lattice constant parameter is conducive to the plastic deformation of the ceramic superconducting core wire, and due to the reduction of oxygen content, the obstacle to dislocations becomes smaller, all of which are conducive to the slip of the powder.

[0016] The above-mentioned method for improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment is characterized in that the Bi2212 precursor powder in step 1 is prepared by coprecipitation, and the atomic ratio of Bi, Sr, Ca, Cu, and O in the Bi2212 precursor powder is 2.10:2.05:1.00:2.00:8. The present invention prepares Bi2212 precursor powder by coprecipitation, which is convenient, fast, and low-cost. By controlling the ratio of each element in the precursor powder, the performance of the Bi2212 wire is guaranteed.

[0017] The above-mentioned method for improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment is characterized in that the number of preliminary sintering in step 2 is two to four times, the temperature of the preliminary sintering is 840°C to 860°C, and the time is 9h to 11h. The present invention controls the parameters of the preliminary sintering to form the Bi2212 precursor powder.

[0018] The above-mentioned method for improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment is characterized in that the deformation rate of each pass in the drawing process described in step 5 is 8% to 12%. The present invention controls the deformation rate of each pass in the drawing process to ensure that the composite blank maintains excellent uniformity and stability during the drawing process, further enhances the plastic deformation capacity of the high-strength Bi2212 wire, and provides a solid foundation for its excellent current carrying performance.

[0019] The above-mentioned method for improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment is characterized in that the single-pass drawing force of the composite wire in step 5 is less than 280MPa, and the critical current density of the Bi2212 wire in step 6 is greater than 1350A / mm 2 The Bi2212 wire prepared by the present invention has excellent plastic deformation performance and current carrying capacity.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] 1. The present invention first prepares Bi2212 precursor powder, and then performs preliminary sintering to lay the foundation for subsequent processing. The Bi2212 lattice structure is optimized through low oxygen partial pressure heat treatment, and the plastic deformation performance and superconducting performance are significantly enhanced. The low oxygen partial pressure heat treatment powder is loaded into a silver tube to form a composite billet composed of Ag and low oxygen partial pressure heat treatment powder, in preparation for wire drawing. The composite billet is drawn into a composite wire through a drawing process, and finally sintered to obtain a Bi2212 wire with excellent plastic deformation performance and excellent current carrying capacity.

[0022] 2. The present invention directly optimizes the lattice structure of Bi2212 ceramic powder by controlling the parameters of heat treatment after low oxygen partial pressure, thereby significantly enhancing its slip performance. This innovative method not only greatly improves the plastic deformation ability of Bi2212 high-temperature superconducting wire, but also significantly enhances its current-carrying performance, providing a new way to prepare high-performance superconducting wire. In addition, the present invention has a simple process and is easy to realize industrial long-line preparation, providing important technical support for the preparation and application of Bi-based superconducting wires, and has a far-reaching impact on promoting the industrialization and wide application of Bi-based superconducting wires.

[0023] 3. The present invention optimizes the Bi2212 lattice structure through low oxygen partial pressure post-heat treatment, reduces the sliding resistance between grains, makes it easier for the ceramic core wire formed by the Bi2212 precursor powder to form uniform deformation in the silver tube sheath, greatly improves the plastic deformation performance of the ceramic core wire, and makes the composite blank easier to deform during the processing, thereby preparing a thinner and more uniform Bi2212 wire.

[0024] 4. The present invention refines the core wire through low oxygen partial pressure post-heat treatment, increases the contact area of ​​the silver superinterface, improves the interface bonding quality, reduces the interface resistance and thermal resistance, improves the current carrying capacity and thermal stability of the Bi2212 wire, and improves the texture of the Bi2212 wire, and the arrangement of superconducting grains is more orderly, which improves the superconducting performance of the Bi-based superconducting wire and reduces the hysteresis loss, which is of great significance to the long-term stable operation of large magnets.

