Preparation method of cross-linked polyolefin diaphragm

By using the A1/B/A2 three-layer coextrusion structure and catalyst in the dry unidirectional stretching diaphragm, the degree of cross-linking of polypropylene is improved, the problems of insufficient lateral strength and degradation of the separator are solved, and the lithium-ion battery is improved security and performance.

CN118970377AActive Publication Date: 2024-11-15WUXI ENERGY NEW MATERIALS TECH CO LTD

Patent Information

Application Number
CN202411028688.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The dry unidirectional stretched diaphragm is prone to tear or short-circuit under the puncture of transverse mechanical forces and lithium dendrites, resulting in safety hazards of lithium-ion batteries. In the process of cross-linking of polypropylene, free radicals cause degradation, resulting in a decrease in molecular weight, affecting performance.

Method used

The crosslinked polyolefin separator with three-layer coextruded structure of A1/B/A2 is used to increase the degree of crosslinking, including melt extrusion, annealing, and stretching. , coating and ultraviolet lamp irradiation steps to form a high crosslinking membrane.

Benefits of technology

The lateral tensile strength and oxidation resistance of the dry diaphragm are significantly improved, the degradation of polypropylene is reduced, and the overall performance of the diaphragm is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970377A_ABST
    Figure CN118970377A_ABST
Patent Text Reader

Abstract

The invention provides a cross-linked polyolefin diaphragm and a preparation method thereof, the cross-linked polyolefin diaphragm comprises an upper surface layer (A1) and a central layer (B), the upper surface layer (A1) and the central layer (B) form an A1 / B structure, the upper surface layer (A1) is formed by copolymerization of first polyolefin with the molecular weight of 500,000-1,000,000 and second polyolefin with the molecular weight of 300,000-800,000; the central layer (B) comprises a third polyolefin having a molecular weight of 500,000-1,000,000. The gel content of the central layer (B) is 0% to 65%. The preparation method comprises the following steps: a melt extrusion step, an annealing step, a stretching step, a coating step, a drying step and an ultraviolet lamp irradiation step. A certain amount of polyethylene is introduced into the surface layer of the base membrane, and meanwhile, a certain amount of catalyst is added into the cross-linking agent, so that the cross-linking degree of polypropylene can be effectively improved, degradation of polypropylene is reduced, and the transverse tensile strength of the dry-method diaphragm is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery diaphragm preparation, and in particular to a method for preparing a cross-linked polyolefin diaphragm. Background Art

[0002] As we all know, the diaphragm is an important component of lithium-ion batteries. The diaphragm's microporous structure, physical and chemical properties, and thermodynamic properties are closely related to the comprehensive performance of the battery. The dry stretching process has received a lot of attention and research due to its simple process and low cost. Among them, the dry uniaxial stretching diaphragm has been widely used in the fields of energy storage and low-end power batteries due to its uniform pore size distribution and good thermal shrinkage performance. Since the uniaxial stretching process only involves longitudinal stretching during the stretching process, the prepared micropores are slit-like structures, so the lateral strength is very small. During the assembly and use of the battery, it is easy to be torn by lateral mechanical forces, or the lithium dendrites formed during the charging and discharging process pierce the diaphragm, causing the battery to short-circuit or micro-short-circuit, creating safety hazards.

[0003] After polyolefin cross-linking, its tensile strength, impact strength, heat resistance, etc. can be improved. The problem of poor transverse strength of polypropylene diaphragms can be improved by cross-linking. Currently, the commonly used cross-linking technologies include peroxide cross-linking, silane graft cross-linking, and radiation cross-linking. However, due to the presence of tertiary carbon atoms, the free radicals generated by the initiator during the cross-linking process attack the tertiary carbon atoms and cause β-chain scission and degradation, resulting in a decrease in the molecular weight of polypropylene, thereby affecting the overall performance of polypropylene. Summary of the invention

[0004] The purpose of the present invention is to improve the cross-linking degree of polypropylene, thereby improving the transverse tensile strength of the dry-process diaphragm.

