Neodymium-iron-boron permanent magnet material and method for improving residual magnetism of neodymium-iron-boron permanent magnet material
By adding lubricant and low molecular hydrocarbon gas to the production of NdFeB permanent magnet materials, the effect of improving residual magnetism without reducing coercive force is achieved, and the improvement of sintered NdFeB permanent magnet materials in the prior art is solved. The problem of residual magnetic induction strength significantly improves material performance.
Patent Information
- Application Number
- CN202411191406.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to increase the residual magnetic induction strength without reducing the coercive force of the sintered NdFeB permanent magnet material, and the existing methods have limited effect on improving the orientation of the blank.
By adding a mixture of lubricant and gasoline-based diluents to the neodymium iron boron powder as an additive, and after hydrogen breaking and dehydrogenation, low molecular hydrocarbon gases, such as acetylene, gas flow grinding, press molding, vacuum sintering and The grain boundary diffuses, introducing carbon evenly into the sintered matrix, and works together to enhance the residual magnetism.
With almost unchanged coercive force, the residual magnetic induction strength of the sintered NdFeB permanent magnet material is greatly improved, and the performance stability of the material is significantly improved.
Smart Images

Figure BDA0005015213000000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of permanent magnetic materials, and in particular to a neodymium iron boron permanent magnetic material and a method for improving the remanence of the neodymium iron boron permanent magnetic material. Background Art
[0002] With the development of technology, the requirements for the performance of sintered NdFeB permanent magnet materials in new motors are also increasing. As an important indicator to measure the magnetic properties of permanent magnet materials, the research results of residual magnetic induction intensity (Br) have not made significant progress in recent years, which has restricted the development of downstream industries.
[0003] At present, the methods to improve the residual magnetic induction intensity of sintered NdFeB permanent magnet materials include reducing the total amount of rare earth in sintered NdFeB permanent magnet materials, using pure neodymium instead of praseodymium and neodymium as raw materials, increasing lubricants or enhancing the orientation magnetic field to improve the orientation degree of NdFeB blanks, etc. However, under the existing process conditions, reducing the total amount of rare earth in sintered NdFeB permanent magnet materials or using pure neodymium instead of praseodymium and neodymium will significantly reduce the coercive force of sintered NdFeB permanent magnet materials. In addition, too low a total amount of rare earth may lead to the formation of α-Fe phase, unstable performance of mass-produced products, etc. At the same time, under the existing technology, the blank orientation forming technology is already very mature, and the method of increasing the orientation degree of the blank by adding lubricants or enhancing the orientation magnetic field has very limited effect on the improvement of the residual magnetic induction intensity of sintered NdFeB permanent magnet materials.
[0004] Based on this, it is very necessary to develop a new production process for sintered NdFeB permanent magnet materials to improve their residual magnetic induction intensity without reducing the coercive force of sintered NdFeB permanent magnet materials. Summary of the invention
[0005] The present invention aims to solve the technical problem of how to improve the residual magnetic strength of sintered NdFeB permanent magnet materials while keeping the coercive force almost unchanged. The present invention aims to provide a NdFeB permanent magnet material and a method for improving the residual magnetic induction strength of NdFeB permanent magnet materials, which can improve the residual magnetic induction strength of NdFeB permanent magnet materials while keeping the coercive force almost unchanged.
[0006] The present invention is achieved through the following technical solutions:
[0007] The first object of the present invention is to provide a method for improving the remanence of NdFeB permanent magnet material, comprising the following steps:
[0008] The alloy raw materials are vacuum melted to prepare NdFeB quick-setting sheets;
[0009] The NdFeB quick-setting sheet is subjected to hydrogen dehydrogenation, air flow milling, compression molding, cold isostatic pressing, vacuum sintering and aging heat treatment in sequence to obtain a blank; before air flow milling, an additive is added to the NdFeB coarse powder, wherein the additive is a mixture of a lubricant and a gasoline-type diluent, and the amount of the additive added accounts for 1-2‰ of the mass fraction of the NdFeB coarse powder;
[0010] Grain boundary diffusion is carried out on the surface of the blank to obtain NdFeB permanent magnet material.
[0011] Furthermore, the lubricant in the additive is one or more of isopropyl alcohol, cyclohexanone and oleic acid amide.
[0012] Furthermore, the gasoline diluent in the additive is one or more of solvent oil, pentane, hexane and heptane.
[0013] Furthermore, the additive is added in an amount of 1.5-2‰ of the mass fraction of the NdFeB coarse powder.
