Secondary battery, preparation method of secondary battery, positive pole piece and preparation method of positive pole piece
By using lithium iron phosphate positive electrode material, Li2NiO2 and Li5FeO4 in lithium iron phosphate batteries, adjusting the material ratio and parameters, the problem that the existing technology cannot simultaneously improve the energy density and cycle life is solved, and high energy density and good cycle performance are achieved. Battery design improves safety.
Patent Information
- Application Number
- CN202411006069.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-15
AI Technical Summary
The existing positive electrode lithium supplement technology cannot simultaneously improve the energy density and cycle life of lithium iron phosphate batteries, and there are safety hazards and material stability problems.
Lithium iron phosphate positive electrode material, Li2NiO2 and Li5FeO4 are used as positive electrode active materials, and a battery with high energy density and good cycle performance is formed by adjusting the material ratio and parameters.
It significantly improves the energy density and circulation performance of lithium iron phosphate batteries, improves safety, and takes into account the improvement of energy density and circulation performance.
Smart Images

Figure BDA0004963043180000021 
Figure BDA0004963043180000031 
Figure BDA0004963043180000051
Abstract
Description
[0001] This application is a divisional application. The application date of the original application is April 17, 2024. The application number is CN202410458717.4, and the name is "Secondary battery and its preparation method, positive electrode sheet, negative electrode sheet and electrical device". Technical Field
[0002] The present invention relates to the technical field of lithium batteries, and in particular to a secondary battery and a preparation method thereof, a positive electrode sheet and a preparation method thereof. Background Art
[0003] The endurance of new energy vehicles has become an important factor restricting their development. At present, the mainstream power batteries are mainly ternary batteries and lithium iron phosphate batteries. Ternary batteries have high energy density, but relatively low economy and safety; lithium iron phosphate batteries have low energy density, but lower manufacturing costs, higher safety, and better cycle life. Therefore, in order to solve the endurance problem of new energy vehicles, improving the energy density and cycle life of lithium iron phosphate batteries is a more direct and feasible method.
[0004] With the advancement of battery design and process manufacturing technology, the internal space of the battery shell has been fully utilized. It is very difficult to increase the energy density through the internal space. At present, the energy density and cycle performance of the material are mainly improved by optimizing the positive electrode active material. The solid electrolyte interface (SEI) of the negative electrode of the lithium-ion battery consumes active lithium, resulting in a decrease in the initial capacity of the battery and a shortened life. A small amount of lithium source can be added before the battery charge and discharge cycle through lithium replenishment technology to improve the initial charge and discharge efficiency while replenishing the lithium loss during the cycle. At present, there are two main ways to replenish lithium: negative electrode lithium replenishment and positive electrode lithium replenishment.
[0005] Negative electrode lithium replenishment technology developed earlier, mainly lithium foil replenishment, lithium powder replenishment, chemical lithium replenishment, etc. Lithium foil replenishment uses the self-discharge mechanism. Through the existence of potential difference, in the presence of electrolyte, when the negative electrode material contacts the lithium metal foil, the electrons spontaneously move to the negative electrode, accompanied by Li + Embedding in the negative electrode. Lithium powder can be added directly to the surface of the negative electrode or added during the negative electrode slurry process. Negative electrode lithium replenishment has a high pre-lithiation capacity, but it has extremely high requirements for equipment and environment. The active lithium chemical reaction is highly active and there are serious safety hazards.
[0006] Positive electrode lithium replenishment technology usually adopts electrochemical method, by adding positive electrode lithium replenishment additives to lithium-ion batteries. During the battery charging process, the positive electrode lithium replenishment additives release active lithium to make up for the consumption of negative electrode SEI, and at the same time can improve the cycle life of the battery. Positive electrode lithium replenishment additives are highly safe, but a single positive electrode lithium replenishment additive still has many shortcomings. For example, Li5FeO4 has a high capacity, and the theoretical specific capacity can be as high as 867mAh / g, but its stability in the air environment is poor, and it produces oxygen when de-lithium; Li2NiO2 has excellent processing performance and does not produce gas when de-lithium, but its impedance is large, which will affect the battery's rate performance and cycle performance.
[0007] Therefore, the existing positive electrode lithium replenishment technology cannot achieve the effect of simultaneously improving the energy density and cycle life of lithium iron phosphate.
[0008] In view of this, the present invention is proposed. Summary of the invention
[0009] The object of the present invention is to provide a secondary battery and a preparation method thereof, a positive electrode plate and a preparation method thereof, aiming to simultaneously improve the energy density and cycle life of a lithium iron phosphate battery.
