Preparation method of efficient electromagnetic wave-absorbing material

By mixing metal powder with metal sulfide and conductive materials and ball milling, a multi-metal sulfide-based electromagnetic wave absorbing material is formed, which solves the problem of insufficient wave absorbing performance in the existing technology, and improves the absorption characteristics of the full-band and broadband performance. .

CN118970477APending Publication Date: 2024-11-15KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411017189.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The attenuation capacity of existing metal sulfide absorbing materials is limited, and the impedance mismatch of the monolithic structure weakens its absorbing performance, making it difficult to effectively absorb electromagnetic waves in the entire frequency band.

Method used

By mixing metal powder with metal sulfide and conductive materials (such as graphene, carbon nanotubes) in a specific proportion and ball milling in an inert gas atmosphere, multiple metal sulfide-based electromagnetic wave absorbing materials are obtained, and multiple loss mechanisms are obtained. To optimize wave absorption performance.

Benefits of technology

The three-band absorption characteristics in the entire frequency band are realized. The absorption area covers all S bands and some areas of the X and Ku bands, and the maximum absorption broadband reaches 4.56GHz, which significantly improves the absorption performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004966105460000011
    Figure HDA0004966105460000011
Patent Text Reader

Abstract

The invention discloses a preparation method of an efficient electromagnetic wave-absorbing material, which comprises the following steps: grinding and mixing metal powder and metal sulfide to obtain mixed powder, loading the mixed powder into a ball milling tank in a glove box, ensuring that the material is in an inert gas atmosphere, and carrying out ball milling on the material and a conductive material to obtain the efficient electromagnetic wave-absorbing material. According to the invention, the combination of the metal sulfide and other dielectric and magnetic materials to obtain a plurality of loss mechanisms and optimize the wave-absorbing performance is an effective strategy, so that the binary metal sulfide-based wave-absorbing material-conductive material can obtain an efficient electromagnetic wave-absorbing material with a three-frequency-band absorption characteristic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of microwave absorption, and in particular to a method for preparing a high-efficiency electromagnetic wave absorbing material. Background Art

[0002] In the past few decades, the rapid development of advanced electronic technology has brought about serious electromagnetic pollution problems. On the one hand, the normal operation of communication electronic equipment will be interfered by electromagnetic pollution, causing electromagnetic signal leakage and electromagnetic compatibility problems. On the other hand, long-term excessive electromagnetic radiation will pose a threat to human health. Therefore, overcoming electromagnetic radiation and interference has become an acute problem in modern society. Ideal absorbing materials are required to have thin thickness, light weight, wide absorption bandwidth, strong absorption intensity and good chemical stability.

[0003] In recent years, metal sulfide-based absorbers have attracted great interest due to their flexible adjustment of size, shape and dimension during synthesis to adjust their physical or chemical properties, which makes them more suitable for the field of wave absorption. However, due to the undesignable structure and imperfect loss mechanism of monometallic sulfide, their attenuation capacity is limited. In addition, the impedance mismatch of monometallic sulfide-based absorbers will also weaken their absorbing performance. By searching relevant literature, it can be found that the structure and morphology rules have a significant impact on the performance of wave absorption. One-dimensional (1D) materials with aspect ratio and anisotropy will form axial carrier channels, which is convenient for promoting the transmission of electrons when interacting with microwaves. Two-dimensional (2D) materials have a relatively large specific surface area, which can increase the interaction area with microwaves, and the lamellar structure can increase microwave scattering to promote attenuation. Three-dimensional (3D) structures with more holes and hollow structures can achieve optimized impedance matching. Therefore, effective specification of the structure is helpful to obtain excellent absorbing performance. Metal sulfides are typical dielectric loss absorbers with a single loss mechanism. Therefore, it would be an effective strategy to combine metal sulfides with other dielectric or magnetic materials to obtain multiple loss mechanisms and optimize their microwave absorbing properties. Summary of the invention

[0004] In view of the above problems, the present invention provides a method for preparing an electromagnetic absorbing material combined with multiple metal sulfides. By combining multiple materials, multiple loss mechanisms are obtained to optimize the absorbing performance.

