Lithium composite oxide

By controlling the molar fraction and particle size ratio of nickel, a bimodal structure with multiple particles and single particles is formed, which solves the problem of deterioration in the life characteristics of the positive electrode active substances with nickel-rich lithium composite oxides at high temperatures, and realizes battery capacity and Improvement of lifespan.

CN118970029APending Publication Date: 2024-11-15ECOPRO BM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411030254.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-10-31
Filing Date
2020-10-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Nickel-rich lithium composite oxide positive electrode active material has deteriorated life characteristics at high temperatures and increased structural instability, resulting in a problem of reduced battery capacity and electrolyte depletion.

Method used

By controlling the mole fraction and particle size ratio of nickel in lithium composite oxide, adjusting the half-maximum width range of the (104) peak of X-ray diffraction to form a bimodal structure with multiple particles and single particles mixed to stabilize the structure and improve the structure Battery life.

Benefits of technology

It effectively suppresses the generation of microcracks, improves the discharge capacity and life of the battery, and improves the storage characteristics and electromagnetic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970029A_ABST
    Figure CN118970029A_ABST
Patent Text Reader

Abstract

A lithium composite oxide according to an embodiment of the present invention contains a mixture of first particles obtained by aggregating n1 (n1 > 40) primary particles and second particles obtained by aggregating n2 (n2 < = 20) primary particles, the lithium composite oxide being represented by chemical formula 1 below, and having a peak width at half maximum FWHM (deg. The range of chemical formula (1, 2 [theta]) is represented by the following relational expression 1:-0.025 < = FWHM (104)-{0.04 + (x first particles-0.6) * 0.25} < = 0.025, and relational expression 2: FWHM (104) = {(FWHM chemical formula 1 power (104)-0.1 * second particle mass ratio) / first particle mass ratio}-FWHMSi power (220).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of a patent application with application number 202011183951.9, application date October 29, 2020, and invention name “Lithium Composite Oxide”. Technical Field

[0002] The present invention relates to a mixture of lithium composite oxides, and more specifically, to a lithium composite oxide that, when first particles and second particles having different numbers of aggregated primary particles are mixed, produces an effect of improving the life characteristics of a battery containing the lithium composite oxide of the present invention by maintaining a prescribed relationship between the range of the half-width (FWHM) value of the (104) peak of X-ray diffraction defined by a hexagonal lattice having an R-3m space group and the molar fraction of nickel in the lithium composite oxide and the mass ratio of the first particles and the second particles. Background Art

[0003] In order to meet the needs of various devices that are becoming smaller and more powerful, it is becoming increasingly important to make lithium batteries smaller and lighter, and to increase their energy density. In other words, high-voltage and high-capacity lithium batteries are becoming increasingly important.

[0004] Lithium composite oxides used as positive electrode active materials for lithium batteries, such as composite metal oxides such as LiCoO2, LiMn2O4, LiNiO2, and LiMnO2, are being studied. Among the above lithium composite oxides, LiCoO2 has excellent life characteristics and charge and discharge efficiency, and therefore is the most widely used. However, it has poor structural stability and is expensive due to the limited resources of cobalt used as a raw material, so there is a disadvantage of limited price competitiveness.

[0005] Lithium manganese oxides such as LiMnO2 and LiMn2O4 have the advantages of excellent thermal stability and low price, but have problems such as small capacity and poor high-temperature characteristics.

[0006] Furthermore, LiNiO2-based positive electrode active materials have battery characteristics of high discharge capacity, but are difficult to synthesize due to the cation mixing problem between lithium and transition metals, and therefore have serious problems in rate characteristics.

