Preparation method of composite positive plate and solid-state battery

By adding mesogenic anatase-type titanium dioxide material prepared by hydrothermal method to the high-nickel composite cathode sheet, the problem of low interface conductivity in solid-state lithium-ion batteries is solved, simplifying the processing process and significantly improving the battery performance.

CN118969949APending Publication Date: 2024-11-15ZHEJIANG FUNLITHIUM NEW ENERGY TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411178592.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The high-nickel positive electrode material in solid-state lithium-ion batteries has low interfacial conductivity, resulting in poor battery performance. The existing technology requires secondary processing of the material, which is complex and costly.

Method used

The mesogenic anatase-type titanium dioxide material with excellent lithium ion conductivity was prepared by hydrothermal method, and added to the high-nickel composite positive electrode sheet to form an efficient lithium ion transmission path through the mesogenic structure to reduce the positive electrode interface resistance.

Benefits of technology

It significantly improves the performance of all-solid-state batteries, reduces the internal resistance of the battery, enhances the embedded and disengagement rate of lithium ions, improves the rate performance and cycle stability, and simplifies the material processing process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The preparation method comprises the following steps: adding a high-nickel ternary positive electrode material, a sulfide solid electrolyte, mesocrystal anatase type titanium dioxide, a lithium salt and a binder into a polar solvent according to a molar ratio of (30-50): (3-8): (1.5-5): (0.5-2.5): (0.5-1.5), stirring for 12-24 hours at normal temperature, and uniformly mixing to obtain a mixed solution; and coating a positive electrode current collector with the mixed solution to obtain a composite positive electrode with a certain thickness, rolling the composite positive electrode under the pressure of 20-50MPa, and punching according to requirements to obtain a compact composite positive electrode plate. The composite positive plate prepared by the method can effectively enhance the ionic conductivity, improve the charge separation and transmission, and improve the thermal stability and the cycle stability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a composite positive electrode sheet and a solid-state battery. Background Art

[0002] As the application of lithium-ion power batteries in the field of new energy vehicles gradually expands, the driving range has become a key factor restricting the development of new energy vehicles. Improving the energy density of lithium-ion batteries is an effective way to solve the anxiety of driving range. High-nickel ternary layered materials have the advantages of high specific capacity, low cost and relatively good safety. They are considered to be one of the most promising high-energy lithium-ion battery positive electrode materials. The advantages of all-solid-state lithium batteries in energy density and thermal stability give it greater development potential. With the acceleration of the industrialization of solid-state batteries, the development of high-nickel ternary positive electrode materials has become the focus of attention in the industry, and its technical advantages in the advanced lithium-ion battery market have become increasingly obvious. However, the interface of solid-state batteries is solid-solid contact. Compared with liquid electrolytes, solid electrolytes are not fluid, so it is difficult to penetrate into the entire electrode and battery interface, resulting in a series of problems with poor interface contact. Therefore, it is necessary to improve the interfacial conductivity of the high-nickel positive electrode to improve the performance of the solid-state battery. For example, the patent with application number CN202210459908.3 proposed "coated modified high-nickel ternary positive electrode material, preparation method thereof and lithium-ion battery", and used acid-base reaction to uniformly deposit a layer of fast ion conductor on the surface of the ternary material, thereby improving the material's cycle performance, rate performance, and low-temperature performance; for example, the patent with application number CN202410537447.6 proposed "a hybrid dual-conductor coated positive electrode material, preparation method thereof and solid-state battery". The surface of the prepared hybrid dual-conductor coated positive electrode material is coated with a mixed coating layer of multi-walled carbon nanotubes and chloride solid electrolytes. The two substances in the mixed layer can cooperate with each other to improve the material's rate and cycle and other electrical properties.

[0003] The above technical solutions can improve the performance of high-nickel positive electrode materials, but they all require secondary treatment of high-nickel powder, and the material processing process is complicated and costly. In view of the above problems, the present invention proposes a method for preparing a composite positive electrode sheet and a solid-state battery, and uses a simple hydrothermal method to prepare a mesomorphous anatase titanium dioxide material with excellent lithium ion conductivity, which is added to a high-nickel composite positive electrode sheet to form an efficient lithium ion transmission pathway, significantly reduce the positive electrode interface resistance, and improve the performance of the all-solid-state battery. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a composite positive electrode sheet and a solid-state battery. A mesogenic anastase titanium dioxide material with excellent lithium ion conductivity is prepared by a simple hydrothermal method and added to a high-nickel composite positive electrode sheet to form an efficient lithium ion transmission pathway, significantly reduce the positive electrode interface resistance, and improve the performance of the all-solid-state battery.