[0005] The technical solution of the present invention is as follows:

[0006] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0007] (1) grinding and mixing metal powder and metal sulfide to obtain a mixed powder;

[0008] (2) The mixed powder is loaded into a ball mill in a glove box to ensure that the material is in an inert gas atmosphere, and the mixed powder is ball milled together with the conductive material at a certain time and rotation speed to obtain the absorbing material.

[0009] The metal powder includes one of iron, cobalt, nickel, manganese and the like.

[0010] The metal sulfide includes one of tin disulfide, germanium sulfide, bismuth sulfide, antimony sulfide and the like.

[0011] The molar ratio of the metal powder to the metal sulfide is 1:1 to 6:1;

[0012] The conductive material includes: one of graphene, fullerene, carbon nanotube, MXene, black phosphorus and the like.

[0013] The mass of the conductive material accounts for 30-70% of the mass of the mixed powder.

[0014] The ball milling time is 1 to 72 hours, and the ball milling speed is 400 to 600 rpm.

[0015] Beneficial effects of the present invention:

[0016] The invention realizes the characteristic of three-band absorption in the full frequency band by preparing binary metal sulfide and compounding with conductive materials, and the wave absorption area basically covers the whole area of ​​S band and part of X band and Ku band; the synthesis of binary metal sulfide of the invention improves the wave absorption performance of monometallic sulfide-based composite material, metal sulfide is a typical dielectric loss material with a single loss mechanism, and the invention combines metal sulfide with other dielectric or magnetic materials to obtain multiple loss mechanisms and optimize its wave absorption performance, which is an effective strategy, so that the binary metal sulfide-based electromagnetic wave absorbing material-conductive material obtains a maximum absorption bandwidth of 4.56 GHz. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Corresponding curves of the high-efficiency absorbing material NSS-3 / GP-50% prepared in Example 1: (a) real part of dielectric constant ε'; (b) real part of magnetic permeability μ'; (c) tanδ ε ; (d) Imaginary part of dielectric constant ε”; (e) Imaginary part of magnetic permeability μ”; (f) tanδ μ ; (g) C0 curve; (h) attenuation constant α; (i) impedance matching ratio Z; (j) 3D reflection loss diagram; (k) 2D reflection loss diagram; (l) reflection loss point and line diagram. DETAILED DESCRIPTION

[0018] The present invention is further described in detail below in conjunction with specific embodiments.

[0019] Example 1

[0020] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0021] Weigh 0.9632 g of nickel powder and 1 g of tin disulfide, grind and mix them to obtain a mixed powder NSS, load the mixed powder NSS into a ball mill in a glove box, ensure that the material is in an argon atmosphere, add 0.9816 g of graphene, and ball mill and mix at 500 r / min for 18 hours to obtain a high-efficiency electromagnetic absorbing material NSS-3 / GP-50%.