[0007] In order to improve the above-mentioned shortcomings, as secondary battery positive electrode active materials, the demand for nickel-rich systems with a nickel content of more than 60% is increasing. However, this nickel-rich system active material has the excellent advantage of high capacity, but as the nickel content increases, the structural instability caused by lithium / nickel cation mixing also increases, and there is a problem of rapid deterioration of life characteristics at room temperature and high temperature due to physical fracture of internal particles caused by micro-cracks and severe depletion of electrolytes. Summary of the invention

[0008] The generation of microcracks, which is the cause of the poor life of nickel-rich positive electrode active materials, is correlated with the size of the primary particles of the positive electrode active material. Specifically, the smaller the size of the primary particles, the more cracks (cracks) caused by repeated contraction / expansion of the particles are suppressed. However, if the size of the primary particles becomes smaller, there is a problem of reduced discharge capacity. In the case where the nickel content in the positive electrode active material increases, if the size of the primary particles becomes smaller, it leads to a deterioration of the life characteristics. Therefore, in order to improve the life characteristics of nickel-rich positive electrode active materials, it is necessary to consider the correlation between the nickel content, the size of the primary particles, and the discharge capacity.

[0009] In order to solve the problems of nickel-rich lithium composite oxides as described above, the purpose of the present invention is to provide a lithium composite oxide that improves life characteristics and capacity characteristics by adjusting the half-peak width to a specified range during X-ray diffraction (XRD) measurement in order to maintain a specified relationship with the molar fraction of nickel in the active material and the mass ratio of the first particle to the second particle.

[0010] In order to solve the above-mentioned problems, the lithium composite oxide of the embodiment of the present invention comprises a mixture of first particles formed by agglomeration of n1 (n1>40) primary particles and second particles formed by agglomeration of n2 (n2≤20) primary particles, the lithium composite oxide is represented by the following chemical formula 1, and the range of the half-peak width FWHM (deg., 2θ) of the peak in the X-ray diffraction peak (104) defined by the hexagonal lattice having the R-3m space group is represented by the following relationship 1:

[0011] Chemical formula 1: Li a Ni x Co y Mn z M 1-x-y-z O2

[0012] (In the above chemical formula 1, M is selected from the group consisting of B, Ba, Ce, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr and combinations thereof, 0.9≤a≤1.3, 0.6≤x≤1.0, 0.0≤y≤0.4, 0.0≤z≤0.4, 0.0≤1-xyz≤0.4)

[0013] Relationship 1: -0.025 ≤ FWHM (104) -{0.04+(x 第一粒子 -0.6)×0.25}≤0.025

[0014] (FWHM of the above relation 1 (104) It is expressed by the following relation 2)

[0015] Relation 2: FWHM (104) ={(FWHM 化学式1powder(104) -0.1×second particle mass ratio) / first particle mass ratio}-FWHM Si powder(220)

[0016] (In the above equation 2, FWHM 化学式1powder(104) represents the half maximum width of the (104) peak observed near 44.5° (2θ) in the X-ray diffraction measurement value of the lithium composite oxide). In addition, in the above relationship 2, FWHM Si powder(220) represents the half-value width of the (220) peak observed near 47.3° (2θ) in the X-ray diffraction measurement value of silicon (Si) powder. 第一粒子 =(xx 第二粒子 × second particle mass ratio) / first particle mass ratio, the above X 第二粒子 represents the nickel molar ratio of the second particle. Also, the mass ratio represents the mass ratio relative to the total mass of the first particle and the second particle added together).

[0017] If particles whose number of primary particles distinguishable by naked eye through scanning electron microscopy (SEM) analysis is greater than n1 are called "multi-particles" and particles whose number of primary particles is less than n2 are called "single particles", then the lithium composite oxide of the embodiment of the present invention is a single-particle mixed bimodal structure formed by a mixture of large particles in the form of multi-particles and basic particles in the form of single particles.

[0018] Compared with a multi-particle mixed bimodal positive electrode active material formed by mixing multiple basic particles in large particles of multiple particles, when a single-particle mixed bimodal structured positive electrode active material is applied to a secondary battery, BET decreases, gas generation is suppressed, and storage characteristics are improved.

[0019] In the second particles of the lithium composite oxide according to the embodiment of the present invention, the number of primary particles may be 20 or less, 15 or less, 10 or less, or 5 or less.

[0020] In the lithium composite oxide of the embodiment of the present invention, as shown in the above relational expression 1, when X-ray diffraction analysis is performed, the range of the half-peak width of the (104) peak is proportional to the nickel content (x 第一粒子 ) and the mass ratio of the first particle and the second particle maintain a specified relationship.