[0005] The technical solution adopted by the present invention to solve the above technical problems is:

[0006] A method for preparing a composite positive electrode sheet comprises the following steps:

[0007] High nickel ternary positive electrode material, sulfide solid electrolyte, mesomorphous anatase titanium dioxide, lithium salt and binder are added to a polar solvent in a molar ratio of 30-50:3-8:1.5-5:0.5-2.5:0.5-1.5, and stirred at room temperature for 12h-24h to mix evenly to obtain a mixed solution; the mixed solution is coated on the positive electrode current collector to obtain a composite positive electrode with a certain thickness, and then the composite positive electrode is rolled under a pressure of 20MPa-50MPa and punched as required to obtain a dense composite positive electrode sheet.

[0008] Preferably, the mass ratio of the high-nickel ternary positive electrode material to the polar solvent is 11-20:12-25.

[0009] Preferably, the lithium salt is one or more of lithium bis(oxalate borate) LiBOB, lithium hexafluorophosphate LiPF6, lithium bis(fluorosulfonyl)imide LiFSI, and lithium bis(trifluoromethanesulfonyl)imide LITFSI.

[0010] Preferably, the binder is one of polyacrylonitrile PAN, polyimide PI, polyvinyl alcohol PVA, polyvinylidene fluoride PVDF and polyacrylamide PAM.

[0011] Preferably, the mesomorphous anatase titanium dioxide includes pure titanium dioxide and its doped and modified derivatives, and the doped and modified derivatives include at least one of nitrogen doping, carbon doping, sulfur doping, metal and oxide modification.

[0012] Preferably, the sulfide solid electrolyte is a binary sulfide electrolyte and / or a ternary sulfide solid electrolyte.

[0013] Preferably, the coating thickness on the surface of the positive electrode current collector is 150 μm-500 μm.

[0014] Preferably, the polar solvent is one of dimethyl sulfoxide, acetonitrile, formamide, trifluoroacetic acid, DMF, hexamethylphosphoramide, methanol, acetic acid, ethanol, isopropanol, pyridine, tetramethylethylenediamine, acetone, triethylamine, n-butanol, dioxane, tetrahydrofuran, and methyl formate.

[0015] Preferably, the mesogenic anatase titanium dioxide is prepared by the following preparation method: a titanium source is dissolved in a 1 mol / L-3 mol / L hydrochloric acid solution, the volume ratio of the titanium source to the hydrochloric acid is 1-3:4-10, the mixture is stirred at 40°C-100°C for 40h-60h, and a white product is obtained by centrifugation. The white product is washed with deionized water to remove residual inorganic ions, and the white product is vacuum dried at 80°C-120°C for 12h-36h, and finally calcined in air at 400°C-500°C for 12h-24h to obtain a mesogenic anatase titanium dioxide powder.

[0016] A solid-state battery comprises a composite negative electrode sheet, a composite solid electrolyte membrane and a composite positive electrode sheet prepared by the above method.

[0017] Compared with the prior art, the advantages of the present invention are:

[0018] 1. By adding mesocrystalline anatase titanium dioxide powder to the composite positive electrode sheet, the mesocrystalline structure of TiO 2 It has a high specific surface area and abundant pores, which helps to form a more efficient ion conduction path and reduce the ion diffusion resistance inside the battery.

[0019] 2. In lithium-ion batteries, TiO 2 The unique crystal structure helps to accelerate the insertion and extraction of lithium ions and improve the overall rate performance of the battery. Compared with the ordinary structure anatase titanium dioxide, after the first cycle, the mesocrystal anatase titanium dioxide and the lattice spacing are widened, providing a more effective ion channel and significantly improving the ion conductivity.

[0020] 3. Since the mesomorphous structure has a large number of pores, the contact area with the electrolyte is increased, the interface resistance is reduced, which is beneficial to improve the charge separation efficiency and improve the overall battery performance.