[0022] Compared with other electromagnetic absorbing materials, the electromagnetic absorbing material NSS-3 / GP-50% obtained in this embodiment has the characteristics of three-band absorption. Figure 1 a and 1d show the frequency dependence of the real and imaginary parts of the complex dielectric constant of the NSS-3 / GP-50% composite sample. The ε′ and ε″ values ​​change from 9.2 and 1.9 at 2.0 GHz to 7.9 and 1.2 at 18.0 GHz, respectively. Due to the frequency dispersion behavior, they show a typical downward trend. In the frequency range of 11.0-17.0 GHz, the ε′-f and ε″-f curves show obvious peaks. According to the traditional dielectric theory and Debye equation, the changes in the ε′-f and ε″-f curves of these samples are determined by the conductive loss and polarization loss. The NSS-3 / GP-50% composite material is characterized by dielectric, while the main dipole polarization and related relaxation phenomena constitute the loss mechanism. Figure 1 b and 1e show the frequency dependence of the real and imaginary parts of the complex magnetic permeability of the NSS-3 / GP-50% composite sample. Magnetic loss is another factor in electromagnetic wave dissipation, which is calculated by the complex magnetic permeability (μr=μ′-jμ″). The blocking effect of non-magnetic media and the high-temperature pinning effect are the main reasons for this phenomenon. It is worth noting that the μ″ value of the sample appears negative at high frequencies, which can be explained by Maxwell's equations. Under the action of external electromagnetic waves, the movement and migration of charges will generate an alternating electric field, which in turn generates an internal magnetic field and releases a certain amount of magnetic energy. NS The S-3 / GP-50% composite material has a high dielectric loss content and a weak magnetic response. The inherent magnetic loss cannot offset the radiation of magnetic energy in the high-frequency range, resulting in a negative μ″ value. Generally speaking, magnetic loss is mainly caused by ferromagnetic resonance, hysteresis loss, domain wall resonance and eddy current loss, among which hysteresis loss is relatively weak in the microwave field and can be ignored. In addition, domain wall resonance mainly occurs in the MHz range, not the GHz range, so the magnetic loss of the sample is mainly due to ferromagnetic resonance and eddy current loss. At the same time, the mechanism of magnetic loss can be explained by the formula C0 = μ"(μ′) -2 f -1 To explain, if C0 is a constant that has nothing to do with frequency changes, the magnetic loss will be completely realized by eddy current loss. Obviously, Figure 1 g, the C0 of NSS-3 / GP-50% composite material changes with the frequency. The results show that the magnetic loss mechanism is not only eddy current loss, but also includes natural resonance and exchange resonance. The attenuation constant α( Figure 1 h) and impedance matching Z( Figure 1 i) are the two most critical parameters for discussing the absorption performance. With the increase of frequency, the α value of NSS-3 / GP-50% composite material shows an overall increasing trend. Combining the α value and dielectric constant of the sample, it can be found that the sample with a high ε″ value generally has a larger α value. It also proves that dielectric loss plays a leading role in the attenuation of electromagnetic waves. The impedance matching value (Z=Z in / Z0) determines whether electromagnetic waves can enter the material without being reflected, while the attenuation constant value specifies the material's attenuation performance for electromagnetic waves. These two factors together determine the material's absorption performance. Generally, the closer the value of Z is to 1, the better the impedance matching performance of the material, and more electromagnetic waves can enter the material without being reflected. Figure 1 It can be seen from Figures 1j, 1k and 1l that the absorbing area covers the entire S band, part of the X band and Ku band, and the effective absorbing frequency band width is 3.91 GHz when the material thickness is 8.30 mm, and the absorption peak reaches 69.31 dB at 2.75 GHz when the thickness is 9.22 mm.

[0023] Example 2

[0024] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0025] Weigh 0.9016 g of manganese powder and 1 g of tin disulfide, grind and mix them to obtain a mixed powder MSS, load the mixed powder MSS into a ball mill in a glove box, ensure that the material is in an argon atmosphere, add 0.9508 g of graphene, and ball mill and mix at 500 r / min for 18 hours to obtain a high-efficiency electromagnetic absorbing material MSS-3 / GP-50%.

[0026] The electromagnetic absorbing material MSS-3 / GP-50% obtained in this embodiment has the characteristics of three-band absorption compared with other electromagnetic absorbing materials. When the thickness of the material is 8.51 mm, the effective absorbing frequency band width is 3.5 GHz, and when the thickness is 5.29 mm, the absorption peak reaches 67.38 dB at 16.25 GHz.

[0027] Example 3

[0028] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0029] Weigh 1.6815g of nickel powder and 1g of germanium sulfide, grind and mix them to obtain a mixed powder NGS, load the mixed powder NGS into a ball mill in a glove box, ensure that the material is in a nitrogen atmosphere, add 1.3408g of graphene, and ball mill and mix at 500r / min for 18h to obtain a high-efficiency electromagnetic absorbing material NGS-3 / GP-50%.

[0030] The electromagnetic absorbing material NGS-3 / GP-50% obtained in this embodiment has the characteristics of three-band absorption compared with other electromagnetic absorbing materials. When the thickness of the material is 4.53 mm, the effective absorbing frequency band width is 3.96 GHz, and when the thickness is 7.07 mm, the absorption peak reaches 64.48 dB at 3.18 GHz.

[0031] Example 4

[0032] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0033] Weigh 0.9632 g of nickel powder and 1 g of tin disulfide, grind and mix them to obtain a mixed powder NSS, load the mixed powder NSS into a ball mill in a glove box, ensure that the material is in a nitrogen atmosphere, add 0.9816 g of graphene, and ball mill and mix at 500 r / min for 12 h to obtain a high-efficiency electromagnetic absorbing material NSS-3 / GP-50%.

