Process for preparing membranes (M) comprising sulfonated poly (arylene ether sulfone) polymers (sp) and non-sulfonated poly (arylene sulfone) polymers (P)

By using poly(vinylpyrrolidone) as a pore-forming additive in poly(arylene ether sulfone) membrane, the problem of poly(vinylpyrrolidone) elution is solved, high purity water permeability and low molecular weight are achieved, and the membrane is improved biocompatibility and application performance.

CN118973692APending Publication Date: 2024-11-15BASF SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031792.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In hemodialysis applications, existing poly(arylene ether sulfone) membranes are elution from the membrane due to the solubility of poly(vinylpyrrolidone) in water, which reduces biocompatibility and impairs patient safety, and is difficult to reduce the Cost to achieve low molecular weight and high water permeability.

Method used

By providing a method, comprising a sulfonated poly(arylene ether sulfone) polymer and a non-sulfonated poly(arylene sulfone) polymer, using poly(vinyl pyrrolidone) as a pore-forming additive, consisting of a specific solution And the treatment steps, a membrane capable of retaining poly(vinylpyrrolidone) in the membrane matrix was prepared to achieve high purity water permeability and low molecular weight retention.

Benefits of technology

Retention of poly(vinylpyrrolidone) in the membrane matrix is ​​achieved, the biocompatibility of the membrane is improved, and the application performance of the membrane is enhanced by increasing the pure water permeability of the membrane and controlling the molecular weight of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005066729860000121
    Figure BDA0005066729860000121
  • Figure BDA0005066729860000131
    Figure BDA0005066729860000131
  • Figure BDA0005066729860000132
    Figure BDA0005066729860000132
Patent Text Reader

Abstract

The present invention relates to a process for preparing a membrane (M) comprising a sulfonated poly (arylene ether sulfone) polymer (sP) and a non-sulfonated poly (arylene sulfone) polymer (P), the membrane (M) obtained by the process and the use of the membrane (M) as an ultrafiltration membrane and / or for hemodialysis applications.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] manual

[0002] The present invention relates to a method for preparing a membrane (M), the membrane (M) obtained by the method and the use of the membrane (M) as an ultrafiltration membrane and / or for hemodialysis applications, the membrane (M) comprising a sulfonated poly(arylene ether sulfone) polymer (sP) and a non-sulfonated poly(arylene sulfone) polymer (P).

[0003] Poly(arylene ether sulfone) polymers are high-performance thermoplastics because they are characterized by high heat resistance, good mechanical properties and inherent flame retardancy (EM Koch, H.-M. Walter, Kunststoffe 80 (1990) 1146; E. Kunststoffe 80, (1990) 1149, N. Inchaurondo-Nehm, Kunststoffe 98, (2008) 190). They are highly biocompatible and are therefore used as materials for forming dialysis membranes (NA Hoenich, KP Katapodis, Biomaterials 23 (2002) 3853) and ultrafiltration (UF) membranes. Ultrafiltration membranes (UF) are believed to have an active filter layer with a molecular weight cutoff of 10 kDa to 100 kDa corresponding to a pore size of 10 nm to 30 nm to effectively remove yeast, bacteria, viruses and macromolecules from water.

[0004] Poly(arylene ether sulfone) membranes are generally prepared by a method comprising two steps: in a first step, a solution is provided, wherein the solution comprises poly(arylene ether sulfone), a pore-forming additive and a solvent; in a second step, the pore-forming additive and the solvent are separated from the solution to obtain the poly(arylene ether sulfone) membrane. Since water-soluble poly(vinyl pyrrolidone) also improves the viscosity of the solution, it is generally added to the poly(arylene ether sulfone) solution as a pore-forming additive (S. Munari et al., Desalination 70 (1988) 265). In addition, for hemodialysis (HD) applications, the remaining amount of poly(vinyl pyrrolidone) in the active filter layer inhibits the adhesion of serum proteins and platelets to the membrane surface.

[0005] WO 2017 / 220363 A1 discloses the use of a membrane M comprising at least one sulfonated polyarylene ether A for removing arsenic compounds AS from an aqueous system, wherein the membrane M is an ultrafiltration membrane or a microfiltration membrane having a molecular weight cutoff of at least 2,500 Da.

[0006] US 2018 / 0345230 A1 discloses a transport membrane comprising a nanoporous polyethersulfone / polyvinylpyrrolidone blend carrier membrane, a hydrophilic polymer inside the nanopores of the carrier membrane, a hydrophilic polymer coating on the surface of the carrier membrane, and metal salts in the hydrophilic polymer coating and in the hydrophilic polymer inside the nanopores of the carrier membrane.