[0021] 4. In terms of lithium ion transport mechanism, mesomorphous anatase titanium dioxide is based on a highly reversible crystallization-amorphous-recrystallization process. The synergistic effect of the amorphous phase and the inherent intergranular rapid diffusion network inside the mesomorph makes the lithium ion diffusion rate inside the structure much higher than that of conventional anatase titanium dioxide. In addition, the final product after delithiation is Li 0.16 TiO 2 , the material stability has been significantly improved, and the interface stability of the high-nickel positive electrode has been further improved. DETAILED DESCRIPTION

[0022] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.

[0023] Example:

[0024] A solid-state battery comprises a composite positive electrode sheet, a composite solid electrolyte membrane and a composite negative electrode sheet of micron-sized silicon particles, wherein the composite solid electrolyte membrane is located between the composite positive electrode sheet and the composite negative electrode sheet.

[0025] Preparation of micron-sized silicon particle composite negative electrode sheet:

[0026] Mesocrystalline anatase titanium dioxide powder, polymer solid electrolyte, sulfide solid electrolyte, micron-sized silicon particles and aqueous binder are added to a polar solvent in a molar ratio of 1.5-3:1-4:0.5-2:20-35:0.01-0.2, and the mass ratio of micron-sized silicon particles to polar solvent is 20-30:45-55, and stirred at room temperature for 10h-30h to obtain a mixed slurry; at room temperature, the mixed slurry is coated on the negative electrode current collector by a doctor blade method or a transfer coating method, and the coating thickness is 50μm-500μm to obtain a composite negative electrode with a certain thickness, and the composite negative electrode is rolled under a pressure of 5MPa-30MPa, and then punched according to requirements to obtain a dense micron-sized silicon particle composite negative electrode sheet. Among them, the particle size of the micron-sized silicon particles is 0.5μm-15μm, and the shape of the silicon particles is not limited.

[0027] The water-based binder is one of styrene-butadiene rubber (SBR) emulsion, carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyacrylonitrile (PAN) and polyacrylate.

[0028] The negative electrode current collector adopts an elastic composite current collector, and the elastic composite current collector is prepared by a preparation method of a current collector for an all-solid-state battery disclosed in application number 202111044090.0, as in Example 1 in the above application document, MF is mixed in a ratio of 4:3 and heated to 85°C, and melamine is continued to be added to the mixture while keeping the temperature constant, so that the mass ratio of melamine to water is 11:12, and stirring is continued until the mixed solution is clear, and the pH of the mixed solution is adjusted with hexamethylenetetramine to make the pH of the mixed solution 8-9, EG is added, and the mass ratio of EG to water is 1:12, and the reaction is carried out for 2min-3min. After the reaction is completed, sodium borate decahydrate is added to make the pH value of the mixed solution 10-10.5, and the mixed solution is cooled to 28°C, and the temperature is kept constant for 3min to obtain a viscous EG / MF prepolymer; EG / MF prepolymer, n-hexane, dimethyl silicone oil, hydrochloric acid and CF are added into a container in a mass ratio of 55:3:1:0.15:0.4, stirred at room temperature for 15 minutes to obtain a foaming liquid; the foaming liquid is quickly introduced into a mold, foamed at 100°C for 35 minutes, and then cured at 125°C for 5 minutes to obtain CF / MF; the CF / MF is carbonized in nitrogen at 850°C for 2 minutes, cooled to room temperature, and then rinsed with water and ethanol to remove residual impurities therein to obtain carbonized CF / MF; the obtained carbonized CF / MF is used as a cathode, copper foil is used as an anode, and 1.0 mol / L copper sulfate solution is used as an electrolyte, a pulse current of 10 mA / cm2 is applied for electrodeposition, and the electrodeposition lasts for 15 minutes to obtain an elastic composite current collector of CF / MF / Cu.

[0029] The negative electrode current collector may also be one of copper foil, porous copper foil, carbon-coated copper foil, composite copper foil and high molecular polymer foil.

[0030] Preparation of composite solid electrolyte membrane:

[0031] Mesomorphous anatase titanium dioxide powder, polymer solid electrolyte, sulfide solid electrolyte, and lithium salt are added to a polar solvent in a molar ratio of 1-2:2-5:3-7:0.2-1, and the mass ratio of sulfide solid electrolyte to polar solvent is 10-20:30-45. Stirring is continued at room temperature for 12h-25h to obtain a mixed slurry. At room temperature, the mixed slurry is coated on a polymer foil by a doctor blade method or a transfer coating method, and dried at 40℃-80℃ in a vacuum environment for 8h-16h. After peeling off the polymer foil, a composite solid electrolyte membrane is obtained, and the thickness of the composite solid electrolyte membrane is 50μm-400μm. Among them, the polymer foil is made of polyethylene terephthalate.