[0010] The present invention is achieved in that:
[0011] In a first aspect, the present invention provides a secondary battery, comprising a positive electrode plate, the positive electrode plate comprising a positive electrode active material and a positive electrode current collector; the positive electrode active material comprises a lithium iron phosphate positive electrode material, a first lithium supplement additive and a second lithium supplement additive, the first lithium supplement additive is Li2NiO2, and the second lithium supplement additive is Li5FeO4;
[0012] Secondary batteries have performance parameters β:
[0013]
[0014] Among them, the performance parameter β satisfies: 6<β<10;
[0015] A1 represents the mass proportion of lithium iron phosphate positive electrode material in the positive electrode active material;
[0016] A2 represents the mass proportion of the first lithium supplement additive in the positive electrode active material;
[0017] A3 represents the mass proportion of the second lithium supplement additive in the positive electrode active material;
[0018] A1, A2, A3 satisfy: A1+A2+A3=1, 80%≤A1≤99%, 0<A2≤15%, 0<A3≤15%;
[0019] M2 represents the initial charge specific capacity of the first lithium supplement additive, in mAh / g; the value range of M2 is 400mAh / g-500mAh / g;
[0020] M3 represents the first charge specific capacity of the second lithium supplement additive, in mAh / g; the value range of M3 is 650mAh / g-750mAh / g;
[0021] C represents the injection coefficient, and its unit is g / Ah. The value of C satisfies: C≤3.6g / Ah.
[0022] In an optional embodiment, the secondary battery further includes a negative electrode plate, the negative electrode plate includes a negative electrode active material and a negative electrode current collector;
[0023] Secondary batteries also have performance parameters α:
[0024]
[0025] Among them, the performance parameter α satisfies: 1.0≤α≤1.13;
[0026] M1 represents the initial charge specific capacity of the lithium iron phosphate cathode material, in mAh / g; the value range of M1 is 150mAh / g-170mAh / g;
[0027] M4 represents the initial charge specific capacity of the negative electrode active material, in mAh / g; the value range of M4 is 350mAh / g-400mAh / g;
[0028] X represents the amount of positive electrode active material on the positive electrode current collector, in mg / cm 2 ; The value of X is 17 mg / cm 2 -32 mg / cm 2 ;
[0029] Y represents the amount of negative electrode active material on the negative electrode current collector, in mg / cm 2 ; The value range of Y is 5mg / cm 2 -20mg / cm 2 ;
[0030] Preferably, the negative electrode active material is graphite;
[0031] Preferably, the values of M1, M2, M3 and M4 are all determined under the condition that the discharge voltage range of the secondary battery is 2.0-4.4V;
[0032] Preferably, 88%≤A1≤99%, 0<A2≤10%, and 0<A3≤10%.
[0033] In an optional embodiment, when preparing the positive electrode sheet, the materials coated on the positive electrode current collector are collectively referred to as the positive electrode total material, and the mass proportion of the positive electrode active material in the positive electrode total material is 92%-99%; the remaining components of the positive electrode total material include a conductive agent, a binder and a dispersant;
[0034] And / or, when preparing the negative electrode plate, the materials coated on the negative electrode collector are collectively referred to as the negative electrode total material, and the mass proportion of the negative electrode active material in the negative electrode total material is 85%-99%; the remaining components in the negative electrode total material include a conductive agent, a binder and a dispersant; wherein the negative electrode collector is selected from at least one of copper foil and composite copper foil, and the thickness of the negative electrode collector is 1μm-20μm.
[0035] In an optional embodiment, the secondary battery further comprises a separator, the separator comprises a substrate and a coating attached to the substrate, the thickness of the substrate is 5 μm-20 μm, and the thickness of the coating is 1 μm-6 μm;
[0036] The substrate is selected from at least one of polypropylene and polyethylene; and the coating is a ceramic material.
[0037] In an optional embodiment, the doping element in the lithium iron phosphate positive electrode material is selected from at least one of Ti, Al, Mg, V, Ni and Mn; and the content of the doping element is less than 5000 ppm.
[0038] And / or, the doping element of the first lithium supplement additive Li2NiO2 is selected from at least one of Ti, Al, Co and Mn;
[0039] And / or, the doping element of the second lithium supplementing additive Li5FeO4 is selected from at least one of Mn, Cu, Mo, Al, Ti, Mg, Zr and Zn;
[0040] Among them, the content of doping elements in the first lithium supplement additive Li2NiO2 is less than 5000ppm; the content of doping elements in the second lithium supplement additive Li5FeO4 is less than 5000ppm.
[0041] In an optional embodiment, the surface of the second lithium supplement additive is coated with a carbon layer, and the mass fraction of carbon in the second lithium supplement additive is 0.2-5.0%;
[0042] Preferably, the mass fraction of carbon in the second lithium supplementing additive is 0.5%-3.0%.
[0043] In a second aspect, the present invention further provides a method for preparing a secondary battery in any of the above embodiments, comprising: defining a performance parameter β during the preparation of the secondary battery, and ensuring that the performance parameter β meets the requirements.