[0005] To achieve the above-mentioned purpose, the present invention provides a cross-linked polyolefin diaphragm, characterized in that it includes an upper surface layer (A1), a center layer (B) and a lower surface layer (A2), forming an A1 / B / A2 three-layer co-extrusion structure, wherein the upper surface layer (A1) includes a first polyolefin with a molecular weight of 500,000-1,000,000 and a second polyolefin with a molecular weight of 300,000-800,000, which are copolymerized; the lower surface layer (A2) includes a first polyolefin with a molecular weight of 500,000-1,000,000 and a second polyolefin with a molecular weight of 300,000-800,000, which are copolymerized; the center layer (B) includes a third polyolefin with a molecular weight of 500,000-1,000,000.

[0006] Preferably, the upper surface layer (A1) and the lower surface layer (A2) have the same composition.

[0007] Preferably, the weight ratio of the first polyolefin to the second polyolefin of the upper surface layer (A1) is (85-95wt%):(5-15wt%); the weight ratio of the first polyolefin to the second polyolefin of the lower surface layer (A2) is (85-95wt%):(5-15wt%).

[0008] Preferably, the thickness ratio of the upper surface layer (A1), the central layer (B) and the lower surface layer (A2) is (15:70:15) to (30:40:30).

[0009] The present invention provides another cross-linked polyolefin separator, characterized in that the central layer (B) comprises a third polyolefin with a molecular weight of 500,000-1,000,000, wherein the gel content of the central layer (B) is 0% to 65%.

[0010] The present invention further provides a method for preparing a cross-linked polyolefin membrane, comprising the following steps:

[0011] (S1) Melt extrusion step: a third polyolefin with a molecular weight of 500,000 to 1,000,000 is put into a melt pump B as the material of the center layer (B), and a diaphragm is obtained after extrusion.

[0012] Preferably, (S1) further includes: 85-95wt% of a first polyolefin with a molecular weight of 500,000-1,000,000 and 5-15wt% of a second polyolefin with a molecular weight of 300,000-800,000 are uniformly mixed as the material of the upper surface layer (A1) or the lower surface layer (A2), and fed into melt pump A, and extruded separately with melt pump B to obtain a diaphragm with a three-layer co-extrusion structure of A1 / B / A2.

[0013] (S2) Annealing step: annealing the membrane obtained in (S1).

[0014] (S3) Stretching step: cold stretching and hot stretching the diaphragm obtained in (S2).

[0015] (S4) Coating step: separately prepare a crosslinking agent solution, and use a coating machine to coat the crosslinking agent solution on the diaphragm obtained in (S3).

[0016] (S5) UV light irradiation step: The diaphragm coated in (S4) is placed under a UV light for a period of time to obtain a cross-linked polyolefin diaphragm.

[0017] Preferably, a drying step (S6) is further included before or after (S5).

[0018] Preferably, in (S4), the crosslinking agent solution is prepared by dissolving a certain proportion of a photoinitiator, a crosslinking agent and a catalyst in a solvent.

[0019] Preferably, the catalyst includes a platinum-based catalyst, a tin-based catalyst, a chloroplatinic acid composite catalyst, a Grubbs catalyst, a ruthenium-based catalyst, a rhodium-based catalyst, a zirconium-based catalyst, a potassium isooctanoate catalyst, a bismuth catalyst, a palladium catalyst, a nickel catalyst, a zinc carboxylate, an iron carboxylate, a lead carboxylate, or a cobalt carboxylate.

[0020] Preferably, in (S4), the ratio of the photoinitiator, the crosslinking agent and the catalyst is 4:10:(1-3).

[0021] Preferably, in (S5), the UV lamp irradiation time is 10-300 seconds.

[0022] The beneficial effect of the present invention is that by introducing a certain amount of polyethylene into the surface layer of the base film, At the same time, adding a certain amount of catalyst to the cross-linking agent can effectively improve the cross-linking degree of polypropylene. Reduce the degradation of polypropylene and thus improve the transverse tensile strength of the dry-process diaphragm. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram illustrating the structure of the present invention.

[0024] Figure 2 It is a flow chart illustrating the preparation method of the present invention.