[0032] The polymer solid electrolyte used in the above-mentioned preparation of the negative electrode sheet and the composite solid electrolyte is at least one or more of polyethylene oxide (PEO), polyvinyl alcohol (PEG), polypropylene (PP), polyacrylate (PBA), polycarbonate (PCE), polypropylene (PAN), polytrimethylene carbonate (PTMC), polyvinyl chloride (PVC), polyamide (PA), and polyvinylidene fluoride (PVDF).

[0033] Preparation of composite positive electrode sheet:

[0034] High nickel ternary positive electrode material, sulfide solid electrolyte, mesomorphous anatase titanium dioxide, lithium salt and binder are added to the solvent in a molar ratio of 30-50:3-8:1.5-5:0.5-2.5:0.5-1.5, and the mass ratio of high nickel ternary positive electrode material to solvent is 11-20:12-25, and the mixture is stirred for 12h-24h at room temperature to obtain a mixed solution; at room temperature, the mixed solution is coated on the positive electrode current collector by a scraper method or a transfer coating method, and the coating thickness is 150μm-500μm to obtain a composite positive electrode with a certain thickness, and then the composite positive electrode is rolled under a pressure of 20MPa-50MPa and punched according to requirements to obtain a dense composite positive electrode sheet. Among them, the binder is one of polyacrylonitrile PAN, polyimide PI, polyvinyl alcohol PVA, polyvinylidene fluoride PVDF, and polyacrylamide PAM. The positive electrode current collector used is one of conventional aluminum foil, perforated aluminum foil, carbon-coated aluminum foil, composite aluminum foil, high molecular polymer foil (such as polyethylene terephthalate), etc.

[0035] The lithium salt used in the preparation of the composite positive electrode sheet and the composite solid electrolyte is one or more of lithium bis(oxalate borate) LiBOB, lithium hexafluorophosphate LiPF6, lithium bis(fluorosulfonyl)imide LiFSI, and lithium bis(trifluoromethanesulfonyl)imide LITFSI.

[0036] Preparation of the aforementioned mesocrystalline anatase titanium dioxide powder: dissolve the titanium source in 1mol / L-3mol / L hydrochloric acid solution, the volume ratio of the titanium source to the hydrochloric acid solution is 1-3:4-10, stir at 40℃-100℃ for 40h-60h, centrifuge to obtain a white product, wash with deionized water 3-6 times to remove the residual inorganic ions in the white product, and then vacuum dry the white product at 80℃-120℃ for 12h-36h, and finally calcine in air at 400℃-500℃ for 12h-24h to obtain mesocrystalline anatase titanium dioxide powder.

[0037] The titanium source includes at least one of dichlorotitacenes, tetraisopropoxytitanium, tetrabutyl titanate, titanium citrate, and titanium tetrachloride. The prepared mesocrystalline anatase titanium dioxide powder includes pure titanium dioxide and its doped and modified derivatives, and the doped and modified derivatives include at least one of nitrogen doping, carbon doping, sulfur doping, metal and oxide modification.

[0038] The sulfide solid electrolyte used in the preparation of the composite negative electrode sheet, composite positive electrode sheet and composite solid electrolyte membrane is a binary sulfide electrolyte and / or a ternary sulfide solid electrolyte. The binary sulfide electrolyte is Li 3 PS 4 and Li 7 P 3 S 11 , the ternary sulfide solid electrolyte is Li 10 G 2 S 12 and Li 6 PS 5 X, wherein X = Cl, Br and I.

[0039] The polar solvent used in the preparation of the composite negative electrode sheet, the composite positive electrode sheet and the composite solid electrolyte membrane is one of acetonitrile, formamide, trifluoroacetic acid, DMSO, DMF, hexamethylphosphoramide, methanol, acetic acid, ethanol, isopropanol, pyridine, tetramethylethylenediamine, acetone, triethylamine, n-butanol, dioxane, tetrahydrofuran and methyl formate.