[0007] US 5,246,582 discloses a synthetic hydrophilic membrane in the form of a hollow fiber or flat membrane, which includes a mixture within a single layer of polysulfone and sulfonated polysulfone, wherein the mixture contains a range providing properties for dialysis and / or ultrafiltration, namely, about 65 wt % to about 95 wt % sulfonated polysulfone and about 5 wt % to about 35 wt % unsulfonated polysulfone.

[0008] In the article "Effect of Molecular Weight of Sulfonated Poly(ether sulfone) (SPES) on the Mechanical Strength and Antifouling Properties of Poly(ether sulfone) / SPES Blend Membranes" (Ind. Eng. Chem. Res., 2017, 56, 11302) by LF. Fang et al., the effect of the molecular weight of sulfonated poly(ether sulfone) on the properties of poly(ether sulfone) / SPES blend membranes was studied. As the molecular weight of SPES increases, the mechanical strength of the membrane increases.

[0009] The article by A. Rahimpour et al., “The influence of sulfonated polyethersulfone (SPES) on surface nanomorphology and performance of polyethersulfone (PES) membrane” (Appl. Surf. Sci., 2010, 256, 1825) describes the sulfonation of polyethersulfone (PES) and the preparation of polyethersulfone (PES) / sulfonated polyethersulfone (SPES) blend membranes by immersion precipitation technology, in which PVP is added as a pore former.

[0010] However, due to its solubility in water, poly(vinyl pyrrolidone) is easily eluted / leached from the membrane and thus reduces the biocompatibility of the dialysis membrane and compromises patient safety during HD treatment (M. Miyata et al., ASAIO Journal (2015) 468).

[0011] It is therefore an object of the present invention to provide an improved poly(arylene ether sulfone) membrane which exhibits reduced poly(vinyl pyrrolidone) leaching. The membrane should also show a low molecular weight cut-off and a high water permeability. The process for preparing the membrane should be easy to perform at relatively low cost.

[0012] This object is achieved by a method for producing a membrane (M), the membrane (M) comprising

[0013] (A) sulfonated poly(arylene ether sulfone) polymer (sP) and

[0014] (B) a non-sulfonated poly(arylene sulfone) polymer (P),

[0015] The method comprises at least steps a) and b):

[0016] a) providing a solution (S), the solution (S) comprising a sulfonated poly(arylene ether sulfone) polymer (sP) according to component (A), a non-sulfonated poly(arylene sulfone) polymer (P) according to component (B), at least one pore-forming additive (C) and at least one solvent (D), wherein the at least one pore-forming additive (C) comprises poly(vinyl pyrrolidone); and

[0017] b) separating the at least one pore forming additive (C) and the at least one solvent (D) from the solution (S) to obtain a membrane (M).

[0018] The object is further achieved by a method for producing a membrane (M), the membrane (M) comprising

[0019] (A) sulfonated poly(arylene ether sulfone) polymer (sP) and

[0020] (B) a non-sulfonated poly(arylene sulfone) polymer (P),

[0021] The method comprises at least steps a) and b):

[0022] a) providing a solution (S), the solution (S) comprising a sulfonated poly(arylene ether sulfone) polymer (sP) according to component (A), a non-sulfonated poly(arylene sulfone) polymer (P) according to component (B), at least one pore-forming additive (C) and at least one solvent (D), wherein the at least one pore-forming additive (C) comprises poly(vinyl pyrrolidone); and

[0023] b) separating the at least one pore-forming additive (C) and the at least one solvent (D) from the solution (S) to obtain a membrane (M),

[0024] wherein the solution (S) in step a) comprises 0.5 to 20 wt.-% of the sulfonated poly(arylene ether sulfone) polymer (sP), 0.5 to 20 wt.-% of the non-sulfonated poly(arylene sulfone) polymer (P), 3 to 20 wt.-% of the at least one pore-forming additive (C) and 40 to 96 wt.-% of the at least one solvent (D), in each case based on the total weight of the solution (S).

[0025] It has surprisingly been found that membranes (M) prepared by the process of the present invention and comprising a sulfonated poly(arylene ether sulfone) polymer (sP) exhibit an increased poly(vinyl pyrrolidone) (PVP) content (PVP 总 and PVP 表面 ), which means that the membranes (M) of the present invention retain poly(vinyl pyrrolidone) in the membrane matrix and thus prevent poly(vinyl pyrrolidone) from leaching out of the membrane matrix. In addition, the membranes (M) of the present invention all show a relative humidity of >50 kg / (hm 2 bar) and a molecular weight cut-off (MWCO) range of 11.2 kDa to 30 kDa.

[0026] The present invention will be described in more detail below.

[0027] Method for preparing membrane (M)

[0028] By the process of the invention comprising at least step a) and step b), a membrane (M) is produced.