[0025] Figure 3A and Figure 3B FIG. 2 is a flow chart illustrating another preparation method of the present invention. DETAILED DESCRIPTION

[0026] In order to make the above and / or other purposes, effects, and features of the present invention more clearly understood, the following is a detailed description of the present invention. The preferred implementation manner is described in detail below:

[0027] See also Figure 1The present invention provides a cross-linked polyolefin separator, characterized in that it comprises an upper surface layer (A1), a center layer (B) and a lower surface layer (A2), forming an A1 / B / A2 three-layer co-extruded structure, wherein the upper surface layer (A1) comprises a first polyolefin with a molecular weight of 500,000-1,000,000 and a second polyolefin with a molecular weight of 300,000-800,000, preferably, the upper surface layer (A1) comprises a first polyolefin with a molecular weight of 500,000-600,000 and a second polyolefin with a molecular weight of 350,000-700,000. The lower surface layer (A2) is formed by copolymerizing a first polyolefin having a molecular weight of 500,000-1,000,000 and a second polyolefin having a molecular weight of 300,000-800,000. Preferably, the upper surface layer (A2) is formed by copolymerizing a first polyolefin having a molecular weight of 500,000-600,000 and a second polyolefin having a molecular weight of 350,000-700,000. The center layer (B) includes a third polyolefin having a molecular weight of 500,000-1,000,000. Preferably, the center layer (B) includes a third polyolefin having a molecular weight of 500,000-600,000.

[0028] In some embodiments, the upper surface layer (A1) and the lower surface layer (A2) have the same composition.

[0029] In some embodiments, the weight ratio of the first polyolefin to the second polyolefin of the upper surface layer (A1) is (85-95wt%):(5-15wt%); the weight ratio of the first polyolefin to the second polyolefin of the lower surface layer (A2) is (85-95wt%):(5-15wt%).

[0030] In some embodiments, the thickness ratio of the upper surface layer (A1), the central layer (B) and the lower surface layer (A2) is (15:70:15) to (30:40:30).

[0031] The present invention further provides another cross-linked polyolefin separator, characterized in that the central layer (B) comprises a third polyolefin with a molecular weight of 500,000-1,000,000, wherein the gel content of the central layer (B) is 0% to 65%.

[0032] See also Figure 2 The present invention provides a method for preparing a cross-linked polyolefin membrane, comprising: Next steps: (S1) Melt extrusion step: a polypropylene with a molecular weight of 500,000 to 1,000,000 is put into a melt pump B as an intermediate layer, and an extruder enters a die head to obtain a diaphragm. (S2) Annealing step: annealing the membrane obtained in (S1). (S3) Stretching step: cold stretching and hot stretching the diaphragm obtained in (S2). (S4) Coating step: separately prepare a crosslinking agent solution, and use a coating machine to coat the crosslinking agent solution on the diaphragm obtained in (S3), wherein the crosslinking agent solution is configured by selecting a certain proportion of a photoinitiator, a crosslinking agent, and a catalyst dissolved in an organic solvent. (S5) UV light irradiation step: placing the diaphragm after drying in (S4) under UV light for a period of time. A cross-linked polyolefin separator was obtained.

[0033] In some preferred embodiments, (S1) further comprises 85-95 wt % of a 50-100 The polypropylene with a molecular weight of 10,000-15wt% and the polyethylene with a molecular weight of 300,000-800,000 are evenly mixed in a mixer as the material of the upper surface layer (A1) or the lower surface layer (A2) and fed into melt pump A, and the polypropylene with a molecular weight of 500,000-1,000,000 is fed into melt pump B as the middle layer. The extruder enters the die head and is divided into two flow paths, thereby obtaining a diaphragm with an A1 / B / A2 three-layer co-extrusion structure, wherein the thickness of the diaphragm with the A1 / B / A2 three-layer co-extrusion structure is (15:70:15) to (30:40:30).

[0034] See also Figure 3A and Figure 3B , before or after (S5), further comprising a drying step (S6).

[0035] In some embodiments, in (S1), the melt extrusion temperature of melt pump A is 180-230°C, The melt extrusion temperature of melt pump B is 200-240°C, the die temperature is 220-250°C, and the cooling roller speed is 60-100m / min; in (S2), the annealing temperature is 120-160°C; in (S3), the cold drawing temperature is 50-130°C, the hot drawing temperature is 130-160°C, and the stretch ratio is 1.5-3; in (S5), the UV lamp irradiation time is 10-300 seconds, preferably 150 seconds, and the irradiation intensity is 1000-5000mW / cm 2 , preferably 3000mW / cm 2 ; (S6), the oven temperature is 50-100°C.

[0036] In some embodiments, in (S4), the ratio of the photoinitiator, the crosslinking agent, and the catalyst is 4:10:(1-3).