[0040] Embodiment 1,

[0041] A solid-state battery is prepared by the following method:

[0042] Preparation of mesocrystalline anatase titanium dioxide powder: First, a certain amount of isopropoxy titanium was dripped into 1.5 mol / L hydrochloric acid, where the volume ratio of isopropoxy titanium to hydrochloric acid was 2:7. Then, stirring was continued at 80°C for 48 hours, and a white product was obtained after centrifugation. The product was washed with deionized water 4 times to remove the residual non-polar ions. The white product was dried at 110°C for 2 hours, and then sintered in nitrogen at 450°C for 16 hours to obtain nitrogen-doped mesocrystalline anatase titanium dioxide powder.

[0043] Preparation of micron-sized silicon particle composite negative electrode sheet:

[0044] The prepared mesomorphous anatase titanium dioxide powder was mixed with polyethylene oxide (PEO) and ternary sulfide solid electrolyte Li 10 G 2 S 12, micron-sized silicon particles and a small amount of polyacrylic acid (PAA) as a binder are added to an acetonitrile solvent in a molar ratio of 1.7:3.0:1.8:23:0.11, and the mass ratio of micron-sized silicon particles to acetonitrile is 25:49. After continuous stirring for 18 hours at room temperature, the mixed slurry is coated on the negative electrode current collector by a scraper method or a transfer coating method to obtain a composite negative electrode with a certain thickness. The micron-sized silicon particles used in the present invention have an average size of 3.5 microns, and the negative electrode current collector used is an elastic composite current collector. The coating thickness of the composite negative electrode is 250 microns. The coated composite negative electrode is rolled under a pressure of 25MPa to obtain a dense composite silicon-based negative electrode, and the rolled negative electrode is punched according to demand to obtain a micron-sized silicon particle composite negative electrode sheet.

[0045] Preparation of composite solid electrolytes:

[0046] The prepared mesomorphous anatase titanium dioxide powder was mixed with polypropylene (PAN) and ternary sulfide solid electrolyte Li 6 PS 5 Cl and lithium salt LITFSI were added into acetonitrile solvent in a molar ratio of 1.3:3.4:5:0.7. 6 PS 5 The mass ratio of Cl to acetonitrile is 17:42. Stirring is continued at room temperature for 23 hours. The mixed liquid is coated on a polymer foil (polyethylene terephthalate) using a scraper method, and dried at 70°C under vacuum for 15 hours. After peeling, a composite solid electrolyte membrane is obtained. The thickness of the composite solid electrolyte membrane is 50-400 μm.

[0047] Preparation of composite positive electrode sheet:

[0048] The high nickel ternary cathode material and ternary sulfide solid electrolyte Li 10 G 2 S 12 , mesomorphous anatase titanium dioxide, lithium bis(trifluoromethanesulfonic acid imide) LITFSI and polyacrylonitrile PAN are added to dimethyl sulfoxide in a molar ratio of 42:7:3.4:2.2:1.1, and the mass ratio of high nickel ternary material to dimethyl sulfoxide is 17:23. Stir for 22 hours at room temperature to mix evenly to obtain a mixed slurry. The mixed slurry is coated on a carbon-coated aluminum foil at room temperature by transfer coating to obtain a composite positive electrode with a certain thickness, and the coating thickness is 420 microns. Finally, the coated composite positive electrode is rolled at a pressure of 45MPa to obtain a dense composite positive electrode, and the rolled positive electrode is punched according to the requirements to obtain a composite positive electrode sheet.

[0049] The composite positive electrode sheet and composite negative electrode sheet prepared above were pressed on both sides of the composite solid electrolyte membrane at 70 standard atmospheres to prepare a button-type all-solid battery. The assembled battery was cycled at room temperature in the voltage range of 2.5V-4.3V at a rate of 0.5C. The internal resistance of the battery was tested by electrochemical impedance spectroscopy, with a frequency range of 0.1HZ to 1MHZ and an applied voltage amplitude of 5mV.

[0050] Embodiment 2,

[0051] Compared with Example 1, mesomorphous anatase titanium dioxide is sintered at 450°C in air and does not contain nitrogen doping. Preparation conditions of composite negative electrode sheet: the molar ratio of mesomorphous anatase titanium dioxide powder, polymer solid electrolyte, sulfide solid electrolyte, micron-sized silicon particles and binder is 3:1:2.0:20:0.2. Preparation conditions of composite positive electrode sheet: high nickel ternary positive electrode material and sulfide solid electrolyte, mesomorphous anatase titanium dioxide, lithium salt and binder are added to isopropanol in a molar ratio of 30:8:1.5:2.5:1.5, stirred at room temperature for 12 hours to mix evenly, and the mass ratio of high nickel ternary material to isopropanol is 11:25. The other conditions are the same as in Example 1.