[0014] Furthermore, the components of the NdFeB quick-setting sheet include rare earth elements, trace elements, B and Fe; the rare earth elements include one or more of La, Ce, Pr, Nd, Gd, Tb, Dy, Ho and Y, with a content of 28.5wt%-32.5wt%; the trace elements include one or more of Ga, Al, Cu, Co, Ti, Zr and Nb, with a content of ≤5wt%; the B content is 0.85wt%-1.1wt%; and the remaining elements are Fe.
[0015] Furthermore, after hydrogen dehydrogenation, argon gas containing low molecular hydrocarbon gas is charged into the hydrogen decomposition furnace to allow the low molecular hydrocarbon gas to diffuse and infiltrate the surface layer of the NdFeB coarse powder.
[0016] Furthermore, the low molecular weight hydrocarbon gas is acetylene.
[0017] Furthermore, the diffusion temperature is 500-700°C.
[0018] Furthermore, the grain boundary diffusion is performed by coating the diffusion source on the surface of the blank through screen printing or spraying process.
[0019] The second object of the present invention is to provide a NdFeB permanent magnet material prepared by the above method.
[0020] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0021] 1. The present invention adds additives to the NdFeB coarse powder before air flow milling and controls the proportion of the additives to make the prepared permanent magnet material have higher remanence.
[0022] 2. The present invention introduces carbon source to evenly introduce carbon into the interior of the sintered NdFeB matrix, and works synergistically with additives to achieve a significant increase in the residual magnetic induction intensity of the sintered NdFeB permanent magnet material while keeping the coercive force almost unchanged. DETAILED DESCRIPTION
[0023] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the technical solutions in the embodiments of the present invention are clearly and completely described below in conjunction with embodiments. Obviously, the schematic implementation modes of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.
[0024] The following is a detailed description of an embodiment of a NdFeB permanent magnet material and a method for improving the remanence of a NdFeB permanent magnet material according to the present invention. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions and repeated descriptions of well-known matters are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art.
[0025] The "range" disclosed in this application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range.
[0026] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0027] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0028] Unless otherwise specified, the terms "include" and "comprising" mentioned in this application may be open-ended or closed-ended. For example, the terms "include" and "comprising" may mean that other substances not listed may also be included or only the listed substances may be included.
[0029] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0030] At present, the methods to improve the residual magnetic induction intensity of sintered NdFeB permanent magnet materials include reducing the total amount of rare earth in sintered NdFeB permanent magnet materials, using pure neodymium instead of praseodymium and neodymium as raw materials, increasing lubricants or enhancing the orientation magnetic field to improve the orientation degree of NdFeB blanks, etc. However, under the existing process conditions, reducing the total amount of rare earth in sintered NdFeB permanent magnet materials or using pure neodymium instead of praseodymium and neodymium will significantly reduce the coercive force of sintered NdFeB permanent magnet materials. In addition, too low a total amount of rare earth may lead to the formation of α-Fe phase, unstable performance of mass-produced products, etc. At the same time, under the existing technology, the blank orientation forming technology is already very mature, and the method of increasing the orientation degree of the blank by adding lubricants or enhancing the orientation magnetic field has very limited effect on the improvement of the residual magnetic induction intensity of sintered NdFeB permanent magnet materials. In order to solve the problems existing in the prior art for improving the remanence strength of sintered NdFeB permanent magnet materials and to improve the remanence while keeping the coercive force almost unchanged, the technical solution of the present invention is to provide a method for improving the remanence of NdFeB permanent magnet materials, comprising the following steps:
[0031] The alloy raw materials are vacuum melted to prepare NdFeB quick-setting sheets;
[0032] The NdFeB quick-setting sheet is subjected to hydrogen dehydrogenation, air flow milling, compression molding, cold isostatic pressing, vacuum sintering and aging heat treatment in sequence to obtain a blank; before air flow milling, an additive is added to the NdFeB coarse powder, wherein the additive is a mixture of a lubricant and a gasoline-type diluent, and the amount of the additive added accounts for 1-2‰ of the mass fraction of the NdFeB coarse powder;
[0033] Grain boundary diffusion is carried out on the surface of the blank to obtain NdFeB permanent magnet material.
[0034] The invention adds additives to the NdFeB coarse powder before air flow milling and controls the proportion of the additives so that the prepared permanent magnetic material has higher remanence and coercive force.