[0037] In some embodiments, the photoinitiator includes but is not limited to aromatic ketone initiators, thioxanthone derivatives, benzil derivatives, benzoin alkyl ethers, benzoin derivatives, acylphosphine oxides, alkyl phenones, benzophenones, acetophenones, anthraquinones, thioxanthones, thiol compounds, condensed ring aromatic hydrocarbons, polysilanes, acylphosphonates, aromatic acylphosphine oxides, aromatic acylphosphonates, diketones, tertiary amine photoinitiator systems, or azos.

[0038] In some preferred embodiments, the photoinitiator includes benzoin, benzoin dimethyl ether, benzoin diethyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzophenone, diphenylacetophenone, acetophenone, α-hydroxyalkylbenzophenone, α-aminoalkylbenzophenone, dibenzoylphenylphosphine oxide, 2,4-dihydroxybenzophenone, Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 1-hydroxycyclohexylbenzophenone, 2,2-dimethoxy-2-phenylacetophenone, thiopropoxythioxanthone, isopropylthioxanthone, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 2-hydroxy-2-methyl-phenylpropiophenone, 2,4,6-trimethylbenzoyldiphenyl 1-[4-(methylthio)phenyl]-2-morpholinopropanone-1, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 1,1-dichloroacetophenone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone, 2-thiobenzimidazole, 2,4,6-tri-s-triazine, pentafluorophenyl, azobisisobutyramidine hydrochloride, 2-hydroxy-methylphenylpropane-1-one, diaryliodonium salt, triaryliodonium salt, alkyliodonium salt, isopropylferrocenium hexafluorophosphate, or isopropylferrocenium hexafluorophosphate.

[0039] In some embodiments, the crosslinking agent includes polyamines, polyols, polyacids, polyacid anhydrides, silicones, benzenesulfonic acids, acrylates, organic peroxides, metal organic compounds, oxazoles, thiazoles, imidazoles, oxazolines, triazines, isocyanates, polyvinylbenzene, polycarbodiimides, silanes, di-tert-butyl peroxide, or urea compounds, and is not limited thereto.