[0052] Embodiment 3,

[0053] Compared with Example 1, the preparation conditions of the composite negative electrode sheet are as follows: the molar ratio of mesomorphic anatase titanium dioxide powder, polymer solid electrolyte, sulfide solid electrolyte, micron-sized silicon particles and binder is 1.5:4:0.5:35:0.01. The preparation conditions of the composite positive electrode sheet are as follows: the high nickel ternary positive electrode material and the sulfide solid electrolyte, mesomorphic anatase titanium dioxide, lithium salt and binder are added to dimethyl sulfoxide in a molar ratio of 50:3:5.0:0.5:0.5, stirred at room temperature for 24 hours to mix evenly, and the mass ratio of high nickel ternary material to dimethyl sulfoxide is 20:12. The other conditions are the same as those in Example 1.

[0054] Embodiment 4,

[0055] Compared with Example 1, the preparation conditions of the composite electrolyte membrane are as follows: mesocrystalline anatase titanium dioxide powder and polymer solid electrolyte, sulfide solid electrolyte Li 3 PS 4 , lithium salt LITFSI was added to acetonitrile solvent in a molar ratio of 2.0:5:3:0.2, and stirred continuously at room temperature for 25 hours. The mixed liquid was coated on a polymer foil (polyethylene terephthalate) by a doctor blade method, and dried at 65°C under vacuum for 12 hours. After peeling, a composite solid electrolyte membrane was obtained. 3 PS 4The mass ratio of acetonitrile to aluminum foil is 20:45. The positive electrode current collector is a conventional aluminum foil, and the negative electrode current collector is a conventional copper foil. The other conditions are the same as those in Example 1.

[0056] Embodiment 5,

[0057] Compared with Example 1, the coating thickness of the composite positive electrode sheet is 500 microns. The composite positive electrode sheet is rolled at a pressure of 50 MPa to obtain a dense composite positive electrode, and the rolled composite positive electrode is punched out as required.

[0058] The composite positive electrode sheet and the composite negative electrode sheet were respectively pressed on both sides of the composite solid electrolyte membrane at 50 standard atmospheres to prepare a button-type all-solid battery. The other conditions were the same as those in Example 1.

[0059] Embodiment 6,

[0060] Compared with Example 1, the preparation conditions of the mesocrystalline anatase titanium dioxide powder are as follows: calcination in air at 450°C for 12 hours; the lithium salt in the composite solid electrolyte is lithium hexafluorophosphate LiPF6. The other conditions are the same as those in Example 1.

[0061] Comparative Example 1

[0062] Compared with Example 1, the mesogenic titanium dioxide was sintered in air at 650° C. to obtain rutile mesogenic titanium dioxide powder. The other conditions were the same as those in Example 1.

[0063] Comparative Example 2

[0064] Compared with Example 1, commercial titanium dioxide powder (LOMON R 996) was used, and the other conditions were the same as those in Example 1.

[0065] Comparative Example 3

[0066] Compared with Example 1, no mesomorphous anatase titanium dioxide is added to the solid electrolyte membrane, and other conditions are the same as those in Example 1.

[0067] Comparative Example 4

[0068] Compared with Example 1, no mesocrystal anatase titanium dioxide is added to the composite positive electrode sheet, and the other conditions are the same as those in Example 1.

[0069] Comparative Example 5

[0070] Compared with Example 1, no mesocrystal anatase titanium dioxide is added to the composite negative electrode sheet, the composite positive electrode sheet and the solid electrolyte membrane, and the other conditions are the same as those in Example 1.

[0071] Comparative Example 6

[0072] Compared with Example 1, the mesomorphous anatase titanium dioxide in the composite negative electrode sheet is replaced by an equal amount of conductive carbon black, and the other conditions are the same as those in Example 1.

[0073] Comparative Example 7

[0074] Compared with Example 1, the composite negative electrode sheet uses nano-scale silicon powder, and the other conditions are the same as those of Example 1.