[0034] The electromagnetic absorbing material NSS-3 / GP-50% obtained in this embodiment has the characteristics of three-band absorption compared with other electromagnetic absorbing materials. When the thickness of the material is 9.12 mm, the effective absorbing frequency band width is 3.28 GHz, and when the thickness is 5.80 mm, the absorption peak reaches 61.61 dB at 13.87 GHz.

[0035] Example 5

[0036] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0037] Weigh 0.9632 g of nickel powder and 1 g of tin disulfide, grind and mix them to obtain a mixed powder NSS. Load the mixed powder NNS into a ball mill in a glove box to ensure that the material is in a nitrogen atmosphere. Add 0.9816 g of graphene and ball mill at 600 r / min for 18 h to obtain a high-efficiency electromagnetic absorbing material NSS-3 / GP-50%.

[0038] The electromagnetic absorbing material NSS-3 / GP-50% obtained in this embodiment has the characteristics of three-band absorption compared with other electromagnetic absorbing materials. When the thickness of the material is 2.07 mm, the effective absorbing frequency band width is 4.13 GHz, and when the thickness is 2.54 mm, the absorption peak reaches 58.31 dB at 5.86 GHz.

[0039] Example 6

[0040] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0041] Weigh 0.9632 g of nickel powder and 1 g of tin disulfide, grind and mix them to obtain a mixed powder NSS. Load the mixed powder NNS into a ball mill in a glove box to ensure that the material is in a nitrogen atmosphere. Add 0.9816 g of graphene and ball mill at 500 r / min for 18 h to obtain a high-efficiency electromagnetic absorbing material NSS-3 / GP-50%.

[0042] The electromagnetic absorbing material NSS-3 / F-50% obtained in this embodiment has the characteristics of three-band absorption compared with other electromagnetic absorbing materials. When the thickness of the material is 5.59 mm, the effective absorbing frequency band width is 2.91 GHz, and when the thickness is 6.32 mm, the absorption peak reaches 43.92 dB at 9.26 GHz.

[0043] Example 7

[0044] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0045] 0.9632 g of nickel powder and 1 g of tin disulfide were weighed and ground and mixed to obtain a mixed powder NSS. The mixed powder NNS was loaded into a ball mill in a glove box to ensure that the material was in an argon atmosphere. 0.9816 g of MXene was added and ball milled at 500 r / min for 18 h to obtain a high-efficiency electromagnetic absorbing material NSS-3 / M-50%.

[0046] The electromagnetic absorbing material NSS-3 / M-50% obtained in this embodiment has the characteristics of three-band absorption compared with other electromagnetic absorbing materials. When the thickness of the material is 3.28 mm, the effective absorbing frequency band width is 4.56 GHz, and when the thickness is 4.23 mm, the absorption peak reaches 62.58 dB at 13.89 GHz.

[0047] Example 8

[0048] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0049] Weigh 0.9632 g of nickel powder and 1 g of tin disulfide, grind and mix them to obtain a mixed powder NSS. Load the mixed powder NNS into a ball mill in a glove box to ensure that the material is in an argon atmosphere. Add 0.5890 g of graphene and ball mill at 500 r / min for 18 h to obtain a high-efficiency electromagnetic absorbing material NSS-3 / GP-30%.

[0050] The electromagnetic absorbing material NSS-3 / GP-30% obtained in this embodiment has the characteristics of three-band absorption compared with other electromagnetic absorbing materials. When the thickness of the material is 8.01 mm, the effective absorbing frequency band width is 3.57 GHz, and when the thickness is 8.93 mm, the absorption peak reaches 65.37 dB at 3.26 GHz.

[0051] Example 9

[0052] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0053] Weigh 0.9632 g of nickel powder and 1 g of tin disulfide, grind and mix them to obtain a mixed powder NSS. Load the mixed powder NNS into a ball mill in a glove box to ensure that the material is in an argon atmosphere. Add 1.3742 g of graphene and ball mill at 500 r / min for 18 h to obtain a high-efficiency electromagnetic absorbing material NSS-3 / GP-70%.

[0054] The electromagnetic absorbing material NSS-3 / GP-70% obtained in this embodiment has the characteristics of three-band absorption compared with other electromagnetic absorbing materials. When the thickness of the material is 8.28 mm, the effective absorbing frequency band width is 3.69 GHz, and when the thickness is 9.03 mm, the absorption peak reaches 70.23 dB at 2.86 GHz.