[0035] As a preferred embodiment, the lubricant in the additive is one or more of isopropanol, cyclohexanone, and oleic acid amide; the gasoline diluent in the additive is one or more of solvent oil, pentane, hexane, and heptane.
[0036] As a preferred embodiment, the additive is added in an amount of 1.5-2‰ of the mass fraction of the NdFeB coarse powder. For example, the additive is added in an amount of 1.5‰ or 2‰ of the mass fraction of the NdFeB coarse powder. The inventors have verified that when the additive is added in an amount of 1.5-2‰ of the mass fraction of the NdFeB coarse powder, the remanence and coercivity are improved to a certain extent compared to when the additive is added in an amount of 1‰, and the effect is better.
[0037] As a preferred embodiment, the components of the NdFeB quick-setting sheet include rare earth elements, trace elements, B and Fe; the rare earth elements include one or more of La, Ce, Pr, Nd, Gd, Tb, Dy, Ho and Y, with a content of 28.5wt%-32.5wt%; the trace elements include one or more of Ga, Al, Cu, Co, Ti, Zr and Nb, with a content of ≤5wt%; the B content is 0.85wt%-1.1wt%; and the remaining elements are Fe.
[0038] As a preferred embodiment, after hydrogen dehydrogenation, argon gas containing low molecular hydrocarbon gas is charged into the hydrogen decomposition furnace to allow the low molecular hydrocarbon gas to diffuse and infiltrate the surface layer of the NdFeB coarse powder.
[0039] As a preferred implementation, the low molecular hydrocarbon gas is acetylene, and the diffusion temperature is 500-700°C.
[0040] In the present invention, the preferred low molecular hydrocarbon gas is acetylene. The inventors have found in their research that the carbon content and performance of the blanks of methane, ethane and ethylene do not change significantly after being introduced into a hydrogen cracking furnace. However, when acetylene is introduced as the gas, a small amount of acetylene will be cracked, thereby uniformly introducing carbon into the sintered NdFeB matrix in the form of carbon black, and synergizing with the additives to achieve a significant improvement in the residual magnetic induction intensity of the sintered NdFeB permanent magnet material without affecting the coercive force of the sintered NdFeB permanent magnet material.
[0041] As a preferred embodiment, the grain boundary diffusion is coated on the surface of the blank by screen printing or spraying. It should be noted that the present invention does not limit the diffusion source of the grain boundary diffusion, and the diffusion source in the prior art can be used for grain boundary diffusion. During the diffusion treatment, the substrate can also be treated by conventional diffusion and aging processes. In the following embodiments of the present invention, Dy is used as the diffusion source for experiments.
[0042] Based on this, the present invention obtains a NdFeB permanent magnet material with high coercive force and high remanence through the above preparation method.
[0043] The technical solution of the present invention is further described in detail below in conjunction with embodiments.
[0044] It should be noted that the experimental methods used in the examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained by those skilled in the art through commercial channels.
[0045] In the following examples, the composition of the matrix blank is (PrNd) 30.3 (GaAlCuCoTiZr) 1.5 Fe 67.34 B 0.96 .
[0046] Comparative Example 1
[0047] A method for improving the remanence of a NdFeB permanent magnet material comprises the following steps:
[0048] (1) The alloy raw materials are vacuum melted and cast into 0.2-0.35 mm thick sheets at a casting temperature of about 1440°C to obtain NdFeB quick-setting sheets;
[0049] (2) dehydrogenating the NdFeB quick-setting sheets at 560-600°C and coarsely crushing them to obtain NdFeB coarse powder;
[0050] (3) adding a mixed additive with a mass fraction of 1‰ to the NdFeB coarse powder, wherein the additive is a mixture of lubricating oil (oleic acid amide) and gasoline diluent (pentane) in a ratio of 1:1;
[0051] (4) preparing NdFeB powder with a particle size of 2-4 μm by jet mill;
[0052] (5) Using a forming press to press a 60*43*39 mm blank, the orientation magnetic field is >1.8T, and cold isostatic pressing is performed at 200MPa;
[0053] (6) Vacuum sintering at 1076°C for 6 hours;
[0054] (7) Aging process 1: 850-950°C, holding time 2-6h, aging process 2: 700-850°C, holding time 3-20h, aging process 3: 450-550°C, holding time 2-6h, to obtain a blank.