[0040] In some preferred embodiments, the crosslinking agent includes divinylbenzene (DVB), triallyl isocyanurate (TAIC), trimethylolpropane trimethacrylate (TMPTMA), trimethylolpropane triacrylate (TMPTA), triallyl cyanurate, allyl methacrylate (AMA), triallyl cyanurate (TAC), tris(2-hydroxyethyl)isocyanuric acid triacrylate (THE I CTA), tert-butyl peroxybenzoate (TBPB), tert-butyl peroxy 3,5,5-trimethylhexanoate (TBP IN), polyethylene glycol dimethacrylate (EGDMA), diisopropyl peroxide (DCP), bis(trimethoxysilylpropyl)amine (BTMSPA), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), dicyclohexylmethane diisocyanate (HMDI), lysine diisocyanate (LDI), I), hydrogen-containing polysiloxane (PMHS), diisocyanate, tetraisocyanate, melamine, trimethylol melamine, 1,4-di-tert-butyl peroxyisopropylbenzene, 2,2-bis(tert-butyl peroxide)butane, tert-butyl hydroperoxide, 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane, diacetone acrylamide, N-hydroxymethyl acrylamide, N-hydroxyethyl acrylamide, N,N'-methylenebisacrylamide, 1,4-butanediol diacrylate, triethylene glycol di( meth)acrylate, tetraethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polybutylene glycol di(meth)acrylate, tri(2-(meth)acryloyloxyethyl)isocyanurate, di(trimethylolpropane) tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, diallyl phthalate, hydroxyethyl acrylate, glycerol dimethacrylate, 1,6-Hexanediol dimethacrylate, glycidyl ether, trimethylolpropane triglycidyl ether, trimethylolpropane diallyl ether, divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, disuccinimidyl suberate, disuccinimidyl glutarate, trimethylolpropane tris(3-mercaptopropionate), formaldehyde, glyoxal, succinic dialdehyde, glutaraldehyde, crotonaldehyde, oxalic acid, malonic acid, citric acid, maleic anhydride, hexahydrophthalic anhydride, succinic anhydride, glycidyl methacrylate, trimethylolaminomethane, epichlorohydrin, trimethylolpropane, pentaerythritol, polyethylene glycol, polypropylene glycol, trimethylolethane, diethylenetriamine, triethylenetetramine, dimethylaminopropylamine, diethylaminopropylamine , triethylenetetramine, methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, diethoxysilane, dimethylsilane, 3-aminopropyltrimethoxysilane, methyltrimethoxysilane, vinyltrimethoxysilane, propyltrimethoxysilane, phenyltrimethoxysilane, vinyltriethoxysilane, vinyltri-tert-butylperoxysilane, KH550 (3-aminopropyltriethoxysilane), KH560 (γ-(2,3-epoxypropyloxy)propyltrimethoxysilane), KH530 (2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane), KH580 (γ-mercaptopropyltriethoxysilane), KH570 (methacryloyloxy functional silicon), vinyltri(β-methoxyethoxy) Silane, 2-isopropylimidazole, mercaptoacetic acid, mercaptopropionic acid, pentaerythritol tetra(3-mercaptopropionic acid) ester, ethoxylated pentaerythritol tetraacrylate, propoxylated pentaerythritol tetraacrylate, (ethoxy) trimethylolpropane triacrylate, neopentyl glycol diacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, isobornyl methacrylate, diisopropylbenzene hydroperoxide, tert-amyl peroxy 2-ethylhexyl carbonate, 1,1-bis(tert-butyl peroxide) cyclohexane, 1,1-bis(tert-butyl peroxide)-3,3,5-trimethylcyclohexane, tert-butyl cumyl peroxide, 2,5-dimethyl-2,5-di(tert-butyl peroxide)-3-hexyne, peroxide Benzoyl, tert-butyl peroxymaleate, N,N'-bisacryloylcysteamine, polyvinyl alcohol, phthalic acid, ammonium sulfate, ammonium persulfate, polyamide, triethanolamine, diamine hydrogen phosphate, tin tetrachloride, azobisisobutyronitrile, azobisisoheptanenitrile, 1,3,5-triaminobenzene, 1,3,5-tris(4-aminophenoxy)benzene, 3,3'-diaminobenzidine, dimethyldiallylammonium chloride, acrylamide, N-(isobutyloxy)methacrylamide, N,N'-vinylbisacrylamide, 1,3,5-triacryloylhexahydro-1,3,5-triazine, triallyl trimellitate, triallyl phosphate, triallyl phosphite, N,N'-m-phenylene bismaleimide, bismaleimide, 1,6-divinyl dodecafluorohexane, octaphenyl POSS, bis(meth)acryloyloxyethyl phosphate, hexamethylenetetramine, acrylic acid, methacrylic acid, methyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, N,N,N′,N′-tetramethylmethanediamine (TMMDA), N,N,N′,N′-tetramethylethylenediamine (TMEDA), N,N,N′,N′-tetramethyl-1,6-hexanediamine ( TMHDA), diethanolamine, triethanolamine, 1,4-butanediol, 1,6-hexanediol, 1,3-butanediol, 1,2-diaminocyclohexane, 1,6-diaminohexane, p-phenylenediamine, toluidine, ethylenediamine, propylenediamine, butylenediamine, hexamethylenediamine, carbodiimide, dimethylol urea, benzyl diamine, polyethylene oxide, divinyl sulfone, trivinylbenzene, triallylamine, dicyclopentadiene, N, N-dimethylbenzylamine, or dicyandiamide.

[0041] In some embodiments, the catalyst includes a platinum-based catalyst, a tin-based catalyst, a chloroplatinic acid composite catalyst, a Grubbs catalyst, a ruthenium-based catalyst, a rhodium-based catalyst, a zirconium-based catalyst, a potassium isooctanoate catalyst, a bismuth catalyst, a palladium catalyst, a nickel catalyst, a zinc carboxylate, an iron carboxylate, a lead carboxylate, or a cobalt carboxylate.

[0042] In some preferred embodiments, the catalyst includes copper acetate, cobalt acetate, ferric acetate, nickel acetate, palladium acetate, ferric sulfate, ketone sulfate, tris(dibenzylideneacetone)dipalladium, Grubbs I generation catalyst, Grubbs II generation catalyst, Grubbs III generation catalyst, Hoveyda-Grubbs I I generation catalyst, tungsten hexachloride, dibutyltin dilaurate, dibutyltin diacetate, stannous acetate, stannous octoate, zinc naphthenate, zinc octoate, or cobalt naphthenate, and is not limited thereto.