[0055] Example 10

[0056] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0057] Weigh 0.3211 g of nickel powder and 1 g of tin disulfide, grind and mix them to obtain a mixed powder NSS. Load the mixed powder NNS into a ball mill in a glove box to ensure that the material is in an argon atmosphere. Add 0.6606 g of graphene and ball mill at 500 r / min for 18 h to obtain a high-efficiency electromagnetic absorbing material NSS-1 / GP-50%.

[0058] The electromagnetic absorbing material NSS-1 / GP-50% obtained in this embodiment has the characteristics of three-band absorption compared with other electromagnetic absorbing materials. When the thickness of the material is 9.42 mm, the effective absorbing frequency band width is 3.87 GHz, and when the thickness is 6.23 mm, the absorption peak reaches 60.01 dB at 14.25 GHz.

[0059] Embodiment 11

[0060] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0061] 1.9264 g of nickel powder and 1 g of tin disulfide were weighed and ground and mixed to obtain a mixed powder NSS. The mixed powder NNS was loaded into a ball mill in a glove box to ensure that the material was in an argon atmosphere. 1.4632 g of graphene was added and ball milled at 500 r / min for 18 h to obtain a high-efficiency electromagnetic absorbing material NSS-6 / GP-50%.

[0062] The electromagnetic absorbing material NSS-6 / GP-50% obtained in this embodiment has the characteristics of three-band absorption compared with other electromagnetic absorbing materials. When the thickness of the material is 8.63 mm, the effective absorbing frequency band width is 4.19 GHz, and when the thickness is 8.38 mm, the absorption peak reaches 66.20 dB at 9.91 GHz.

[0063] Example 12

[0064] A method for preparing a high-efficiency electromagnetic absorbing material, the steps are as follows:

[0065] Weigh 0.9632 g of nickel powder and 1 g of tin disulfide, grind and mix them to obtain a mixed powder NSS. Load the mixed powder NNS into a ball mill in a glove box to ensure that the material is in a nitrogen atmosphere. Add 0.9816 g of graphene and ball mill at 400 r / min for 24 hours to obtain a high-efficiency electromagnetic absorbing material NSS-3 / GP-50%.

[0066] The electromagnetic absorbing material NSS-3 / GP-50% obtained in this embodiment has the characteristics of three-band absorption compared with other electromagnetic absorbing materials. When the thickness of the material is 6.86 mm, the effective absorbing frequency band width is 3.18 GHz, and when the thickness is 7.03 mm, the absorption peak reaches 45.31 dB at 15.24 GHz.

[0067] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A method for preparing a high-efficiency electromagnetic absorbing material, characterized in that: Here are the steps: (1) grinding and mixing metal powder and metal sulfide to obtain a mixed powder; (2) The mixed powder is loaded into a ball mill in a glove box, the material is placed in an inert gas atmosphere, and ball milled together with the conductive material to obtain an absorbing material.

2. The method for preparing the high-efficiency electromagnetic absorbing material according to claim 1, characterized in that: The metal powder is one of iron, cobalt, nickel and manganese powder.

3. The method for preparing the high-efficiency electromagnetic absorbing material according to claim 1, characterized in that: The metal sulfide is one of tin disulfide, germanium sulfide, bismuth sulfide and antimony sulfide.

4. The method for preparing the high-efficiency electromagnetic absorbing material according to claim 1, characterized in that: The molar ratio of the metal powder to the metal sulfide is 1:1 to 6:

1.

5. The method for preparing the high-efficiency electromagnetic absorbing material according to claim 1, characterized in that: The conductive material is one of graphene, fullerene, carbon nanotube, MXene and black phosphorus.

6. The method for preparing the high-efficiency electromagnetic absorbing material according to claim 1, characterized in that: The mass of the conductive material accounts for 30-70% of the mass of the mixed powder.

7. The method for preparing the high-efficiency electromagnetic absorbing material according to claim 1, characterized in that: The ball milling time is 1 to 72 hours, and the ball milling speed is 400 to 600 rpm.

Citation Information

Cited By

  • Preparation method of wave-absorbing and flame-retardant bimetallic heterojunction nano composite material

    CN120904663A