[0029] In the context of the present invention, the term "membrane" means a semi-permeable structure capable of separating two fluids or separating molecules and / or ionic components or particles from a liquid. Therefore, the membrane acts as a selective barrier, allowing some particles, substances or chemicals to pass through while retaining other particles, substances or chemicals. The membrane can have various geometric shapes, such as flat sheets, spirally wound, pillow blocks, tubular, single-hole hollow fibers or porous hollow fibers.

[0030] Flat sheet membranes and hollow fiber membranes are preferred.

[0031] The membrane (M) is prepared by a process comprising at least step a) and step b):

[0032] a) providing a solution (S), the solution (S) comprising a sulfonated poly(arylene ether sulfone) polymer (sP) according to component (A), a non-sulfonated poly(arylene sulfone) polymer (P) according to component (B), at least one pore-forming additive (C) and at least one solvent (D), wherein the at least one pore-forming additive (C) comprises poly(vinyl pyrrolidone); and

[0033] b) separating the at least one pore forming additive (C) and the at least one solvent (D) from the solution (S) to obtain a membrane (M).

[0034] Step a)

[0035] In step a), a solution (S) is provided, which comprises a sulfonated poly(arylene ether sulfone) polymer (sP) according to component (A), a non-sulfonated poly(arylene sulfone) polymer (P) according to component (B), at least one pore-forming additive (C) and at least one solvent (D), wherein the at least one pore-forming additive (C) comprises poly(vinyl pyrrolidone).

[0036] In the context of the present invention, "at least one pore-forming additive" means exactly one pore-forming additive and also mixtures of two or more pore-forming additives.

[0037] In the context of the present invention, "at least one pore-forming additive, wherein at least one pore-forming additive (C) comprises poly(vinylpyrrolidone)" means that the pore-forming additive may consist of poly(vinylpyrrolidone) or may comprise poly(vinylpyrrolidone) and at least one further pore-forming additive.

[0038] A further object of the present invention is therefore also a process for producing a membrane (M), wherein the at least one pore-forming additive (C) consists of poly(vinylpyrrolidone).

[0039] In the context of the present invention, "at least one solvent" means exactly one solvent and also mixtures of two or more solvents.

[0040] The solution (S) in step a) may be provided by any method known to a person skilled in the art. For example, the solution (S) may be provided in step a) in conventional containers, which may include stirring means and preferably temperature control means. Preferably, the solution (S) is provided by dissolving the sulfonated poly(arylene ether sulfone) polymer (sP), the non-sulfonated poly(arylene sulfone) polymer (P) and the at least one pore-forming additive (C) in the at least one solvent (D), wherein the at least one pore-forming additive (C) comprises poly(vinyl pyrrolidone).

[0041] Dissolving the sulfonated poly(arylene ether sulfone) polymer (sP), the non-sulfonated poly(arylene sulfone) polymer (P) and the at least one pore forming additive (C) in the at least one solvent (D) to provide a solution (S) is preferably carried out under stirring, wherein the at least one pore forming additive (C) comprises poly(vinyl pyrrolidone).

[0042] Step a) is preferably carried out at elevated temperature, especially in the range of 20 to 100° C., more preferably in the range of 40 to 80° C. A person skilled in the art will choose the temperature according to the at least one solvent (D).

[0043] The solution (S) preferably comprises the sulfonated poly(arylene ether sulfone) polymer (sP), the non-sulfonated poly(arylene sulfone) polymer (P) and the at least one pore-forming additive (C), wherein the at least one pore-forming additive (C) comprises poly(vinyl pyrrolidone), completely dissolved in the at least one solvent (D). This means that the solution (S) preferably does not comprise solid particles of the sulfonated poly(arylene ether sulfone) polymer (sP), the non-sulfonated poly(arylene sulfone) polymer (P) and the at least one pore-forming additive (C), wherein the at least one pore-forming additive (C) comprises poly(vinyl pyrrolidone). Thus, the sulfonated poly(arylene ether sulfone) polymer (sP), the non-sulfonated poly(arylene sulfone) polymer (P) and the at least one pore-forming additive (C), wherein the at least one pore-forming additive (C) comprises poly(vinyl pyrrolidone), preferably cannot be separated from the at least one solvent (D) by filtration.

[0044] The solution (S) may comprise 0.5 to 25 wt.-% of the sulfonated poly(arylene ether sulfone) polymer (sP), 0.5 to 25 wt.-% of the non-sulfonated poly(arylene sulfone) polymer (P), 3 to 30 wt.-% of the at least one pore-forming additive (C), and 20 to 96 wt.-% of the at least one solvent (D), in each case based on the total weight of the solution (S).

[0045] Preferably, the solution (S) comprises 0.5 to 20 wt.-% of the sulfonated poly(arylene ether sulfone) polymer (sP), 0.5 to 20 wt.-% of the non-sulfonated poly(arylene sulfone) polymer (P), 3 to 20 wt.-% of the at least one pore-forming additive (C) and 40 to 96 wt.-% of the at least one solvent (D), in each case based on the total weight of the solution (S).