[0025] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION

[0026] Example 1

[0027] This embodiment includes the following steps:

[0028] Step 1: Prepare Bi2212 precursor powder with an atomic ratio of Bi, Sr, Ca, Cu, and O of 2.10:2.05:1.00:2.00:8 by coprecipitation method;

[0029] Step 2: The Bi2212 precursor powder prepared in step 1 is preliminarily sintered three times at a temperature of 850° C. for 10 h to obtain a preliminarily sintered powder;

[0030] Step 3: subjecting the preliminary sintered powder obtained in step 2 to low oxygen partial pressure post-heat treatment to obtain low oxygen partial pressure post-heat treatment powder; the low oxygen partial pressure post-heat treatment has an oxygen partial pressure of 500 Pa, a temperature of 550° C., and a time of 10 h;

[0031] Step 4: putting the low oxygen partial pressure heat-treated powder obtained in step 3 into a silver tube to obtain a composite blank;

[0032] Step 5: Drawing the composite blank obtained in step 4 to obtain a composite wire; the deformation rate of each drawing process is 8% to 12%;

[0033] Step 6: finally sintering the composite wire obtained in step 5 to obtain a Bi2212 wire with excellent plastic deformation performance and excellent current carrying capacity.

[0034] After testing, the single-pass pulling force of the composite wire prepared in this embodiment is 251MPa, and the critical current density (Jc) of the prepared Bi2212 wire is 1700A / mm2 under 4.2K, 12T conditions. The superconducting core wire in the Bi2212 wire is uniformly deformed without breakage or peeling, and the fluctuation range of the uniformity of the superconducting core wire diameter is ±9.4%.

[0035] Comparative Example 1

[0036] This comparative example comprises the following steps:

[0037] Step 1: Prepare Bi2212 precursor powder with an atomic ratio of Bi, Sr, Ca, Cu, and O of 2.10:2.05:1.00:2.00:8 by coprecipitation method;

[0038] Step 2: The Bi2212 precursor powder prepared in step 1 is preliminarily sintered three times at a temperature of 850° C. for 10 h to obtain a preliminarily sintered powder;

[0039] Step 3, subjecting the preliminary sintered powder obtained in step 2 to low oxygen partial pressure post-heat treatment to obtain low oxygen partial pressure post-heat treatment powder; the oxygen partial pressure in the low oxygen partial pressure post-heat treatment is 10000 Pa, the temperature is 550° C., and the time is 10 h;

[0040] Step 4: putting the low oxygen partial pressure heat-treated powder obtained in step 3 into a silver tube to obtain a composite blank;

[0041] Step 5: Drawing the composite blank obtained in step 4 to obtain a composite wire; the deformation rate of each drawing process is 8% to 12%;

[0042] Step 6: finally sinter the composite wire obtained in step 5 to obtain Bi2212 wire.

[0043] After testing, the single-pass pulling force of the composite wire prepared in this comparative example is 305MPa, and the critical current density (Jc) of the prepared Bi2212 wire is 990A / mm2 under 4.2K, 12T conditions. The superconducting core wire in the Bi2212 wire is unevenly deformed, and breakage and peeling occur. The fluctuation range of the uniformity of the superconducting core wire diameter is ±22.6%.

[0044] By comparing Example 1 with Comparative Example 1, it can be seen that the low oxygen partial pressure post-heat treatment has significant advantages in improving the performance of Bi2212 superconducting wire. Specifically: ① The plastic deformation performance is significantly improved: The single-pass pulling force and deformation uniformity (core wire diameter uniformity) of the composite wire in Example 1 are better than those in Comparative Example 1, showing better plastic deformation ability, which is conducive to the preparation of thinner and more uniform high-strength Bi2212 wires; ② The current carrying performance is greatly improved: The critical current density (Jc) of the Bi2212 wire in Example 1 at 4.2K and 12T reaches 1700A / mm 2, which is about 70% higher than that of comparative example 1, indicating that its current carrying capacity is significantly improved; ③ Optimization of wire diameter uniformity: The diameter fluctuation range of the Bi2212 wire superconducting core wire in Example 1 is small, showing excellent uniformity, which is helpful to improve the overall performance and service life of the high-strength Bi2212 wire. The present invention significantly improves the plastic deformation performance, current carrying capacity, hysteresis loss and wire diameter uniformity of the high-strength Bi2212 wire through low oxygen partial pressure post-heat treatment technology, which provides strong support for the development and application of superconducting technology.

[0045] Example 2

[0046] This embodiment includes the following steps:

[0047] Step 1: Prepare Bi2212 precursor powder with an atomic ratio of Bi, Sr, Ca, Cu, and O of 2.10:2.05:1.00:2.00:8 by coprecipitation method;

[0048] Step 2: The Bi2212 precursor powder prepared in step 1 is preliminarily sintered four times at a temperature of 840° C. for 11 h to obtain a preliminarily sintered powder;

[0049] Step 3: subjecting the preliminary sintered powder obtained in step 2 to low oxygen partial pressure heat treatment to obtain low oxygen partial pressure heat treated powder; the low oxygen partial pressure heat treatment has an oxygen partial pressure of 10 Pa, a temperature of 580° C. and a time of 6 h;

[0050] Step 4: putting the low oxygen partial pressure heat-treated powder obtained in step 3 into a silver tube to obtain a composite blank;

[0051] Step 5: Drawing the composite blank obtained in step 4 to obtain a composite wire; the deformation rate of each drawing process is 8% to 12%;

[0052] Step 6: finally sintering the composite wire obtained in step 5 to obtain a Bi2212 wire with excellent plastic deformation performance and excellent current carrying capacity.