[0043] In some embodiments, the organic solvent of the cross-linking agent solution includes monohydric alcohol, polyhydric alcohol, ethers, or benzenes, but is not limited thereto.

[0044] In some embodiments, the organic solvent of the cross-linking agent solution includes deionized water, N,N-dimethylformamide, formamide, N,N-dimethylacetamide, N-methylpyrrolidone, N-methylpyrrolidine, dimethyl sulfoxide, p-xylene, tetrahydrofuran, dichloromethane butanone, ethyl acetate, n-propyl acetate, n-butyl acetate, sec-butyl acetate, n-propanol, isopropanol, n-butanol, cyclohexanol, diacetone alcohol, n-hexane, petroleum ether, cyclohexane, ether, dioxane, toluene, xylene, dimethyl carbonate, ethyl acetate, chloroform, diphenyl ether, liquid paraffin, polyethylene glycol, and cyclopentane.

[0045] In some preferred embodiments, the organic solvent of the cross-linking agent solution includes methanol, ethanol, or acetone.

[0046] The present invention reduces the degradation ratio of polypropylene by adding a small amount of polyethylene into the raw materials for producing the polypropylene diaphragm; at the same time, metal ions are introduced into the crosslinking agent formula as catalysts, which can catalyze the crosslinking effect and also act as antioxidants to inhibit free radical degradation of the polymer.

[0047] The present invention is further described in detail below through specific examples.

[0048] A cross-linked polyolefin diaphragm is provided, characterized in that it comprises an upper surface layer (A1), a center layer (B) and a lower surface layer (A2), forming an A1 / B / A2 three-layer co-extruded structure, wherein the upper surface layer (A1) comprises a first polyolefin with a molecular weight of 500,000-1,000,000 and a second polyolefin with a molecular weight of 300,000-800,000, which are copolymerized; the lower surface layer (A2) comprises a first polyolefin with a molecular weight of 500,000-1,000,000 and a second polyolefin with a molecular weight of 300,000-800,000, which are copolymerized; and the center layer (B) comprises a third polyolefin with a molecular weight of 500,000-1,000,000.

[0049] Example 1 uses a first polyolefin with a molecular weight of 550,000 and a second polyolefin with a molecular weight of 600,000 to copolymerize to form upper and lower surface layers; the center layer uses a third polyolefin with a molecular weight of 550,000. Weigh 100 parts by mass of ethanol solution, add 10 parts of cross-linking agent TAMPTA, 4 parts of photoinitiator benzophenone, and 1 part of catalyst copper acetate, mix and stir to obtain a cross-linking agent solution C. Then use a coating machine to evenly coat solution C on the cross-linked precursor film, then dry the solvent in an oven at 70°C, and irradiate under ultraviolet light for 50s to obtain a cross-linked polyolefin diaphragm. The relevant physical properties and gel content of the obtained cross-linked polyolefin diaphragm were detected, and the specific data and results can be seen in Table 1 and Table 2.

[0050] In Example 2, the catalyst was replaced with 1.5 parts of copper acetate catalyst, and the rest was the same as in Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0051] In Example 3, the catalyst was replaced with 2 parts of copper acetate catalyst, and the rest was the same as in Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0052] In Example 4, the catalyst was replaced with 3 parts of copper acetate catalyst, and the rest was the same as in Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0053] Example 5: The catalyst was replaced with 3 parts of copper acetate catalyst and irradiated with UV light for 100 s. The rest is the same as Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0054] Example 6: The catalyst was replaced with 3 parts of copper acetate catalyst and irradiated with UV light for 150 seconds. The rest is the same as Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0055] Example 7: The catalyst was replaced with 3 parts of copper acetate catalyst and irradiated with UV light for 200 seconds. The rest is the same as Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0056] In Example 8, the molecular weight of the first polyolefin and the third polyolefin was replaced with 450,000, the catalyst was replaced with 3 parts of copper acetate catalyst, and the ultraviolet light was irradiated for 150 seconds. The rest was the same as in Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0057] In Example 9, the molecular weight of the first polyolefin and the third polyolefin was replaced with 700,000, the catalyst was replaced with 3 parts of copper acetate catalyst, and the ultraviolet light was irradiated for 150 seconds. The rest was the same as in Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0058] Example 10: The molecular weight of the second polyolefin was replaced with 350,000, the catalyst was replaced with 3 parts of copper acetate, and the ultraviolet light was irradiated for 150 seconds. The rest was the same as Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0059] Example 11: The molecular weight of the second polyolefin was replaced with 850,000, the catalyst was replaced with 3 parts of copper acetate, and the ultraviolet light was irradiated for 150 seconds. The rest was the same as Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0060] Example 12: The molecular weight of the third polyolefin was replaced with 500,000, the catalyst was replaced with 3 parts of copper acetate, and the UV light was irradiated for 150 seconds. The rest was the same as Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0061] Example 13: The molecular weight of the third polyolefin was replaced with 600,000, the catalyst was replaced with 3 parts of copper acetate, and the ultraviolet light was irradiated for 150 seconds. The rest was the same as Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0062] In Comparative Example 1, no catalyst was added, and the UV lamp was irradiated for 200 seconds. The rest was the same as in Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested. The specific results can be seen in Table 2.