[0021] According to the above relationship 1, the optimal range of the half-peak width of the lithium composite oxide of the embodiment of the present invention can be -0.25 to 0.25 or -0.20 to 0.20. When the lithium composite oxide with a single-particle mixed bimodal structure within the above optimal range of the half-peak width is applied to a secondary battery, the electromagnetic storage characteristics and life characteristics are excellent.

[0022] In the lithium composite oxide of the embodiment of the present invention, when performing X-ray diffraction analysis, the half-peak width value will deviate and error depending on various parameters such as the state of the analysis equipment, the X-ray source, and the measurement conditions. Therefore, as shown in the above-mentioned relationship 2, the half-peak width of silicon powder (Si powder) is corrected as the standard sample.

[0023] In the lithium composite oxide of the embodiment of the present invention, the average particle size of the first particles may be 8 μm to 20 μm, 9 μm to 18 μm, 10 μm to 15 μm, or 10 μm to 13 μm.

[0024] In the lithium composite oxide of the embodiment of the present invention, the average particle size of the second particles may be 0.1 μm to 7 μm, 2 μm to 5 μm, or 3 μm to 4 μm.

[0025] The crystal structure of the lithium composite oxide according to the embodiment of the present invention may be hexagonal α-NaFeO 2 (R-3m space group).

[0026] In the lithium composite oxide of the present invention, when the nickel content x in the above chemical formula 1 is 0.97 to 0.99, the FWHM represented by the above relational formula 2 is (104) The range of θ can be 0.108°(2θ) to 0.162°(2θ).

[0027] In the lithium composite oxide of the present invention, when the nickel content x in the above chemical formula 1 is 0.93 to 0.95, the FWHM represented by the above relational formula 2 is (104) The range of θ can be 0.098°(2θ) to 0.152°(2θ).

[0028] In the lithium composite oxide of the present invention, when the nickel content x in the above chemical formula 1 is 0.87 to 0.89, the FWHM represented by the above relational formula 2 is (104) The range of θ can be 0.083°(2θ) to 0.137°(2θ).

[0029] In the lithium composite oxide of the present invention, when the nickel content x in the above chemical formula 1 is 0.79 to 0.81, the FWHM represented by the above relational formula 2 is (104) The range of θ can be 0.063°(2θ) to 0.117°(2θ).

[0030] Although not specifically described in the present invention, when performing X-ray diffraction analysis of the lithium composite oxide of the present invention, in addition to the (104) peak, multiple peaks such as (003) and (101) are observed, and each peak has a different FWHM value. When performing X-ray diffraction analysis of the lithium composite oxide of the present invention, multiple peaks detected at positions other than the (104) peak may also have FWHM ranges that are different from each other while maintaining a prescribed relationship with the molar fraction of nickel and the mass ratio of the first particle to the second particle.

[0031] The preparation method of the lithium composite oxide of an embodiment of the present invention includes: a first step, synthesizing a first positive electrode active material precursor comprising first particles formed by agglomeration of n1 (n1>40) primary particles, adding a lithium compound and calcining to prepare the first positive electrode active material; a second step, synthesizing a second positive electrode active material precursor comprising second particles formed by agglomeration of n2 (n2≤20) primary particles, adding a lithium compound and calcining; a third step, preparing the second positive electrode active material by crushing the substance formed in the above-mentioned second step; a fourth step, mixing the above-mentioned first positive electrode active material and the second positive electrode active material; and a fifth step, coating or doping the above-mentioned mixed substance with substance M and then heat treating it.

[0032] In the method for preparing the lithium composite oxide according to the embodiment of the present invention, the lithium compound added in the first step or the second step may be LiOH.

[0033] In the method for preparing the lithium composite oxide according to the embodiment of the present invention, the average particle size of the first positive electrode active material prepared in the first step may be 8 μm to 20 μm, 9 μm to 18 μm, 10 μm to 15 μm or 10 μm to 13 μm.

[0034] In the method for preparing the lithium composite oxide according to the embodiment of the present invention, the average particle size of the second positive electrode active material prepared in the third step may be 0.1 μm to 7 μm, 2 μm to 5 μm or 3 μm to 4 μm.