[0044] In a third aspect, the present invention further provides a positive electrode plate, comprising a positive electrode active material and a positive electrode current collector, wherein the positive electrode active material comprises a lithium iron phosphate positive electrode material, a first lithium supplement additive and a second lithium supplement additive, wherein the first lithium supplement additive is Li2NiO2 and the second lithium supplement additive is Li5FeO4; the positive electrode plate is used to manufacture a secondary battery;
[0045] Secondary batteries have performance parameters β:
[0046]
[0047] Among them, the performance parameter β satisfies: 6<β<10;
[0048] A1 represents the mass proportion of lithium iron phosphate positive electrode material in the positive electrode active material;
[0049] A2 represents the mass proportion of the first lithium supplement additive in the positive electrode active material;
[0050] A3 represents the mass proportion of the second lithium supplement additive in the positive electrode active material;
[0051] A1, A2, A3 satisfy: A1+A2+A3=1, 80%≤A1≤99%, 0<A2≤15%, 0<A3≤15%;
[0052] M2 represents the initial charge specific capacity of the first lithium supplement additive, in mAh / g; the value range of M2 is 400mAh / g-500mAh / g;
[0053] M3 represents the first charge specific capacity of the second lithium supplement additive, in mAh / g; the value range of M3 is 650mAh / g-750mAh / g;
[0054] C represents the injection coefficient, and its unit is g / Ah. The value of C satisfies: C≤3.6g / Ah.
[0055] In an optional embodiment, the secondary battery further includes a negative electrode plate, the negative electrode plate includes a negative electrode active material and a negative electrode current collector;
[0056] Secondary batteries also have performance parameters α:
[0057]
[0058] Among them, the performance parameter α satisfies: 1.0≤α≤1.13;
[0059] M1 represents the initial charge specific capacity of the lithium iron phosphate cathode material, in mAh / g; the value range of M1 is 150mAh / g-170mAh / g;
[0060] M4 represents the initial charge specific capacity of the negative electrode active material, in mAh / g; the value range of M4 is 350mAh / g-400mAh / g;
[0061] X represents the amount of positive electrode active material on the positive electrode current collector, in mg / cm 2 ; The value of X is 17 mg / cm 2 -32 mg / cm 2 ;
[0062] Y represents the amount of negative electrode active material on the negative electrode current collector, in mg / cm 2 ; The value range of Y is 5mg / cm 2 -20mg / cm 2 ;
[0063] Preferably, the negative electrode active material is graphite;
[0064] Preferably, the values of M1, M2, M3 and M4 are all determined under the condition that the discharge voltage range of the secondary battery is 2.0-4.4V;
[0065] Preferably, 88%≤A1≤99%, 0<A2≤10%, and 0<A3≤10%.
[0066] In a fourth aspect, the present invention further provides a method for preparing a positive electrode sheet in any of the above-mentioned embodiments, wherein a performance parameter β is defined during the preparation of the positive electrode sheet, and the performance parameter β meets the requirements.
[0067] The present invention has the following beneficial effects: by using lithium iron phosphate positive electrode material, Li2NiO2 and Li5FeO4 as positive electrode active materials, by adjusting the blending ratio, limiting the blending ratio, the gram capacity of the active material and the injection coefficient and other parameters to meet specific relationships, the gram capacity and cycle performance of the lithium iron phosphate battery can be significantly improved, so that the lithium-ion battery can have the advantages of higher energy density, better cycle performance, higher safety and the like at the same time. DETAILED DESCRIPTION
[0068] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0069] An embodiment of the present invention provides a secondary battery, including a positive electrode plate, a negative electrode plate and a separator. According to the parameters of the positive electrode plate, the negative electrode plate and the separator, a first performance parameter α and a second performance parameter β are defined. By adjusting the expressions of the first performance parameter α and the second performance parameter β, the first performance parameter α and the second performance parameter β are made to satisfy a specific value range, so that the secondary battery has the advantages of high energy density and good cycle performance.
[0070] Specifically, the positive electrode plate includes a positive electrode active material and a positive electrode current collector, and the positive electrode active material is the main component of the positive electrode active coating formed on the positive electrode current collector; the negative electrode plate includes a negative electrode active material and a negative electrode current collector, and the negative electrode active material is the main component of the negative electrode active coating formed on the negative electrode current collector. Among them, the method for regulating the value of the first performance parameter α and the second performance parameter β provided in the embodiment of the present invention is for lithium iron phosphate batteries. Specifically, the positive electrode active material includes a lithium iron phosphate positive electrode material, a first lithium supplement additive and a second lithium supplement additive, the first lithium supplement additive is Li2NiO2, and the second lithium supplement additive is Li5FeO4. By adding Li2NiO2 and Li5FeO4 dual lithium supplement materials, the disadvantages of a single lithium supplement material can be compensated, which is conducive to the preparation of a battery with high energy density and good cycle performance.
[0071] The expressions of the first performance parameter α and the second performance parameter β are as follows:
[0072]
[0073] The first performance parameter α satisfies: 1.0≤α≤1.13, and the second performance parameter β satisfies: 6<β<10. By adjusting the values of α and β, the inventors found that within this range, the battery can take into account both energy density and cycle performance.
[0074] Specifically, the value of the first performance parameter α can be 1.00, 1.02, 1.05, 1.08, 1.10, 1.13, etc., and the value of the second performance parameter β can be 6.0, 7.0, 8.0, 9.0, 10.0, etc.
[0075] In the expressions of the first performance parameter α and the second performance parameter β, the meanings of the parameters are as follows:
[0076] A1 represents the mass proportion of lithium iron phosphate positive electrode material in the positive electrode active material. When it is substituted into the expression, it is substituted into the percentage, such as 90%, which is 0.9.