[0046] A further object of the present invention is therefore also a process for producing a membrane (M), wherein the solution (S) in step a) comprises from 0.5 to 20% by weight of a sulfonated poly(arylene ether sulfone) polymer (sP), from 0.5 to 20% by weight of a non-sulfonated poly(arylene sulfone) polymer (P), from 3 to 20% by weight of the at least one pore-forming additive (C) and from 40 to 96% by weight of the at least one solvent (D), in each case based on the total weight of the solution (S).

[0047] As the at least one solvent (D), any solvent known to those skilled in the art for sulfonated poly(arylene ether sulfone) polymers (sP), non-sulfonated poly(arylene sulfone) polymers (P) and the at least one pore-forming additive (C) is suitable. Preferably, the at least one solvent (D) is soluble in water. Thus, the at least one solvent (D) is preferably selected from the group consisting of N-alkyl-2-pyrrolidone, preferably N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-butyl-2-pyrrolidone and N-tert-butyl-2-pyrrolidone, 2-pyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, dimethylformamide, N,N-dimethyl-2-hydroxypropaneamide, N,N-diethyl-2-hydroxypropaneamide, γ-valerolactone, dihydro-levulinone, 5-(dimethylamino)-2-methyl-5-oxopentanoic acid methyl ester and sulfolane. N-Alkyl-2-pyrrolidones, γ-valerolactone and N,N-dimethyl-2-hydroxypropaneamide are particularly preferred. N-Methylpyrrolidone is most preferred as the at least one solvent (D).

[0048] Therefore, another object of the present invention is also a method for preparing a membrane (M), wherein the at least one solvent (D) is selected from the group consisting of: N-alkyl-2-pyrrolidone, preferably N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-butyl-2-pyrrolidone and N-tert-butyl-2-pyrrolidone, 2-pyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, dimethylformamide, N,N-dimethyl-2-hydroxypropaneamide, N,N-diethyl-2-hydroxypropaneamide, γ-valerolactone, dihydrolevoglucose ketone, 5-(dimethylamino)-2-methyl-5-oxopentanoic acid methyl ester and cyclopentane.

[0049] The solution (S) may comprise, for example, at least one solvent (D) in the range of 20 wt % to 96 wt %, preferably at least one solvent (D) in the range of 40 wt % to 96 wt %, and most preferably at least one solvent (D) in the range of 50 wt % to 70 wt %, based on the total weight of the solution (S).

[0050] The solution (S) provided in step a) further comprises at least one pore-forming additive (C) for membrane preparation, wherein the at least one pore-forming additive (C) comprises poly(vinyl pyrrolidone).

[0051] Another suitable pore-forming additive (C) is poly(alkylene oxide) and alcohol.

[0052] Examples of suitable poly(alkylene oxides) are poly(ethylene oxide), poly(propylene oxide) and poly(ethylene oxide)-poly(propylene oxide) copolymers. Examples of suitable alcohols are diols or triols such as glycerol.

[0053] As further pore-forming additives (C), preference is given to alcohols, in particular glycerol.

[0054] Therefore, another object of the present invention is also a process for preparing a membrane (M), wherein the at least one pore-forming additive (C) also comprises at least one alcohol, preferably glycerol.

[0055] Preferably, the at least one pore-forming additive (C) comprises in the range of 17 to 75 wt% of poly(vinylpyrrolidone) and in the range of 25 to 83 wt% of at least one alcohol, preferably glycerol.

[0056] More preferably, the at least one pore-forming additive (C) comprises poly(vinylpyrrolidone) in the range of 31.25 wt.-% to 43.75 wt.-% and at least one alcohol, preferably glycerol, in the range of 56.25 wt.-% to 68.75 wt.-%.

[0057] In a preferred embodiment, the at least one pore-forming additive (C) consists of poly(vinylpyrrolidone) and at least one alcohol, preferably glycerol.

[0058] The solution (S) may comprise the at least one pore-forming additive (C), for example, in an amount of 3 to 30 wt%, preferably 3 to 20 wt%, based on the total weight of the solution (S).

[0059] In a preferred embodiment, solution (S) comprises 3 to 15 wt.-% of poly(vinylpyrrolidone) and 5 to 15 wt.-% of at least one alcohol, based on the total weight of solution (S).

[0060] In a more preferred embodiment, solution (S) comprises 5 to 7 wt.-% of poly(vinylpyrrolidone) and 9 to 11 wt.-% of at least one alcohol, based on the total weight of solution (S).

[0061] It is clear to a person skilled in the art that the weight percentages of the sulfonated poly(arylene ether sulfone) polymer (sP), the non-sulfonated poly(arylene sulfone) polymer (P), the at least one pore-forming additive (C) and the at least one solvent (D) included in the solution (S) generally add up to 100 weight percent.