[0035] In the method for preparing the lithium composite oxide according to the embodiment of the present invention, after calcination in the first step, after calcination in the second step, or after pulverization in the third step, a water washing step may be further included.

[0036] In the method for preparing the lithium composite oxide according to the embodiment of the present invention, after the heat treatment in the fifth step, a water washing step may be further included.

[0037] In the preparation method of the lithium composite oxide of the embodiment of the present invention, the substance M in the fifth step can be selected from the group consisting of B, Ba, Ce, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr and their combinations, but is not limited to this.

[0038] The lithium composite oxide of the present invention has the effect of preventing microcracks of the first particles by maintaining a specified relationship between the range of the half-width value of the (104) peak defined by the hexagonal lattice having the R-3m space group and the molar fraction of nickel and the mass ratio of the first particles to the second particles, thereby ultimately producing an improved life characteristic of a battery containing a nickel-rich positive electrode active material. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a scanning electron microscope photograph of the lithium composite oxide according to an example of the present invention.

[0040] Figure 2 and Figure 3 The graph is a result of particle size analysis of the mixing mass ratio of macroparticles to elementary particles of the lithium composite oxide of the example of the present invention.

[0041] Figure 4 and Figure 5 A graph comparing the battery characteristics of single-particle hybrid bimodal and multi-particle hybrid bimodal structures.

[0042] Figure 6 The X-ray diffraction analysis results of the lithium composite oxides of the examples and comparative examples of the present invention are shown.

[0043] Figure 7 1 is the X-ray diffraction analysis result of the silicon powder according to the embodiment of the present invention.

[0044] Figure 8 and Fig. 9This is a graph comparing the battery characteristics of the lithium composite oxides of the examples of the present invention and the comparative examples.

[0045] Fig.10 and Fig.11 This is a graph comparing the battery characteristics of the lithium composite oxides of the examples of the present invention and the comparative examples.

[0046] Fig.12 and Fig.13 This is a graph comparing the battery characteristics of the lithium composite oxides of the examples of the present invention and the comparative examples. DETAILED DESCRIPTION

[0047] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to the following examples.

[0048] Determination methods and meaning of terms

[0049] When performing X-ray diffraction measurement, a Cu-Kα1 radiation source was used as an X-ray source, and measurement was performed in the range of 10-70° (2θ) at a step size of 0.02° by a θ-2θ scan (Bragg-Brentano parafocusing geometry) method.

[0050] In the determination relative to FWHM (104) and FWHM of silica fume (220) When the half-peak width is measured, the calculation is performed using Gaussian function fitting. The Gaussian function fitting for measuring the half-peak width can be performed using a variety of academic / public / commercial software known to those skilled in the art.

[0051] As silicon powder, silicon powder (product number: 215619) from Sigma-Aldrich was used.

[0052] like Figure 2 and Figure 3 As shown, the mixing mass ratio of macroparticles to elementary particles was confirmed by particle size analysis.

[0053] "Half-peak width range value" refers to FWHM (104) The value of v{0.04+(x-0.6)×0.25}, "optimal range of half-peak width" refers to the case where the half-peak width value is -0.025 to 0.025.

[0054] “FWHM 大粒子(104) ” refers to the FWHM of large particles (104) Value, "FWHM 基本粒子(104) ” refers to the FWHM of elementary particles (104) Value, "FWHM混合(104) " refers to the FWHM of lithium composite oxides prepared by mixing macroparticles and elementary particles (104) value.

[0055] Preparation Example 1

[0056] The positive electrode active material having a molar fraction of 0.80 for multiple large-particle nickel and a molar fraction of 0.85 for single elementary-particle nickel were prepared by the following method.

[0057] Synthesis of Large Particle Cathode Active Materials

[0058] First, nickel sulfate, cobalt sulfate and manganese sulfate are prepared, and a coprecipitation reaction is performed to synthesize a precursor, and LiOH is added to the synthesized precursor and then calcined to prepare a lithium composite oxide. Specifically, LiOH is mixed into the precursor, and an O2 atmosphere is maintained in a calcining furnace, and the temperature is raised by 1°C per minute for 10 hours. After that, the positive electrode active material is prepared by natural cooling.