[0055] (8) Performing grain boundary diffusion on the above blank to obtain NdFeB permanent magnet material:
[0056] The sintered NdFeB permanent magnet blank is processed into a square magnet with a thickness of 2mm in the magnetization direction (the length and width are arbitrary) by multi-wire cutting. Dy is evenly coated on the surface of the magnet by screen printing, and the Dy coating amount is controlled to be 0.65wt%. Heat treatment is carried out in a vacuum sintering furnace, and the heat treatment includes a primary heat treatment temperature range of 850℃-950℃, a heat treatment time of 5h-40h, a secondary heat treatment temperature range of 400℃-700℃, a heat treatment time of 2.5h-6.5h, and the vacuum degree of the diffusion furnace is controlled to 10 -1 -10 -4 Pa, so that the diffused NdFeB permanent magnet material is obtained.
[0057] Example 1
[0058] The difference between this embodiment and comparative example 1 is that a mixed additive with a mass fraction of 1.5‰ is added to the NdFeB coarse powder, and the other conditions remain unchanged.
[0059] Example 2
[0060] The difference between this embodiment and comparative example 1 is that a mixed additive with a mass fraction of 2‰ is added to the NdFeB coarse powder, and other conditions remain unchanged.
[0061] Comparative Example 2
[0062] The difference between this comparative example and comparative example 1 is that: after the hydrogen dehydrogenation is completed, argon containing methane is filled into the hydrogen dehydrogenation furnace, and the reaction is carried out under the condition that the temperature does not exceed 650°C. During the reaction, the furnace should rotate at a uniform speed to ensure uniform carbon adhesion. After the reaction is completed, argon is filled into the furnace for protection and excess methane is discharged, and the hydrogen dehydrogenation furnace is cooled by water cooling. When the temperature of the NdFeB coarse powder in the furnace drops to room temperature, it is taken out of the furnace. Then, a mixed additive with a mass fraction of 1‰ is added before the NdFeB coarse powder is jet-milled. The additive is a mixture of lubricating oil (oleic acid amide) and gasoline diluent (pentane) in a ratio of 1:1; then, orientation molding and sintering are carried out according to the process of the comparative example.
[0063] Comparative Example 3
[0064] The difference between this embodiment and comparative example 2 is that the gas filled into the hydrogen cracking furnace after the hydrogen cracking dehydrogenation is completed is changed to argon containing ethane, and the other conditions remain unchanged.
[0065] Comparative Example 4
[0066] The difference between this embodiment and comparative example 2 is that the gas charged into the hydrogen cracking furnace after the hydrogen cracking dehydrogenation is completed is changed to argon containing ethylene, and the other conditions remain unchanged.
[0067] Example 3
[0068] The difference between this embodiment and comparative example 2 is that the gas filled into the hydrogen cracking furnace after the hydrogen cracking dehydrogenation is completed is changed to argon containing acetylene, and the other conditions remain unchanged.
[0069] Example 4
[0070] The difference between this embodiment and embodiment 3 is that a mixed additive with a mass fraction of 1.5‰ is added to the NdFeB coarse powder, and the other conditions remain unchanged.
[0071] Example 5
[0072] The difference between this embodiment and embodiment 3 is that a mixed additive with a mass fraction of 2‰ is added to the NdFeB coarse powder, and the other conditions remain unchanged.
[0073] The C content and magnetic properties of the sintered NdFeB permanent magnet materials produced in the comparative example and the embodiment were respectively detected by using the CS-3000 CS analyzer and the NIM-62000 permanent magnet precision measurement system. The diffused sample was first polished to a light finish by double-sided grinding, and then five diffused samples were stacked and taken. The test results are shown in Table 1.
[0074] Table 1. Carbon content and magnetic properties of sintered NdFeB permanent magnet materials of comparative examples and embodiments
[0075]
[0076] From the data in Table 1, we can see that:
[0077] When the additive addition amount in comparative example 1 is 1‰, the matrix remanence is 14.45 kGs and the coercive force is 14.02 kOe. By increasing the proportion of additives in embodiments 1 and 2, the remanence of the samples before and after diffusion is improved, and the coercive force can be slightly improved after diffusion.
[0078] Comparative Examples 2-4 are respectively introduced with methane, ethane and ethylene gases. Compared with Comparative Example 1, the remanence and coercive force of the blank are basically unchanged, indicating that the introduction of methane, ethane and ethylene as carbon sources has basically no effect on the performance of the blank.