[0075] Table 1. Comparison of test results of different all-solid-state batteries

[0076] sample Internal resistance(Ω) Capacity retention rate after 100 cycles (%) Example 1 23.3 89.8 Example 2 30.6 86.2 Example 3 27.7 87.6 Example 4 27.1 88.5 Example 5 26.8 88.7 Example 6 25.5 88.1 Comparative Example 1 44.6 70.8 Comparative Example 2 50.3 66.3 Comparative Example 3 33.7 80.9 Comparative Example 4 39.2 75.1 Comparative Example 5 58.4 64.8 Comparative Example 6 42.8 71.4 Comparative Example 7 35.4 79.2

[0077] The specific test results are shown in Table 1. Combined with Examples 1-6, it can be seen that within the technical requirements of the present invention, the internal resistance and cycle life of the all-solid-state battery have been significantly improved, and Example 1 has the best technical effect. Combined with Example 1 and Comparative Examples 1-6, it is found that the mesogenic anatase titanium dioxide powder prepared by the present invention can significantly reduce the internal resistance of the battery and increase the cycle life of the battery. Compared with conventional commercial titanium dioxide powder and rutile titanium dioxide, the mesogenic anatase titanium dioxide prepared by the present invention is composed of tiny grains of several nanometers, which reduces structural defects such as twins or dislocations in the crystal structure, and is conducive to the appearance of amorphous Li during the lithiation process. 0.5 TiO 2 phase rather than orthorhombic phase Li 0.5 TiO 2 , thus improving the lithium storage capacity and lithium ion conductivity of titanium dioxide materials, while the chemical / mechanical properties of the amorphous phase improve the cycle stability of the battery. The composite silicon negative electrode used in the present invention is micron-sized, has a lower specific surface area than nanoparticles, and has low side reactions with solid electrolytes, which reduces material costs. In addition, the elastic current collector provides a strong support force to buffer the volume changes of the silicon negative electrode during charging and discharging. Filling a small amount of solid electrolyte and mesocrystal rutile titanium dioxide particles maintains the mechanical stability of the interface between silicon micron particles and the lithium ion transmission channel, so the cycle life and internal resistance of the all-solid-state battery are significantly improved. The above results show that the method proposed in the present invention can significantly improve the internal resistance and cycle stability of silicon-based all-solid-state batteries, providing important technical support for the development of high-performance lithium-ion power batteries.

[0078] By adding mesocrystalline anatase titanium dioxide to the composite electrolyte membrane, since the mesocrystalline anatase titanium dioxide is composed of tiny subunits gathered together in the same direction, the highly ordered structure is formed, which is conducive to the rapid transport of electrons and has a higher specific surface area and more defect sites at the atomic level. Compared with the ordinary structure anatase titanium dioxide, after the first cycle, the mesocrystalline anatase titanium dioxide and the lattice spacing are widened, providing a more effective ion channel and significantly improving the ion conductivity. At the same time, since the mesocrystalline structure has a large number of pores, it increases the contact area with the electrolyte and reduces the interface resistance, which is conducive to improving the charge separation efficiency and improving the overall battery performance. In terms of lithium ion transport mechanism, mesocrystalline anatase titanium dioxide is based on a highly reversible crystallization-amorphous-recrystallization process. The synergistic effect of the amorphous phase and the inherent intergranular rapid diffusion network inside the mesocrystal makes the lithium ion diffusion rate inside the structure much higher than that of conventional anatase titanium dioxide, and because the final product after delithiation is Li with good chemical / mechanical stability 0.16 TiO 2 The material stability has been significantly improved, and the interface stability between the solid electrolyte and the positive and negative electrodes has been further improved.

[0079] Micron-sized pure silicon particles are used in the negative electrode, with a particle size range of 0.5 μm-15 μm. The shape of silicon particles is not restricted, and the silicon material itself has a certain electronic conductivity (about 3×10 -5 S / cm), in order to avoid unnecessary interface side reactions and improve the battery energy density, the negative electrode sheet prepared by the present invention does not add any inactive carbon conductive agent, and adds electrochemically active mesocrystal rutile titanium dioxide to improve the electrode specific capacity and interface conductivity. Compared with nano silicon particles, the negative electrode prepared by micron-sized silicon particles has high conductivity and high volume energy density. However, silicon particles will undergo a maximum volume change of about 300% during the lithium ion deintercalation process. The volume shrinkage of silicon particles during the delithiation process leads to pores inside the negative electrode, causing the internal resistance of the negative electrode sheet to increase and reduce battery performance. To solve this problem, the present invention adds an elastic composite solid electrolyte with electrochemical activity to the above-mentioned silicon particles, fills the pores generated when the silicon particles shrink in volume during lithium deintercalation, always ensures contact with the silicon particles, and has lithium storage capacity, which can significantly improve the transmission speed of lithium ions between silicon particles. The negative electrode current collector adopts an elastic composite current collector, which can provide sufficient elasticity to mitigate the volume change of the silicon-based negative electrode system during the charging and discharging process.