[0077] A2 represents the mass proportion of the first lithium supplement additive in the positive electrode active material, and when it is substituted into the expression, it is also substituted into a percentage, such as 5%, that is, 0.05.
[0078] A3 represents the mass proportion of the second lithium supplement additive in the positive electrode active material, and when it is substituted into the expression, it is also substituted into a percentage, such as 5%, that is, 0.05.
[0079] In some embodiments, A1+A2+A3=1, and under the premise that the sum of the three equals 1, 80%≤A1≤99%, 0<A2≤15%, 0<A3≤15%; preferably, 88%≤A1≤99%, 0<A2≤10%, 0<A3≤10%. Specifically, the value of A1 can be 80%, 82%, 84%, 86%, 88%, 90%, 92%, 95%, 97%, 99%, etc., and the value of A2 can be 0.1%, 0.5%, 0.7%, 1.0%, 2.0%, 3.0%, 4.0%, 5.0%, 6.0%, 7.0%, 8.0%, 9.0%, 10.0%, 11.0%, 12.0%, 13.0%, 14.0%, 15.0%, 16.0%, 17.0%, 18.0%, 19.0%, 20.0%, 21.0%, 22.0%, 23.0%, 24.0%, 25.0%, 26.0%, 27.0%, 28.0%, 29.0%, 30.0%, 31.0%, 32.0%, 33.0%, 34.0%, 35.0%, 36.0%, 37.0%, 38.0%, 39.0%, 40.0%, 41.0%, 42.0%, 43.0%, 44.0%, 45.0%, 46.0%, 47.0%, 48.0%, 49.0%, 50.0%, 51.0%, 52.0%, 53.0%, 54.0%, 55.0%, 56.0%, 57.0%, 58.0%, 59.0%, %, 12.0%, 13.0%, 14.0%, 15.0%, etc., the value of A3 can be 0.1%, 0.5%, 0.7%, 1.0%, 2.0%, 3.0%, 4.0%, 5.0%, 6.0%, 7.0%, 8.0%, 9.0%, 10.0%, 11.0%, 12.0%, 13.0%, 14.0%, 15.0%, etc.
[0080] M1 represents the first charge specific capacity of the lithium iron phosphate positive electrode material, in mAh / g. Under the condition of the secondary battery discharge voltage range of 2.0-4.4V, its value is relatively fixed, generally 150mAh / g-170mAh / g, preferably 158mAh / g-165mAh / g, such as 150mAh / g, 160mAh / g, 170mAh / g, etc.
[0081] M2 represents the first charging specific capacity of the first lithium supplement additive Li2NiO2, and the unit is mAh / g. Since the material is fixed, under the condition of the secondary battery discharge voltage range of 2.0-4.4V, its value is also relatively fixed, generally 400mAh / g-500mAh / g, preferably 400mAh / g-440mAh / g, such as 400mAh / g, 420mAh / g, 430mAh / g, 440mAh / g, 450mAh / g, 480mAh / g, 500mAh / g, etc.
[0082] M3 represents the first charge specific capacity of the second lithium supplement additive Li5FeO4, in units of mAh / g. Since the material is fixed, under the condition of the secondary battery discharge voltage range of 2.0-4.4V, its value is also relatively fixed, generally 650mAh / g-750mAh / g, preferably 690mAh / g-710mAh / g, such as 650mAh / g, 680mAh / g, 700mAh / g, 750mAh / g.
[0083] M4 represents the initial charge specific capacity of the negative electrode active material, in mAh / g, and the value of different materials is slightly different. The value range of M4 is 350mAh / g-400mAh / g; preferably 370mAh / g-380mAh / g. For example, the negative electrode active material can be a graphite material, specifically artificial graphite or natural graphite, or a mixture of artificial graphite and natural graphite. The initial charge specific capacity M4 of graphite is 375mAh / g.
[0084] C represents the filling coefficient, which is a fixed constant determined when designing the battery. It is the ratio of the amount of electrolyte filled in the battery to the designed discharge capacity of the battery. The calculation formula of the electrolyte filling coefficient = filling amount / capacity, and the unit is g / Ah.
[0085] In some embodiments, the value of C satisfies: C≤3.6g / Ah, preferably 2.9g / Ah-3.5g / Ah, such as 2.9g / Ah, 3.0g / Ah, 3.1g / Ah, 3.2g / Ah, 3.3g / Ah, 3.4g / Ah, 3.5g / Ah, etc.
[0086] X represents the amount of positive electrode active material on the positive electrode current collector, in mg / cm 2 That is, X represents the amount of positive electrode active material (including lithium iron phosphate positive electrode material, the first lithium supplement additive and the second lithium supplement additive) contained in each square centimeter of positive electrode current collector, and the value of X is 17 mg / cm 2 -32mg / cm 2 , such as 17 mg / cm 2 , 20mg / cm 2 , 25mg / cm 2 、30mg / cm 2 、32mg / cm 2 wait.