[0062] The duration of step a) may vary within wide limits. The duration of step a) is preferably in the range of 10 min to 48 h (hours), especially in the range of 10 min to 24 h, and more preferably in the range of 15 min to 12 h. A person skilled in the art will choose the duration of step a) so as to obtain a homogeneous solution of the sulfonated poly(arylene ether sulfone) polymer (sP), the non-sulfonated poly(arylene sulfone) polymer (P) and the at least one pore-forming additive (C) in the at least one solvent (D).

[0063] Step b)

[0064] In step b), the at least one pore-forming additive (C) and the at least one solvent (D) are separated from the solution (S) to obtain a membrane (M).

[0065] The solution (S) provided in step a) may be filtered before separating the at least one pore-forming additive (C) and the at least one solvent (D) from the solution (S) in step b) to obtain a filtered solution (fS). The following embodiments and preferred requirements for separating the at least one pore-forming additive (C) and the at least one solvent (D) from the solution (S) are also applicable to separating the at least one pore-forming additive (C) and the at least one solvent (D) from the filtered solution (fS).

[0066] In addition, the solution (S) may be degassed in step a) to obtain a degassed solution (dS) before separating the at least one pore-forming additive (C) and the at least one solvent (D) from the solution (S) in step b). This embodiment is preferred. The following embodiments and preferred requirements for separating the at least one pore-forming additive (C) and the at least one solvent (D) from the solution (S) are also applicable to separating the at least one pore-forming additive (C) and the at least one solvent (D) from the degassed solution (dS).

[0067] The degassing of the solution (S) in step a) can be performed by any method known to the person skilled in the art, for example via vacuum or by allowing the solution (S) to stand.

[0068] The separation of the at least one pore-forming additive (C) and the at least one solvent (D) from the solution (S) can be performed by any method known to a person skilled in the art to be suitable for separating pore-forming additives and solvents from polymers.

[0069] Preferably, separation of the at least one pore-forming additive (C) and the at least one solvent (D) from the solution (S) is performed via a phase inversion method.

[0070] Therefore, another object of the present invention is also a process for preparing a membrane (M), wherein the separation of the at least one pore-forming additive (C) and the at least one solvent (D) in step b) is carried out via a phase inversion method.

[0071] If the separation of the at least one pore-forming additive (C) and the at least one solvent (D) is carried out via a phase inversion process, the membrane (M) obtained is generally a porous membrane.

[0072] Therefore, another object of the present invention is a membrane (M), wherein the membrane (M) is a porous membrane (M).

[0073] As known to those skilled in the art, a porous membrane (M) generally has a top layer, which is the active filter layer, and a support structure at the bottom. The top layer and the support structure generally comprise pores, wherein the pore size distribution of the top layer is practically the only determining factor for the properties of the membrane. Generally speaking, the pore size of the top layer is smaller than the pore size of the support structure at the bottom.

[0074] Preferably, the pore size of the membrane (M) increases from the top layer used for separation to the bottom of the membrane (M). Therefore, such membranes (M) are also referred to as asymmetric membranes (M).

[0075] Therefore, another object of the present invention is a membrane (M), wherein the membrane (M) is asymmetric.

[0076] The minimum pore size of the membrane (M) is preferably <10 nm.

[0077] The support structures may have a diameter of up to 10 μm.

[0078] Phase inversion process in the context of the present invention means a process in which dissolved sulfonated poly(arylene ether sulfone) polymer (sP) and dissolved non-sulfonated poly(arylene sulfone) polymer (P) are converted into a solid phase. Therefore, the phase inversion process can also be indicated as a precipitation process. According to step b), the conversion is performed by separating the at least one pore-forming additive (C) and the at least one solvent (D) from the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P). Suitable phase inversion processes are known to the person skilled in the art.

[0079] The phase inversion method can be carried out, for example, by cooling the solution (S). During this cooling, the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P) included in the solution (S) precipitate. Another possibility for carrying out the phase inversion method is to contact the solution (S) with a steam which is a non-solvent for the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P). Then, the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P) will also precipitate. Suitable steam (which is a non-solvent for the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P)) is, for example, a protic polar solvent in its gaseous state as described below. Another phase inversion method preferred in the context of the present invention is a phase inversion carried out by immersing the solution (S) in at least one protic polar solvent.

[0080] Therefore, in one embodiment of the present invention, in step b), the at least one pore-forming additive (C) and the at least one solvent (D) comprised in the solution (S) are separated from the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P) comprised in the solution (S) by immersing the solution (S) in at least one protic polar solvent.

[0081] This means that the membrane (M) is formed by immersing the solution (S) in at least one protic polar solvent.