[0059] Next, distilled water was added to the lithium composite oxide, followed by washing for 1 hour. The washed lithium composite oxide was filtered and then dried to obtain a large-particle positive electrode active material having an average diameter of 11 to 13 μm.

[0060] Method for synthesizing single elementary particle positive electrode active material

[0061] First, nickel sulfate, cobalt sulfate and manganese sulfate are prepared, and a coprecipitation reaction is performed to synthesize a precursor, and LiOH is added to the synthesized precursor and then calcined to prepare a lithium composite oxide. Specifically, LiOH is mixed into the precursor, and an O2 atmosphere is maintained in a calcining furnace, and the temperature is increased by 1°C per minute to perform a heat treatment at a temperature of 900°C for 10 hours, and then the positive electrode active material is prepared by natural cooling.

[0062] Next, the lithium composite oxide was pulverized into particles of 3 to 4 μm using a pulverizer, and then washed with distilled water for 1 hour. The washed lithium composite oxide was filtered and then dried to obtain a single-particle elementary particle positive electrode active material.

[0063] Mixing macroparticles and elementary particles to prepare the final bimodal cathode active material

[0064] Then, the large-particle positive electrode active material and the single-particle basic particle positive electrode active material are mixed with a boron-containing raw material (H3BO3) using a mixer to apply boron. 0.2 weight percent of the boron-containing raw material (H3BO3) is mixed relative to the total weight of the lithium composite oxide. The heat treatment is performed for 5 hours in the same calcining furnace while maintaining an O2 atmosphere and increasing the temperature by 2°C per minute, and then the lithium composite oxide is obtained by natural cooling.

[0065] The scanning electron microscope photograph of the prepared lithium composite oxide was measured and Figure 1 Shown in.

[0066] Preparation Example. Preparation of battery

[0067] The positive electrode active material for lithium secondary battery prepared according to the preparation example, artificial graphite as a conductive material, and polyvinylidene fluoride (PVdF) as a binding material were mixed in a weight ratio of 85:10:5 to prepare a slurry. The slurry was evenly coated on an aluminum foil with a thickness of 15 μm and vacuum dried at a temperature of 135°C to prepare a positive electrode for lithium secondary battery.

[0068] The above-mentioned positive electrode and lithium foil are used as counter electrodes, a porous polypropylene film with a thickness of 20 μm is used as a separator, and a coin battery is prepared by a conventional method using an electrolyte solution in which LiPF6 is dissolved at a concentration of 1.15 M in a solvent mixed with ethylene carbonate, diethyl carbonate and ethyl methyl carbonate in a volume ratio of 3:1:6.

[0069] Experimental Example 1

[0070] The X-ray diffraction analysis results of Examples 1-1 to 1-4 and Comparative Examples 1-1 to 1-2 prepared according to the preparation method of Preparation Example 1 are as follows: Figure 6 It was confirmed that all samples were hexagonal α-NaFeO2 (R-3m space group) structures.

[0071] In addition, in order to correct the half-peak width, the results of analyzing silicon powder using the same X-ray diffraction equipment and under the same conditions are as follows Figure 7 shown.

[0072] Then, the FWHM was determined respectively. (104) The values ​​are shown in Table 1 and Table 2.

[0073] Table 1

[0074]

[0075]

[0076] Table 2

[0077]

[0078] After preparing a lithium composite oxide having a molar fraction of 0.80 for large-particle nickel and a molar fraction of 0.85 for elementary particles of nickel as a single particle according to the preparation method of Preparation Example 1, the FWHM of the macroparticle mass ratio, elementary particle mass ratio, and nickel molar fraction was measured. 混合(104)Then, the discharge capacity and life characteristics of the battery prepared in the above preparation example were measured and the results are shown in Table 3, Figure 8 and Fig. 9 Shown in.

[0079] Table 3

[0080]

[0081]

[0082] Through Table 3, Figure 8 and Fig. 9 It can be confirmed that the discharge capacity and life of the batteries of Examples 1-1 to 1-4 whose half-peak width range values ​​satisfy the half-peak width optimal range are excellent, but the discharge capacity and life of the batteries of Comparative Examples 1-1 to 1-2 whose half-peak width range values ​​do not satisfy the half-peak width optimal range are poor.