[0087] Specifically, when preparing the positive electrode sheet, the materials coated on the positive electrode current collector are collectively referred to as the total positive electrode material. The mass proportion of the positive electrode active material in the total positive electrode material is 92%-99%, and the remaining components are conductive agents (such as conductive carbon black), binders (such as polyvinylidene fluoride), and dispersants (such as N-methylpyrrolidone). In other words, the single-sided coating surface density of the positive electrode active material is X = a*X 正极总材料 , the value of a is 92%-99%.
[0088] Specifically, LiFePO4 is the main component of the lithium iron phosphate positive electrode material, and may also contain a small amount of doping elements, the doping elements are selected from at least one of Ti, Al, Mg, V, Ni and Mn, and may be any one or more of the above, and the content of each doping element is less than 5000ppm.
[0089] Specifically, the first lithium supplement additive Li2NiO2 may also contain a small amount of doping elements, the doping element is selected from at least one of Ti, Al, Co and Mn, and may be any one or more of the above, and the doping amount is not limited and may be less than 5000ppm.
[0090] Specifically, the second lithium supplement additive Li5FeO4 may also contain a small amount of doping elements, and the doping elements are selected from at least one of Mn, Cu, Mo, Al, Ti, Mg, Zr and Zn, and may be any one or more of the above. The surface of the second lithium supplement additive may also be coated with a carbon layer, and the mass fraction of carbon in the second lithium supplement additive is 0.2-5.0%, preferably 0.5%-3.0%, such as 0.2%, 0.5%, 1.0%, 2.0%, 3.0%, 4.0%, 5.0%, etc.
[0091] Y represents the amount of negative electrode active material on the negative electrode current collector, in mg / cm 2 ; That is, Y represents the amount of negative electrode active material (such as graphite) contained in each square centimeter of negative electrode current collector. The value range of Y is 5 mg / cm 2 -20mg / cm 2 , preferably 8 mg / cm 2 -15 mg / cm 2 , such as 5 mg / cm 2 , 8mg / cm 2 、10mg / cm 2 , 12mg / cm 2 、15mg / cm 2 、18mg / cm 2 , 20mg / cm 2 wait.
[0092] Specifically, the materials attached to the negative electrode current collector are collectively referred to as the total negative electrode materials. The mass proportion of the negative electrode active materials in the total negative electrode materials is 85%-99%, preferably 92%-99%, and the remaining components are conductive agents (such as conductive carbon black), binders (such as polyvinylidene fluoride), and dispersants (such as N-methylpyrrolidone). In other words, the surface density of the single-sided coating of the negative electrode active material Y = b*Y 负极总材料 , b is the proportion of negative electrode active material in the total negative electrode material, and the value is 92%-99%.
[0093] In some embodiments, the negative electrode current collector is selected from at least one of copper foil and composite copper foil, and the thickness of the negative electrode current collector is 1 μm-20 μm, preferably 4 μm-10 μm, such as 1 μm, 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, 15 μm, 20 μm, etc.
[0094] In some embodiments, the diaphragm includes a substrate and a coating attached to the substrate, the thickness of the substrate is 5 μm-20 μm (such as 5 μm, 10 μm, 15 μm, 20 μm, etc.), and the thickness of the coating is 1 μm-6 μm (such as 1 μm, 2 μm, 4 μm, 6 μm, etc.). The substrate is selected from at least one of polypropylene (PP) and polyethylene (PE), and can be PP, PE, or a composite material of PP / PE. The coating is a ceramic material, and the specific material is not limited, mainly alumina or a binder, or a composite material of alumina and a binder.
[0095] It should be noted that the first performance parameter α represents the excess ratio of the charging capacity of the negative electrode sheet relative to the charging capacity of the positive electrode sheet. If the α value is too low, there is a risk of lithium deposition on the negative electrode sheet during charging; if the α value is too high, the amount of dressing on the negative electrode sheet is too large, and the negative electrode sheet needs to consume more active lithium when forming the SEI film (solid electrolyte interface film), which is not conducive to the use of the positive electrode material capacity and will reduce the energy density of the battery.
[0096] It should be noted that the number of cells of the secondary battery provided in the embodiment of the present invention is not limited, and the secondary battery can be in the form of a battery pack.
[0097] An embodiment of the present invention provides a method for preparing a secondary battery. During the preparation of the secondary battery, a first performance parameter α and a second performance parameter β are defined, and the first performance parameter α and the second performance parameter β meet requirements.
[0098] Specifically, during the preparation process, the values of A1, A2, A3, M2, and M3, as well as the surface density of the active material coating and the injection coefficient when preparing the positive and negative electrode sheets are regulated. By regulating the value ranges of the above parameters and constructing expressions for the first performance parameter α and the second performance parameter β, the values of α and β are made to meet a specific range. The inventors found that this method can better balance the relationship between energy density and cycle life, so that the energy density of the battery cell is effectively improved, and the cycle is maintained at a good level.