[0082] Suitable at least one protic polar solvent is known to the skilled person.The at least one protic polar solvent is preferably a non-solvent for the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P).

[0083] Preferred at least one protic polar solvent is water, methanol, ethanol, n-propanol, isopropanol, glycerol, ethylene glycol and mixtures thereof.Preferably, the at least one protic polar solvent is a water-based coagulation bath.

[0084] Therefore, another object of the present invention is a process for preparing a membrane (M), wherein the at least one protic polar solvent is a water-based coagulation bath.

[0085] Preferably, the water-based coagulation bath comprises, besides water, further components, for example the same solvent (D) as comprised in the solution (S) or an alcohol, in particular glycerol.

[0086] Step b) generally comprises providing a solution (S) in a form corresponding to the form of the membrane (M) obtained in step b).

[0087] Therefore, in one embodiment of the present invention, step b) comprises casting of the solution (S) to obtain a thin film of the solution (S).

[0088] Therefore, in a preferred embodiment of the present invention, step b) comprises the following steps:

[0089] b-1) casting the solution (S) provided in step a) to obtain a thin film of the solution (S);

[0090] b-2) immersing the thin film of the solution (S) into at least one protic polar solvent, wherein the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P) included in the thin film of the solution (S) are at least partially separated from the at least one pore-forming additive (C) and the at least one solvent (D) included in the thin film of the solution (S) to obtain a membrane (M1) in the form of a thin film, and

[0091] b-3) washing the membrane (M1) with water, wherein the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P) included in the membrane (M1) are substantially completely separated from at least one pore-forming additive (C) and at least one solvent (D) included in the membrane (M1) to obtain the membrane (M).

[0092] Therefore, another object of the present invention is a method for preparing a membrane (M), wherein step b) comprises the following steps:

[0093] b-1) casting the solution (S) provided in step a) to obtain a thin film of the solution (S),

[0094] b-2) immersing a thin film of solution (S) into at least one protic polar solvent, wherein the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P) included in the thin film of solution (S) are at least partially separated from at least one pore-forming additive (C) and at least one solvent (D) included in the thin film of solution (S) to obtain a membrane (M1) in the form of a thin film, and

[0095] b-3) washing the membrane (M1) with water, wherein the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P) included in the membrane (M1) are substantially completely separated from at least one pore-forming additive (C) and at least one solvent (D) included in the membrane (M1) to obtain the membrane (M).

[0096] In the context of the present invention, the term "at least partially" means that preferably at least 50 wt.-%, more preferably at least 60 wt.-%, of the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P), based on the total weight of the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P) comprised in the film of the solution (S), are separated from the at least one pore-forming additive (C) and the at least one solvent (D).

[0097] In the context of the present invention, the term "substantially completely" means that preferably at least 90 wt.-%, more preferably at least 95 wt.-%, of the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P), based on the total weight of the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P) comprised in the membrane (M1), are separated from the at least one pore-forming additive (C) and the at least one solvent (D).

[0098] In a preferred embodiment, the film (M) exhibits an increased poly(vinyl pyrrolidone) (PVP) content (PVP 总 and PVP 表面 ), which means that the membrane (M) of the present invention retains the poly(vinyl pyrrolidone) in the membrane matrix and thus prevents the poly(vinyl pyrrolidone) from leaching out of the membrane matrix.

[0099] Preferably, the film (M) has a poly(vinylpyrrolidone) content PVPtotal in the range of 0.8 to 5 wt.-%, based on the total weight of the film (M).

[0100] In step b-1), the solution (S) can be cast by any method known to those skilled in the art. Typically, the solution (S) is cast with a casting knife heated to a temperature in the range of 20°C to 100°C, preferably in the range of 40°C to 80°C.

[0101] Therefore, another object of the present invention is a process for preparing a membrane (M), wherein step b-1) is carried out at a temperature ranging from 40°C to 80°C.

[0102] The solution (S) is typically cast on a substrate that is non-reactive with the sulfonated poly(arylene ether sulfone) polymer (sP), the non-sulfonated poly(arylene sulfone) polymer (P), the at least one pore-forming additive (C), or the at least one solvent (D) included in the solution (S).

[0103] Suitable substrates are known to the skilled person and are, for example, selected from glass plates, polymer films and polymer fabrics (such as nonwoven materials).

[0104] In step b-2), a thin film of solution (S) is immersed in at least one protic polar solvent, preferably at a temperature in the range of 20 to 80°C, more preferably in the range of 20 to 60°C.

[0105] In step b-3), the membrane (M1 ) is preferably washed at a temperature ranging from 20 to 80°C, more preferably at a temperature ranging from 20 to 60°C.

[0106] The membrane (M) obtained in step b-3) is preferably a flat sheet membrane.

[0107] The membrane (M) can be used as an ultrafiltration and / or hemodialysis membrane.