[0083] Preparation Example 2

[0084] A positive electrode active material having a molar fraction of multi-particle large-particle nickel of 0.88 and a positive electrode active material having a molar fraction of single-particle elementary-particle nickel of 0.88 were prepared.

[0085] Synthesis of multi-particle large-particle cathode active materials

[0086] First, nickel sulfate, cobalt sulfate and manganese sulfate are prepared, and a coprecipitation reaction is performed to synthesize a precursor, and LiOH is added to the synthesized precursor and then calcined to prepare a lithium composite oxide. Specifically, LiOH is mixed into the precursor, and an O2 atmosphere is maintained in a calcining furnace, and the temperature is raised by 1°C per minute for 10 hours. After heat treatment, the positive electrode active material is prepared by natural cooling, thereby preparing a large-particle positive electrode active material with an average diameter of 11 to 13 μm.

[0087] Method for synthesizing single elementary particle positive electrode active material

[0088] First, nickel sulfate, cobalt sulfate and manganese sulfate are prepared, and a coprecipitation reaction is performed to synthesize a precursor, and LiOH is added to the synthesized precursor and then calcined to prepare a lithium composite oxide. Specifically, LiOH is mixed into the precursor, and an O2 atmosphere is maintained in a calcining furnace, and the temperature is increased by 1°C per minute to perform a heat treatment at a temperature of 900°C for 10 hours, and then the positive electrode active material is prepared by natural cooling.

[0089] Next, the lithium composite oxide was pulverized into particles of 3 to 4 μm using a pulverizer to obtain a single-particle elementary particle positive electrode active material.

[0090] Mixing macroparticles and elementary particles to prepare the final bimodal positive electrode active material

[0091] Then, the multi-particle large-particle positive electrode active material and the single-particle basic-particle positive electrode active material were mixed with Al2O3 and ZrO2 using a mixer to apply aluminum (Al) and zirconium (Zr). The heat treatment was performed for 5 hours at a temperature increase of 2°C per minute in the same calcining furnace while maintaining an O2 atmosphere, and then naturally cooled.

[0092] Next, distilled water was added to the lithium composite oxide, followed by washing with water for 1 hour, filtration, and drying to obtain a lithium composite oxide.

[0093] Experimental Example 2

[0094] The X-ray diffraction analysis results of Examples 2-1 to 2-4 and Comparative Examples 2-1 to 2-2 prepared according to the preparation method of Preparation Example 2 above confirm that all samples have a hexagonal α-NaFeO2 (R-3m space group) structure.

[0095] Then, the FWHM was determined respectively. (104) The values ​​are shown in Tables 4 and 5.

[0096] Table 4

[0097]

[0098]

[0099] Table 5

[0100]

[0101] After preparing a lithium composite oxide having a molar fraction of 0.88 for large-particle nickel and a molar fraction of 0.88 for elementary particles of nickel as a single particle according to the preparation method of Preparation Example 2, the FWHM of the large-particle mass ratio, elementary particle mass ratio, and nickel molar fraction was measured. 混合(104) Then, the discharge capacity and life characteristics of the battery prepared in the above preparation example were measured and the results are shown in Table 6, Fig.10 and Fig.11 Shown in.

[0102] Table 6

[0103]

[0104]

[0105] Through Table 6, Fig.10 and Fig.11It can be confirmed that in the case of Examples 2-1 to 2-4 where the half-width range values ​​satisfy the half-width optimal range, the discharge capacity and life of the battery are excellent, but the discharge capacity and life of the battery of Comparison Examples 2-1 to 1-2 where the half-width range values ​​do not satisfy the half-width optimal range are poor.

[0106] Preparation Example 3

[0107] A lithium composite oxide was prepared in the same manner as in Preparation Example 2 except that the molar fraction of nickel in the multi-particle macroparticle was 0.94 and the molar fraction of nickel in the single-particle elementary particle was 0.92, and titanium (Ti) and zirconium were applied as coatings.