[0099] The embodiment of the present invention further provides a positive electrode plate, the positive electrode plate includes a positive electrode active material and a positive electrode current collector, the positive electrode active material includes a lithium iron phosphate positive electrode material, a first lithium supplement additive and a second lithium supplement additive, the first lithium supplement additive is Li2NiO2, and the second lithium supplement additive is Li5FeO4; the positive electrode plate is used to make a secondary battery, the secondary battery includes a positive electrode plate, a negative electrode plate and a separator, the negative electrode plate includes a negative electrode active material and a negative electrode current collector;
[0100] The secondary battery has a first performance parameter α and a second performance parameter β, and satisfies the following relationship:
[0101]
[0102] Wherein, the first performance parameter α satisfies: 1.0≤α≤1.13, and the second performance parameter β satisfies: 6<β<10;
[0103] In the formula, A1 represents the mass proportion of lithium iron phosphate positive electrode material in the positive electrode active material;
[0104] A2 represents the mass proportion of the first lithium supplement additive in the positive electrode active material;
[0105] A3 represents the mass proportion of the second lithium supplement additive in the positive electrode active material;
[0106] M1 represents the first charge specific capacity of lithium iron phosphate positive electrode material, in mAh / g;
[0107] M2 represents the initial charge specific capacity of the first lithium supplement additive, in mAh / g;
[0108] M3 represents the first charge specific capacity of the second lithium supplement additive, in mAh / g;
[0109] M4 represents the first charge specific capacity of the negative electrode active material, in mAh / g;
[0110] X represents the amount of positive electrode active material on the positive electrode current collector, in mg / cm 2 ;
[0111] Y represents the amount of negative electrode active material on the negative electrode current collector, in mg / cm 2 ;
[0112] C represents the filling coefficient, and its unit is g / Ah.
[0113] The value range of each parameter can be found in the parameter specification above and will not be repeated here.
[0114] The embodiment of the present invention further provides a negative electrode plate, the negative electrode plate includes a negative electrode active material and a negative electrode current collector, the negative electrode plate is used to make a secondary battery, the secondary battery includes a positive electrode plate, a negative electrode plate and a separator, the positive electrode plate includes a positive electrode active material and a positive electrode current collector, the positive electrode active material includes a lithium iron phosphate positive electrode material, a first lithium supplement additive and a second lithium supplement additive, the first lithium supplement additive is Li2NiO2, and the second lithium supplement additive is Li5FeO4;
[0115] The secondary battery has a first performance parameter α and a second performance parameter β, and satisfies the following relationship:
[0116]
[0117] Wherein, the first performance parameter α satisfies: 1.0≤α≤1.13, and the second performance parameter β satisfies: 6<β<10;
[0118] In the formula, A1 represents the mass proportion of lithium iron phosphate positive electrode material in the positive electrode active material;
[0119] A2 represents the mass proportion of the first lithium supplement additive in the positive electrode active material;
[0120] A3 represents the mass proportion of the second lithium supplement additive in the positive electrode active material;
[0121] M1 represents the first charge specific capacity of lithium iron phosphate positive electrode material, in mAh / g;
[0122] M2 represents the initial charge specific capacity of the first lithium supplement additive, in mAh / g;
[0123] M3 represents the first charge specific capacity of the second lithium supplement additive, in mAh / g;
[0124] M4 represents the first charge specific capacity of the negative electrode active material, in mAh / g;
[0125] X represents the amount of positive electrode active material on the positive electrode current collector, in mg / cm 2 ;
[0126] Y represents the amount of negative electrode active material on the negative electrode current collector, in mg / cm 2 ;
[0127] C represents the filling coefficient, and its unit is g / Ah.
[0128] The value range of each parameter can be found in the parameter specification above and will not be repeated here.
[0129] The embodiment of the present invention further provides an electrical device, including the above-mentioned secondary battery, and may also include an electrical appliance, and the secondary battery is used to power the electrical appliance.
[0130] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0131] Example 1
[0132] This embodiment provides a method for preparing a secondary battery. During the preparation process, expressions for a first performance parameter α and a second performance parameter β are constructed so that the parameter values meet the requirements. The specific steps are as follows:
[0133] (1) Preparation of positive electrode sheet
[0134] Take the positive electrode active material lithium iron phosphate LiFePO4, take the lithium supplement additive Li2NiO2, the doping element is Al, and the doping element content is 500ppm. Take the lithium supplement additive Li5FeO4, the doping elements are Al and Ti, and the total doping element content is 8000ppm. The value of M1 is 160mAh / g, the value of M2 is 420mAh / g, and the value of M3 is 700mAh / g.
[0135] Lithium iron phosphate, Li2NiO2 and Li5FeO4 are used as positive electrode active materials, and the mass proportions of lithium iron phosphate, Li2NiO2 and Li5FeO4 in the positive electrode active materials are controlled to be 95.5%, 0.5% and 4% respectively.
[0136] The positive electrode active material, conductive carbon black, and binder polyvinylidene fluoride were mixed in a mass ratio of 97:1:2, and a dispersant polyvinyl pyrrolidone was added to form a positive electrode slurry with a solid content of 57%-61%. The positive electrode slurry was evenly coated on the front and back sides of the positive electrode collector, and the coating amount of the positive electrode active material on the positive electrode collector was controlled to be 24.6 mg / cm 2 After drying, a coating is formed, and the electrode sheet is compacted by roller pressing to obtain a positive electrode sheet, and the compaction density PD is controlled to be 2.55g / cm 3 Among them, the positive electrode current collector is an aluminum foil with a thickness of 13 μm.