[0063] In Comparative Example 2, the catalyst was replaced with 3 parts of a non-metallic catalyst organic phosphorus compound, and the UV light was irradiated for 200 seconds. The rest was the same as in Example 1. The relevant physical properties and gel content of the obtained cross-linked polyolefin separator were tested, and the specific results can be seen in Table 2.

[0064] Comparative Example 3: The physical properties of the uncrosslinked precursor film were tested.

[0065] Table 1 First Polyolefin (10,000) Second polyolefin (10,000) The third polyolefin (10,000) Photoinitiator Crosslinking agent catalyst UV light irradiation(s) Example 1 55 60 55 4 10 1 50 Example 2 55 60 55 4 10 1.5 50 Example 3 55 60 55 4 10 2 50 Example 4 55 60 55 4 10 3 50 Example 5 55 60 55 4 10 3 100 Example 6 55 60 55 4 10 3 150 Example 7 55 60 55 4 10 3 200 Example 8 45 60 45 4 10 3 150 Example 9 70 60 70 4 10 3 150 Example 10 55 35 55 4 10 3 150 Embodiment 11 55 85 55 4 10 3 150 Example 12 55 60 50 4 10 3 150 Example 13 55 60 60 4 10 3 150 Comparative Example 1 55 60 55 4 10 - 200 Comparative Example 2 55 60 55 4 10 3 200 Comparative Example 3 55 60 55 - - - -

[0066] Table 2

[0067] The gel content can directly reflect the degree of cross-linking of polyolefins. It can be seen from Table 2 that When no crosslinking agent is added, there is no crosslinking of polyolefin, so the gel content is 0; when no catalyst is added to the crosslinking agent solution, or the catalyst is a non-metallic catalyst, the gel content is low. After the catalyst is added, the gel content is significantly increased, and as the catalyst content increases, the gel content continues to increase. It should be noted here that the UV light irradiation time also affects the degree of crosslinking. From Table 2, when the UV light irradiation time is 150s, the gel content reaches the maximum value. If the irradiation continues, the degree of crosslinking will decrease.

[0068] The gel content is calculated using a Soxhlet extractor, and the specific test method is as follows: (1) Weigh 0.5±0.05 g of the cross-linked product and place it in a clean and dry 100-120 mesh copper mesh; weigh the copper mesh in advance, record it as m1, weigh the mass of the product plus the copper mesh, record it as m2, accurate to 1 mg; (2) Take a certain amount of xylene and put it into a round-bottom flask (the mass of xylene and sample is not less than 500:1, and ensure that the sample and the sieve are completely placed in the solvent), turn on the heating device, heat the xylene to boiling, and reflux the sample for 10 hours. The reflux rate is controlled at 20-40 drops / min; (3) Carefully remove the copper mesh, place it in an oven at 120°C and dry it for 6 h, and weigh it, which is recorded as m3; (4) The formula for calculating gel content is as follows:

[0069] From the tensile and needle punching data in Table 2, it can be seen that after the polypropylene diaphragm is cross-linked, In particular, the strength in the transverse direction is significantly improved, and the higher the degree of cross-linking, the higher the strength; the needle punching strength is also significantly improved with the increase of the degree of cross-linking.