[0053] After testing, the single-pass pulling force of the composite wire prepared in this embodiment is 258MPa, and the critical current density (Jc) of the prepared Bi2212 wire is 1400A / mm2 under 4.2K, 12T conditions. The superconducting core wire in the Bi2212 wire is uniformly deformed without breakage or peeling, and the fluctuation range of the uniformity of the superconducting core wire diameter is ±11%.

[0054] Example 3

[0055] This embodiment includes the following steps:

[0056] Step 1: Prepare Bi2212 precursor powder with an atomic ratio of Bi, Sr, Ca, Cu, and O of 2.10:2.05:1.00:2.00:8 by coprecipitation method;

[0057] Step 2: The Bi2212 precursor powder prepared in step 1 is subjected to a secondary preliminary sintering at a temperature of 860° C. for 9 h to obtain a preliminary sintered powder;

[0058] Step 3: subjecting the preliminary sintered powder obtained in step 2 to low oxygen partial pressure post-heat treatment to obtain low oxygen partial pressure post-heat treatment powder; the low oxygen partial pressure post-heat treatment has an oxygen partial pressure of 1000 Pa, a temperature of 520° C., and a time of 12 h;

[0059] Step 4: putting the low oxygen partial pressure heat-treated powder obtained in step 3 into a silver tube to obtain a composite blank;

[0060] Step 5: Drawing the composite blank obtained in step 4 to obtain a composite wire; the deformation rate of each drawing process is 8% to 12%;

[0061] Step 6: finally sintering the composite wire obtained in step 5 to obtain a Bi2212 wire with excellent plastic deformation performance and excellent current carrying capacity.

[0062] After testing, the single-pass pulling force of the composite wire prepared in this embodiment is 270MPa, and the critical current density (Jc) of the prepared Bi2212 wire is 1350A / mm2 under 4.2K, 12T conditions. The superconducting core wire in the Bi2212 wire is uniformly deformed without breakage or peeling, and the fluctuation range of the uniformity of the superconducting core wire diameter is ±12%.

[0063] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment, characterized in that: The method comprises the following steps: Step 1, preparing Bi2212 precursor powder; Step 2: Preliminarily sintering the Bi2212 precursor powder prepared in step 1 to obtain a preliminary sintered powder; Step 3: subjecting the preliminary sintered powder obtained in step 2 to low oxygen partial pressure post-heat treatment to obtain low oxygen partial pressure post-heat treatment powder; the oxygen partial pressure in the low oxygen partial pressure post-heat treatment is 10Pa-1000Pa, the temperature is 520°C-580°C, and the time is 6h-12h; Step 4: putting the low oxygen partial pressure heat-treated powder obtained in step 3 into a silver tube to obtain a composite blank; Step 5: Drawing the composite blank obtained in step 4 to obtain a composite wire; Step 6: finally sintering the composite wire obtained in step 5 to obtain a Bi2212 wire with excellent plastic deformation performance and excellent current carrying capacity.

2. The method of improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment according to claim 1, characterized in that: The Bi2212 precursor powder in step one is prepared by a co-precipitation method, and the atomic ratio of Bi, Sr, Ca, Cu, and O in the Bi2212 precursor powder is 2.10:2.05:1.00:2.00:

8.

3. The method of improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment according to claim 1, characterized in that: The number of preliminary sintering in step 2 is two to four times, the temperature of the preliminary sintering is 840° C. to 860° C., and the time is 9 h to 11 h.

4. The method of improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment according to claim 1, characterized in that: The deformation rate of each drawing process in step 5 is 8% to 12%.

5. The method of improving the plastic deformation performance and current carrying capacity of Bi2212 wire by low oxygen partial pressure post-heat treatment according to claim 1, characterized in that: The single-pass pulling force of the composite wire in step 5 is less than 280 MPa, and the critical current density of the Bi2212 wire in step 6 is greater than 1350 A / mm 2 .