[0137] (2) Negative electrode sheet preparation
[0138] The negative electrode active material artificial graphite, conductive agent conductive carbon black, binder styrene butadiene rubber SBR, and dispersant sodium carboxymethyl cellulose CMC were mixed in a mass ratio of 95:1:2:2, and deionized water as a dispersant was added to form a negative electrode slurry with a solid content of 48%-53%. The negative electrode slurry was evenly coated on the front and back sides of the negative electrode current collector, and the coating amount Y of the negative electrode active material on the negative electrode current collector was controlled to be 13.2 mg / cm 2 The coated electrode sheet is obtained by heating and drying, and then the electrode sheet is compacted by roller pressing to obtain the negative electrode sheet. The first charge specific capacity M4 of the negative electrode active material is 375 mAh / g, and the negative electrode current collector is a copper foil with a thickness of 6 μm.
[0139] (3) Preparation of isolation membrane
[0140] A nano-alumina coating is applied on both sides of the diaphragm, and the solvent is removed by drying in a vacuum oven. The thickness of the PE base film is 7 μm, and the thickness of the coating is 3 μm.
[0141] (4) Assembly
[0142] The positive and negative electrode sheets and separators obtained above are stacked in a Z-shape in the order of "separator-negative electrode sheet-separator-positive electrode sheet" to ensure that the positive electrode sheet is completely in the middle of the negative electrode sheet. After stacking, hot pressing-ear welding-packaging-baking are carried out to control the total water content of the positive and negative electrode sheets and separators after baking to be 250ppm, and the electrolyte is injected to control the injection coefficient C to be 3.5g / Ah.
[0143] This embodiment also provides a secondary battery prepared by the above preparation method.
[0144] Embodiment 2-5
[0145] The difference between Examples 2-5 and Example 1 is that the parameter values are different. The parameters with different values are listed in Table 1.
[0146] Comparative Example 1-2
[0147] The difference between Comparative Example 1-2 and Example 1 is that the parameter values are different. The parameters with different values are listed in Table 1.
[0148] Table 1 Parameter control of the preparation process of the embodiment and the comparative example and the performance of the secondary battery obtained
[0149]
[0150] It can be seen from Table 1 that the embodiment of the present invention can take into account both energy density and cycle performance by controlling 1.0≤α≤1.13, 6<β<10. Exceeding the above range will result in unsatisfactory energy density or poor life.
[0151] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A secondary battery, characterized in that: It includes a positive electrode plate, wherein the positive electrode plate includes a positive electrode active material and a positive electrode current collector; the positive electrode active material includes a lithium iron phosphate positive electrode material, a first lithium supplement additive and a second lithium supplement additive, wherein the first lithium supplement additive is Li2NiO2, and the second lithium supplement additive is Li5FeO4; The secondary battery has a performance parameter β: Wherein, the performance parameter β satisfies: 6<β<10; A1 represents the mass proportion of the lithium iron phosphate positive electrode material in the positive electrode active material; A2 represents the mass proportion of the first lithium supplement additive in the positive electrode active material; A3 represents the mass proportion of the second lithium supplement additive in the positive electrode active material; A1, A2, A3 satisfy: A1+A2+A3=1, 80%≤A1≤99%, 0<A2≤15%, 0<A3≤15%; M2 represents the initial charge specific capacity of the first lithium supplement additive, in mAh / g; the value range of M2 is 400mAh / g-500mAh / g; M3 represents the first charge specific capacity of the second lithium supplement additive, in mAh / g; the value range of M3 is 650mAh / g-750mAh / g; C represents the injection coefficient, and its unit is g / Ah. The value of C satisfies: C≤3.6g / Ah.
2. The secondary battery according to claim 1, characterized in that: The secondary battery further comprises a negative electrode plate, wherein the negative electrode plate comprises a negative electrode active material and a negative electrode current collector; The secondary battery also has a performance parameter α: Wherein, the performance parameter α satisfies: 1.0≤α≤1.13; M1 represents the initial charge specific capacity of the lithium iron phosphate positive electrode material, in mAh / g; the value range of M1 is 150mAh / g-170mAh / g; M4 represents the initial charge specific capacity of the negative electrode active material, in mAh / g; the value range of M4 is 350mAh / g-400mAh / g; X represents the amount of the positive electrode active material applied to the positive electrode current collector, in mg / cm 2 ; The value of X is 17 mg / cm 2 -32 mg / cm 2 ; Y represents the amount of the negative electrode active material applied to the negative electrode current collector, in mg / cm 2 ; The value range of Y is 5mg / cm 2 -20mg / cm 2 ; Preferably, the negative electrode active material is graphite; Preferably, the values of M1, M2, M3 and M4 are all determined under the condition that the discharge voltage range of the secondary battery is 2.0-4.4V; Preferably, 88%≤A1≤99%, 0<A2≤10%, and 0<A3≤10%.