[0070] However, what is described above is only a preferred embodiment of the present invention, but it cannot be used to limit the patent protection scope of the present invention; therefore, all simple equivalent changes and modifications made according to the patent protection scope of the present invention and the contents of the specification still fall within the patent protection scope of the present invention.

Claims

1. A cross-linked polyolefin separator, characterized in that: It comprises an upper surface layer (A1) and a central layer (B) to form an A1 / B structure, wherein the upper surface layer (A1) comprises a first polyolefin with a molecular weight of 500,000-1,000,000 and a second polyolefin with a molecular weight of 300,000-800,000; and the central layer (B) comprises a third polyolefin with a molecular weight of 500,000-1,000,000.

2. The cross-linked polyolefin membrane according to claim 1, characterized in that: It further includes a lower surface layer (A2), which is arranged in sequence as an upper surface layer (A1), a center layer (B) and a lower surface layer (A2), forming an A1 / B / A2 three-layer co-extrusion structure, wherein the lower surface layer (A2) includes a first polyolefin with a molecular weight of 500,000-1,000,000 and a second polyolefin with a molecular weight of 300,000-800,000.

3. The cross-linked polyolefin membrane according to claim 2, characterized in that: The upper surface layer (A1) and the lower surface layer (A2) have the same composition.

4. The cross-linked polyolefin separator according to claim 2, characterized in that: The weight ratio of the first polyolefin to the second polyolefin of the upper surface layer (A1) is (85-95wt%):(5-15wt%); the weight ratio of the first polyolefin to the second polyolefin of the lower surface layer (A2) is (85-95wt%):(5-15wt%).

5. A cross-linked polyolefin separator, characterized in that: The central layer (B) comprises a third polyolefin with a molecular weight of 500,000-1,000,000, wherein the gel content of the central layer (B) is 0% to 65%.

6. A method for preparing a cross-linked polyolefin separator, comprising the following steps: (S1) melt extrusion step: a third polyolefin with a molecular weight of 500,000 to 1,000,000 is put into a melt pump B as a material for the center layer (B), and a diaphragm is obtained after extrusion; (S2) Annealing step: annealing the membrane obtained in (S1); (S3) stretching step: cold stretching and hot stretching the diaphragm obtained in (S2); (S4) coating step: preparing a crosslinking agent solution and coating the crosslinking agent solution on the separator obtained in (S3) using a coating machine; and (S5) UV light irradiation step: The diaphragm coated in (S4) is placed under a UV light for a period of time to obtain a cross-linked polyolefin diaphragm.

7. The preparation method according to claim 6, characterized in that: (S1) further includes: 85-95wt% of a first polyolefin with a molecular weight of 500,000-1,000,000 and 5-15wt% of a second polyolefin with a molecular weight of 300,000-800,000 are uniformly mixed as the material of the upper surface layer (A1) or the lower surface layer (A2), and are fed into melt pump A, and extruded separately with melt pump B to obtain a diaphragm with a three-layer co-extruded structure of A1 / B / A2.

8. The preparation method according to claim 6, characterized in that: Before or after (S5), a drying step (S6) is further included.

9. The preparation method according to claim 6, characterized in that: In (S4), the crosslinking agent solution is prepared by dissolving a certain proportion of a photoinitiator, a crosslinking agent, and a catalyst in a solvent.

10. The preparation method according to claim 9, characterized in that: The catalyst includes a platinum-based catalyst, a tin-based catalyst, a chloroplatinic acid composite catalyst, a Grubbs catalyst, a ruthenium-based catalyst, a rhodium-based catalyst, a zirconium-based catalyst, a potassium isooctanoate catalyst, a bismuth catalyst, a palladium catalyst, a nickel catalyst, a zinc carboxylate, an iron carboxylate, a lead carboxylate, or a cobalt carboxylate.

Citation Information

Patent Citations

  • Cross-linked multilayer porous polymer membrane battery separators

    CN104425790A

  • Interlayer crosslinking co-extrusion battery diaphragm, preparation method thereof and battery

    CN116231231A

  • Porous polyolefin substrate containing cross-linked structure, method for producing same, and separator containing cross-linked structure

    CN116583995A

  • Microporous Polymeric Membrane, Battery Separator, and Battery

    US20100297491A1

Cited By

  • Amitraz PE acaricidal tablet and preparation method thereof

    CN120787951A

  • Method for preparing crosslinked polyolefin microporous membrane

    WO2026116639A1