[0108] A further object of the present invention is therefore also the use of the membrane (M) as an ultrafiltration membrane and / or for hemodialysis applications.

[0109] In order to obtain a dense membrane, the separation in step b) may be performed by evaporating the at least one solvent (D) comprised in the solution (S).

[0110] For the preparation of single-pore hollow fibers, step b) can be performed by extruding the solution (S) through an extrusion nozzle with a desired number of hollow needles. The coagulation liquid is then injected into the extruded polymer through the hollow needles during extrusion so that parallel continuous channels extending in the extrusion direction are formed in the extruded polymer. Preferably, the pore size on the outer surface of the extruded membrane is controlled by contacting the outer surface with a mild coagulant after leaving the extrusion nozzle so that the shape is fixed in the absence of an active layer on the outer surface, and then contacting the membrane with a strong coagulant.

[0111] Membrane (M)

[0112] Another object of the present invention is also a membrane prepared by the above-mentioned method of the present invention.

[0113] The membrane (M) comprises a sulfonated poly(arylene ether sulfone) polymer (sP) and a non-sulfonated poly(arylene sulfone) polymer (P).

[0114] Preferably, the membrane (M) comprises 5 to 90 wt.-%, more preferably 7.5 to 80 wt.-% of the sulfonated poly(arylene ether sulfone) polymer (sP), based on the total weight of the membrane (M).

[0115] Therefore, another object of the present invention is a membrane (M), wherein the membrane (M) comprises 5 to 90 wt.-% of the sulfonated poly(arylene ether sulfone) polymer (sP), based on the total weight of the membrane (M).

[0116] The membrane (M) also preferably comprises 10 to 95 wt.-%, more preferably 20 to 92.5 wt.-% of non-sulfonated poly(arylene sulfone) polymer (P), based on the total weight of the membrane (M).

[0117] In a preferred embodiment, the membrane (M) therefore comprises 5 to 90% by weight of sulfonated poly(arylene ether sulfone) polymer (sP) and 10 to 95% by weight of non-sulfonated poly(arylene sulfone) polymer (P), based in each case on the total weight of the membrane (M).

[0118] The membrane (M) preferably has a pressure of >50 kg / (hm2) determined using a pressure cell with a diameter of 74 mm using ultrapure water (no saline, filtered through a Millipore UF system) at 23°C and 1 bar water pressure. 2 bar). The pure water permeability (PWP) is calculated as follows (Formula (1)):

[0119]

[0120] PWP: Pure water permeability [kg / bar hm 2 ]

[0121] m: Mass of permeate water [kg]

[0122] A: membrane area [m 2 ]

[0123] P: Pressure [bar]

[0124] t: time of penetration experiment [h].

[0125] Therefore, another object of the present invention is a membrane (M), wherein the membrane (M) has a density of >50 kg / hm 2 Pure water permeability in bar.

[0126] In a preferred embodiment, the membrane (M) has a molecular weight cut-off of 10 kDa to 30 kDa.

[0127] Therefore, another object of the present invention is a membrane (M), wherein the membrane (M) has a molecular weight cut-off in the range of 10 kDa to 30 kDa.

[0128] Component (A )

[0129] The solution (S) includes a sulfonated poly(arylene ether sulfone) polymer (sP) as component (A). In this case, the terms "sulfonated poly(arylene ether sulfone) polymer (sP)" and "component (A)" are used synonymously and thus have the same meaning.

[0130] In this case, the term "sulfonated poly(arylene ether sulfone) polymer (sP)" is understood to mean exactly one sulfonated poly(arylene ether sulfone) polymer (sP) and also mixtures of two or more sulfonated poly(arylene ether sulfone) polymers (sP).

[0131] In a preferred embodiment, the sulfonated poly(arylene ether sulfone) polymer (sP) comprises units of formula (I)

[0132]

[0133] in

[0134] t and q: each independently 0, 1, 2 or 3,

[0135] Q, T and Y: each independently a chemical bond or selected from -O-, -S-, -SO2-, -S(=O)-, -(C=O)-, -N=N- and -CR a R b - a group, wherein R a and R b are independently a hydrogen atom or a C1-C 12 Alkyl, C1-C 12 Alkoxy or C6-C 18 An aryl group, and wherein at least one of Q, T and Y is -SO2- and

[0136] Ar and Ar 1 : Each independently is an arylene group having 6 to 18 carbon atoms

[0137] And among them

[0138] At least one unit (I) comprises an arylene group substituted with at least one -SO2X group, wherein X is selected from the group consisting of Cl and O- in combination with a cation equivalent, wherein the cation equivalent is H + , Li + 、Na + , K + Mg 2+ , Ca 2+ or NH4 + .