[0080] Compared with conventional nano-titanium dioxide and micro-titanium dioxide materials, the synergistic effect of the inherent inter-granular rapid diffusion network within the mesogenic anatase-type titanium dioxide enables its lithium ion diffusion rate to be higher and can significantly improve the material's cycle stability.

[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a composite positive electrode sheet, characterized in that: The following steps are involved: High nickel ternary positive electrode material, sulfide solid electrolyte, mesomorphous anatase titanium dioxide, lithium salt and binder are added to a polar solvent in a molar ratio of 30-50:3-8:1.5-5:0.5-2.5:0.5-1.5, and stirred at room temperature for 12h-24h to mix evenly to obtain a mixed solution; the mixed solution is coated on the positive electrode current collector to obtain a composite positive electrode with a certain thickness, and then the composite positive electrode is rolled under a pressure of 20MPa-50MPa and punched as required to obtain a dense composite positive electrode sheet.

2. The method for preparing a composite positive electrode sheet according to claim 1, characterized in that: The mass ratio of the high-nickel ternary positive electrode material to the polar solvent is 11-20:12-25.

3. The method for preparing a composite positive electrode sheet according to claim 1, characterized in that: The lithium salt is one or more of lithium bis(oxalate borate) LiBOB, lithium hexafluorophosphate LiPF6, lithium bis(fluorosulfonyl)imide LiFSI, and lithium bis(trifluoromethanesulfonyl)imide LITFSI.

4. The method for preparing a composite positive electrode sheet according to claim 1, characterized in that: The binder is one of polyacrylonitrile PAN, polyimide PI, polyvinyl alcohol PVA, polyvinylidene fluoride PVDF and polyacrylamide PAM.

5. The method for preparing a composite positive electrode sheet according to claim 1, characterized in that: The mesomorphous anatase titanium dioxide includes pure titanium dioxide and its doped and modified derivatives, wherein the doped and modified derivatives include at least one of nitrogen doping, carbon doping, sulfur doping, metal and oxide modification.

6. The method for preparing a composite positive electrode sheet according to claim 1, characterized in that: The sulfide solid electrolyte is a binary sulfide electrolyte and / or a ternary sulfide solid electrolyte.

7. The method for preparing a composite positive electrode sheet according to claim 1, characterized in that: The coating thickness on the surface of the positive electrode current collector is 150 μm-500 μm.

8. The method for preparing a composite positive electrode sheet according to claim 1, characterized in that: The polar solvent is one of dimethyl sulfoxide, acetonitrile, formamide, trifluoroacetic acid, DMF, hexamethylphosphoramide, methanol, acetic acid, ethanol, isopropanol, pyridine, tetramethylethylenediamine, acetone, triethylamine, n-butanol, dioxane, tetrahydrofuran, and methyl formate.

9. The method for preparing a micron-sized silicon particle composite negative electrode sheet according to claim 1, characterized in that: The mesocrystalline anatase titanium dioxide is prepared by the following preparation method: a titanium source is dissolved in a 1 mol / L-3 mol / L hydrochloric acid solution, the volume ratio of the titanium source to the hydrochloric acid is 1-3:4-10, the mixture is stirred at 40°C-100°C for 40h-60h, and a white product is obtained by centrifugation. The white product is washed with deionized water to remove residual inorganic ions, and the white product is vacuum dried at 80°C-120°C for 12h-36h, and finally calcined in air at 400°C-500°C for 12h-24h to obtain a mesocrystalline anatase titanium dioxide powder.

10. A solid-state battery, characterized in that: The invention comprises a composite negative electrode sheet, a composite solid electrolyte membrane and a composite positive electrode sheet prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of current collector for all-solid-state battery and application of current collector in battery

    CN114551893A

  • Coated modified high-nickel ternary positive electrode material, preparation method thereof and lithium ion battery

    CN114784248A

  • Mixed double-conductor coated positive electrode material, preparation method thereof and solid-state battery