[0079] In Example 3, acetylene gas was introduced, which significantly improved the remanence of the sample before and after diffusion, while the coercive force remained basically unchanged, compared with Comparative Example 1. This proves that the introduction of acetylene can evenly introduce carbon into the sintered NdFeB matrix, thereby improving the remanent magnetic induction intensity of the sintered NdFeB permanent magnet material while keeping the coercive force almost unchanged.
[0080] In Examples 4 and 5, the amount of additives is further increased compared to Example 3. From the data, it can be seen that the remanence of the samples can also be significantly improved before and after diffusion. Among them, the coercive force of Example 5 decreases to a certain extent, but the decrease is very small. In Example 4, not only the remanence is significantly improved, but the coercive force is basically unchanged, and the comprehensive effect is the best. This shows that when the amount of additives added is 1.5‰, the synergistic effect of acetylene and additives is more obvious and the synergistic effect is better.
[0081] Finally, it should be noted that the above specific embodiments are only used to explain in detail the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific implementation method of the present invention and is not used to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above specific embodiments, ordinary technicians in this field should understand that it is still possible to modify the technical solutions recorded in the above embodiments, or to replace or improve some or all of the technical features therein. These modifications, equivalent replacements and improvements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and description of the present invention.
Claims
1. A method for improving the remanence of NdFeB permanent magnet material, characterized in that: The following steps are involved: The alloy raw materials are vacuum melted to prepare NdFeB quick-setting sheets; The NdFeB quick-setting sheet is subjected to hydrogen dehydrogenation, air flow milling, compression molding, cold isostatic pressing, vacuum sintering and aging heat treatment in sequence to obtain a blank; before air flow milling, an additive is added to the NdFeB coarse powder, wherein the additive is a mixture of a lubricant and a gasoline-type diluent, and the amount of the additive added accounts for 1-2‰ of the mass fraction of the NdFeB coarse powder; Grain boundary diffusion is carried out on the surface of the blank to obtain NdFeB permanent magnet material.
2. A method for improving the remanence of NdFeB permanent magnet material according to claim 1, characterized in that: The lubricant in the additive is one or more of isopropanol, cyclohexanone and oleic acid amide.
3. The method for improving the remanence of NdFeB permanent magnet material according to claim 1, characterized in that: The gasoline diluent in the additive is one or more of solvent oil, pentane, hexane and heptane.
4. The method for improving the remanence of NdFeB permanent magnet material according to claim 1, characterized in that: The additive amount accounts for 1.5-2‰ of the mass fraction of the NdFeB coarse powder.
5. The method for improving the remanence of NdFeB permanent magnet material according to claim 1, characterized in that: The components of the NdFeB quick-setting sheet include rare earth elements, trace elements, B and Fe; the rare earth elements include one or more of La, Ce, Pr, Nd, Gd, Tb, Dy, Ho and Y, with a content of 28.5wt%-32.5wt%; the trace elements include one or more of Ga, Al, Cu, Co, Ti, Zr and Nb, with a content of ≤5wt%; the B content is 0.85wt%-1.1wt%; and the remaining elements are Fe.
6. A method for improving the remanence of NdFeB permanent magnet material according to claim 1, wherein argon containing low molecular hydrocarbon gas is charged into the hydrogen cracking furnace after hydrogen cracking and dehydrogenation, so that the low molecular hydrocarbon gas diffuses and infiltrates into the surface layer of the NdFeB coarse powder.
7. The method for improving the remanence of NdFeB permanent magnet material according to claim 6, wherein the low molecular hydrocarbon gas is acetylene.
8. The method for improving the remanence of NdFeB permanent magnet material according to claim 6, wherein the diffusion temperature is 500-700°C.
9. The method for improving the remanence of NdFeB permanent magnet material according to claim 1, wherein the grain boundary diffusion is performed by coating the diffusion source on the surface of the blank through screen printing or spraying process.
10. A neodymium iron boron permanent magnet material, characterized in that: The method is prepared by any one of claims 1 to 9.
Citation Information
Patent Citations
Method for preparing rare earth permanent magnet
CN101404195A
Neodymium iron boron permanent magnet alloy material
CN112397269A
Treatment method for soft magnetic metallic materials
CN113015820A
Production of rare earth-iron based sintered permanent magnet and molding material
JP1996170103A
Sintered magnet and production method for sintered magnet
US20210272727A1
Cited By
Neodymium-iron-boron magnet material and preparation method and application thereof
CN120126919A
Neodymium iron boron magnet material and its preparation method and application
CN120126919B
Aging temperature stability additive for sintered neodymium iron boron as well as preparation method and application of aging temperature stability additive
CN121260622A