[0108] Experimental Example 3

[0109] The X-ray diffraction analysis results of Examples 3-1 to 3-4 and Comparative Examples 3-1 to 3-2 prepared according to the preparation method of Preparation Example 3 above confirm that all samples have a hexagonal α-NaFeO2 (R-3m space group) structure.

[0110] Then, the FWHM was determined respectively. (104) The values ​​are shown in Tables 7 and 8.

[0111] Table 7

[0112]

[0113]

[0114] Table 8

[0115]

[0116] After preparing a lithium composite oxide having a molar fraction of 0.94 for large-particle nickel and a molar fraction of 0.92 for elementary particles of nickel as a single particle according to the preparation method of the above-mentioned Preparation Example 3, the FWHM of the large-particle mass ratio, elementary particle mass ratio, and nickel molar fraction was measured. 混合(104) Then, the discharge capacity and life characteristics of the battery prepared in the above preparation example were measured and the results are shown in Table 9, Fig.12 and Fig.13 Shown in.

[0117] Table 9

[0118]

[0119]

[0120] Through Table 9, Fig.12 and Fig.13It can be confirmed that the discharge capacity and life of the batteries of Examples 3-1 to 3-4 whose half-peak width range values ​​satisfy the half-peak width optimal range are excellent, but the discharge capacity and life of the batteries of Comparative Examples 3-1 to 3-2 whose half-peak width range values ​​do not satisfy the half-peak width optimal range are poor.

[0121] Experimental Example 4. Comparison of multi-particle mixed bimodal state and single-particle mixed bimodal state

[0122] When preparing high-nickel NCM bimodal positive electrode active material by mixing large particles and basic particles in the form of multiple particles, compared with basic particles in the form of multiple particles, if basic particles in the form of single particles are mixed, BET decreases, gas generation is suppressed, and storage characteristics are improved.

[0123] The gas generation rate and life characteristics when using a multi-particle mixed bimodal state and a single-particle mixed bimodal state are compared and shown in Table 10. Figure 4 and Figure 5 Shown in.

[0124] Reference Figure 4 It was confirmed that the volume change of the pouch cell due to gas generation when placed at high temperature was more than twice as high in the multi-particle mixed bimodal state as in the single-particle mixed bimodal state.

[0125] Table 10

[0126]

[0127]

Claims

1. A lithium composite oxide, It is characterized in that A mixture comprising first particles formed by agglomeration of n1 primary particles and second particles formed by agglomeration of n2 primary particles, wherein n1>40, n2≤20, The average particle size of the first particles is 8 μm to 20 μm. The average particle size of the second particles is 0.1 μm to 7 μm. The lithium composite oxide is represented by the following chemical formula 1: In the following chemical formula 1, x is 0.97 to 0.99, and the FWHM represented by the following relational formula 2 is (104) The range of satisfies 0.108°(2θ) to 0.162°(2θ), Chemical formula 1: Li a Ni x Co y Mn z M 1-x-y-z O 2 In the above chemical formula 1, M is selected from the group consisting of B, Ba, Ce, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr and combinations thereof, 0.9≤a≤1.3, 0.6≤x≤1.0, 0≤y≤0.4, 0≤z≤0.4, 0≤1-xyz≤0.4, and Relation 2: FWHM (104) ={(FWHM 化学式1powder(104) -0.1×second particle mass ratio) / first particle mass ratio}-FWHM Sipowder(220) In the above equation 2, FWHM 化学式1powder(104) represents the half-value width of the (104) peak observed near 44.5° (2θ) in the X-ray diffraction measurement value of the lithium composite oxide, Furthermore, in the above equation 2, FWHM Sipowder(220) The half-value width of the (220) peak observed near 47.3° (2θ) in the X-ray diffraction measurement value of silicon powder, the silicon powder being Sigma-Aldrich No. 215619 silicon powder.