3. The secondary battery according to claim 2, characterized in that: When preparing the positive electrode sheet, the materials coated on the positive electrode current collector are collectively referred to as positive electrode total materials, and the mass proportion of the positive electrode active material in the positive electrode total materials is 92%-99%; the remaining components of the positive electrode total materials include a conductive agent, a binder and a dispersant; And / or, when preparing the negative electrode plate, the materials coated on the negative electrode collector are collectively referred to as negative electrode total materials, and the mass proportion of the negative electrode active material in the negative electrode total materials is 85%-99%; the remaining components in the negative electrode total materials include conductive agents, binders and dispersants; wherein the negative electrode collector is selected from at least one of copper foil and composite copper foil, and the thickness of the negative electrode collector is 1μm-20μm.
4. The secondary battery according to any one of claims 1 to 3, characterized in that: The secondary battery further comprises a separator, wherein the separator comprises a substrate and a coating layer attached to the substrate, wherein the thickness of the substrate is 5 μm-20 μm, and the thickness of the coating layer is 1 μm-6 μm; The substrate is selected from at least one of polypropylene and polyethylene; and the coating is a ceramic material.
5. The secondary battery according to any one of claims 1 to 3, characterized in that: The doping element in the lithium iron phosphate positive electrode material is selected from at least one of Ti, Al, Mg, V, Ni and Mn; and the content of the doping element is less than 5000 ppm. And / or, the doping element of the first lithium supplement additive Li2NiO2 is selected from at least one of Ti, Al, Co and Mn; And / or, the doping element of the second lithium supplementing additive Li5FeO4 is selected from at least one of Mn, Cu, Mo, Al, Ti, Mg, Zr and Zn; Among them, the content of doping elements in the first lithium supplement additive Li2NiO2 is less than 5000ppm; the content of doping elements in the second lithium supplement additive Li5FeO4 is less than 5000ppm.
6. The secondary battery according to claim 5, characterized in that: The surface of the second lithium supplement additive is coated with a carbon layer, and the mass fraction of carbon in the second lithium supplement additive is 0.2-5.0%; Preferably, the mass fraction of carbon in the second lithium supplementing additive is 0.5%-3.0%.
7. A method for preparing a secondary battery according to any one of claims 1 to 6, characterized in that: The method comprises: defining a performance parameter β during the process of preparing the secondary battery, and making the performance parameter β meet the requirements.
8. A positive electrode sheet, characterized in that: It comprises a positive electrode active material and a positive electrode current collector, wherein the positive electrode active material comprises a lithium iron phosphate positive electrode material, a first lithium supplement additive and a second lithium supplement additive, wherein the first lithium supplement additive is Li2NiO2 and the second lithium supplement additive is Li5FeO4; the positive electrode plate is used to make a secondary battery; The secondary battery has a performance parameter β: Wherein, the performance parameter β satisfies: 6<β<10; A1 represents the mass proportion of the lithium iron phosphate positive electrode material in the positive electrode active material; A2 represents the mass proportion of the first lithium supplement additive in the positive electrode active material; A3 represents the mass proportion of the second lithium supplement additive in the positive electrode active material; A1, A2, A3 satisfy: A1+A2+A3=1, 80%≤A1≤99%, 0<A2≤15%, 0<A3≤15%; M2 represents the initial charge specific capacity of the first lithium supplement additive, in mAh / g; the value range of M2 is 400mAh / g-500mAh / g; M3 represents the first charge specific capacity of the second lithium supplement additive, in mAh / g; the value range of M3 is 650mAh / g-750mAh / g; C represents the injection coefficient, and its unit is g / Ah. The value of C satisfies: C≤3.6g / Ah.
9. The positive electrode sheet according to claim 8, characterized in that: The secondary battery further comprises a negative electrode plate, wherein the negative electrode plate comprises a negative electrode active material and a negative electrode current collector; The secondary battery also has a performance parameter α: Wherein, the performance parameter α satisfies: 1.0≤α≤1.13; M1 represents the initial charge specific capacity of the lithium iron phosphate positive electrode material, in mAh / g; the value range of M1 is 150mAh / g-170mAh / g; M4 represents the initial charge specific capacity of the negative electrode active material, in mAh / g; the value range of M4 is 350mAh / g-400mAh / g; X represents the amount of the positive electrode active material applied to the positive electrode current collector, in mg / cm 2 ; The value of X is 17 mg / cm 2 -32 mg / cm 2 ; Y represents the amount of the negative electrode active material applied to the negative electrode current collector, in mg / cm 2 ; The value range of Y is 5mg / cm 2 -20mg / cm 2 ; Preferably, the negative electrode active material is graphite; Preferably, the values of M1, M2, M3 and M4 are all determined under the condition that the discharge voltage range of the secondary battery is 2.0-4.4V; Preferably, 88%≤A1≤99%, 0<A2≤10%, and 0<A3≤10%.
10. A method for preparing the positive electrode sheet according to claim 8 or 9, characterized in that: In the process of preparing the positive electrode plate, a performance parameter β is defined, and the performance parameter β meets the requirements.