2. A lithium composite oxide, It is characterized in that A mixture comprising first particles formed by agglomeration of n1 primary particles and second particles formed by agglomeration of n2 primary particles, wherein n1>40, n2≤20, The average particle size of the first particles is 8 μm to 20 μm. The average particle size of the second particles is 0.1 μm to 7 μm. The lithium composite oxide is represented by the following chemical formula 1: In the following chemical formula 1, x is 0.93 to 0.95, and the FWHM represented by the following relational formula 2 is (104) The range of satisfies 0.098°(2θ) to 0.152°(2θ), Chemical formula 1: Li a Ni x Co y Mn z M 1-x-y-z O 2 In the above chemical formula 1, M is selected from the group consisting of B, Ba, Ce, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr and combinations thereof, 0.9≤a≤1.3, 0.6≤x≤1.0, 0≤y≤0.4, 0≤z≤0.4, 0≤1-xyz≤0.4, and Relation 2: FWHM (104) ={(FWHM 化学式1powder(104) -0.1×second particle mass ratio) / first particle mass ratio}-FWHM Sipowder(220) In the above equation 2, FWHM 化学式1powder(104) represents the half-value width of the (104) peak observed near 44.5° (2θ) in the X-ray diffraction measurement value of the lithium composite oxide, Furthermore, in the above equation 2, FWHM Sipowder(220) The half-value width of the (220) peak observed near 47.3° (2θ) in the X-ray diffraction measurement value of silicon powder, the silicon powder being Sigma-Aldrich No. 215619 silicon powder.

3. A lithium composite oxide, It is characterized in that A mixture comprising first particles formed by agglomeration of n1 primary particles and second particles formed by agglomeration of n2 primary particles, wherein n1>40, n2≤20, The average particle size of the first particles is 8 μm to 20 μm. The average particle size of the second particles is 0.1 μm to 7 μm. The lithium composite oxide is represented by the following chemical formula 1: In the following chemical formula 1, x is 0.87 to 0.89, and the FWHM represented by the following relational formula 2 is (104) The range of satisfies 0.083°(2θ) to 0.137°(2θ), Chemical formula 1: Li a Ni x Co y Mn z M 1-x-y-z O 2 In the above chemical formula 1, M is selected from the group consisting of B, Ba, Ce, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr and combinations thereof, 0.9≤a≤1.3, 0.6≤x≤1.0, 0≤y≤0.4, 0≤z≤0.4, 0≤1-xyz≤0.4, and Relation 2: FWHM (104) ={(FWHM 化学式1powder(104) -0.1×second particle mass ratio) / first particle mass ratio}-FWHM Sipowder(220) In the above equation 2, FWHM 化学式1powder(104) represents the half-value width of the (104) peak observed near 44.5° (2θ) in the X-ray diffraction measurement value of the lithium composite oxide, Furthermore, in the above equation 2, FWHM Sipowder(220) The half-value width of the (220) peak observed near 47.3° (2θ) in the X-ray diffraction measurement value of silicon powder, the silicon powder being Sigma-Aldrich No. 215619 silicon powder.

4. A lithium composite oxide, It is characterized in that A mixture comprising first particles formed by agglomeration of n1 primary particles and second particles formed by agglomeration of n2 primary particles, wherein n1>40, n2≤20, The average particle size of the first particles is 8 μm to 20 μm. The average particle size of the second particles is 0.1 μm to 7 μm. The lithium composite oxide is represented by the following chemical formula 1: In the following chemical formula 1, x is 0.79 to 0.81, and the FWHM represented by the following relational formula 2 is (104) The range of satisfies 0.063°(2θ) to 0.117°(2θ), Chemical formula 1: Li a Ni x Co y Mn z M 1-x-y-z O 2 In the above chemical formula 1, M is selected from the group consisting of B, Ba, Ce, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr and combinations thereof, 0.9≤a≤1.3, 0.6≤x≤1.0, 0≤y≤0.4, 0≤z≤0.4, 0≤1-xyz≤0.4, and Relation 2: FWHM (104) ={(FWHM 化学式1powder(104) -0.1×second particle mass ratio) / first particle mass ratio}-FWHM Sipowder(220) In the above equation 2, FWHM 化学式1powder(104) represents the half-value width of the (104) peak observed near 44.5° (2θ) in the X-ray diffraction measurement value of the lithium composite oxide, Furthermore, in the above equation 2, FWHM Sipowder(220) The half-value width of the (220) peak observed near 47.3° (2θ) in the X-ray diffraction measurement value of silicon powder, the silicon powder being Sigma-Aldrich No. 215619 silicon powder.