[0139] Therefore, another object of the present invention is a process wherein the sulfonated poly(arylene ether sulfone) polymer (sP) comprises units of formula (I)

[0140]

[0141] in

[0142] t and q: each independently 0, 1, 2 or 3,

[0143] Q, T and Y: each independently a chemical bond or selected from -O-, -S-, -SO2-, -S(=O)-, -(C=O)-, -N=N- and -CR a R b - a group, wherein R a and R b are independently a hydrogen atom or a C1-C 12 Alkyl, C1-C 12 Alkoxy or C6-C 18 An aryl group, and wherein at least one of Q, T and Y is -SO2- and

[0144] Ar and Ar 1 : Each independently is an arylene group having 6 to 18 carbon atoms

[0145] And among them

[0146] At least one unit (I) comprises an arylene group substituted with at least one -SO2X group, wherein X is selected from Cl and O in combination with a cation equivalent. - The group consisting of wherein the cation equivalent is H + , Li + 、Na + , K + Mg 2+ , Ca 2+ or NH4 + .

[0147] Among the above conditions, if Q, T or Y is a chemical bond, this should be understood to mean that the adjacent group on the left and the adjacent group on the right are directly bonded to each other via a chemical bond. It will be easily understood that at least one of the groups consisting of Q, T and Y is -SO2-, which means that at least one of Q, T and Y in formula (I) is -SO2-. As a result, for example, when q=0, at least one of T and Y is -SO2-; when, for example, t=0, at least one of Q and Y is -SO2-, and when q=0 and t=0, then Y is SO2.

[0148] If Q, T or Y is -CR a R b -, then R a and R b are independently a hydrogen atom or a C1-C 12 -alkyl, C1-C 12 -alkoxy or C6-C 18 - an aryl group.

[0149] Preferred C1-C 12-Alkyl groups include straight-chain and branched saturated alkyl groups having 1 to 12 carbon atoms. The following radicals should be mentioned in particular: C1-C6-alkyl radicals such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, 2- or 3-methylpentyl, and longer chain radicals such as unbranched heptyl, octyl, nonyl, decyl, undecyl, lauryl and their mono- or poly-branched analogs.

[0150] Available C1-C above 12 The alkyl radicals that can be used in the -alkoxy group include the alkyl radicals having 1 to 12 carbon atoms as defined above. The cycloalkyl radicals that can be preferably used include in particular C3-C 12 -cycloalkyl radicals, for example cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclopropylmethyl, cyclopropylethyl, cyclopropylpropyl, cyclobutylmethyl, cyclobutylethyl, cyclopentylethyl, -propyl, -butyl, -pentyl, -hexyl, cyclohexylmethyl, -dimethyl and -trimethyl.

[0151] Ar and Ar 1 Each independently is C6-C 18 -arylene group. Ar is preferably derived from an electron-rich aromatic substance susceptible to electrophilic attack, preferably selected from the group consisting of hydroquinone, resorcinol, dihydroxynaphthalene, especially 2,7-dihydroxynaphthalene and 4,4'-bisphenol. Preferably, Ar 1 is unsubstituted C6- or C 12 -Arylene group.

[0152] Available C6-C 18 -Arylene groups Ar and Ar 1 Particularly included are phenylene groups such as 1,2-, 1,3- and 1,4-phenylene, naphthylene groups such as 1,6-, 1,7-, 2,6- and 2,7-naphthylene, and arylene groups derived from anthracene, phenanthrene and naphthacene.

[0153] Preferably, in a preferred embodiment, Ar and Ar of formula (I) 1 Each is independently selected from the group consisting of 1,4-phenylene, 1,3-phenylene, naphthylene, especially 2,7-dihydroxynaphthylene and 4,4'-biphenylene.

[0154] Preferred sulfonated poly(arylene ether sulfone) polymers (sP) are those comprising as repeating structural units at least one of the following units Ia to Io, wherein at least one unit (I) comprises an arylene group substituted with at least one -SO2X group, wherein X is selected from the group consisting of Cl and O- in combination with a cation equivalent, wherein the cation equivalent is H +, Li + 、Na + , K + Mg 2+ , Ca 2+ or NH4 + :

[0155]

[0156]

[0157] In addition to the preferred units Ia to Io, preference is also given to those units in which one or more 1,4-phenylene units derived from hydroquinone are replaced by 1,3-phenylene units derived from resorcinol or by naphthylene units derived from dihydroxynaphthalene.

[0158] Particularly preferred units of the general formula (I) are units Ia, Ig and Ik. It is also particularly preferred that the sulfonated poly(arylene ether sulfone) polymer of component (A) consists essentially of one unit of the units of the general formula (I), in particular of units selected from the group consisting of Ia, Ig and Ik.

[0159] In a particularly preferred embodiment, Ar = 1,4-phenylene, t = 1, q = 0, T is a bond and Y = SO2. A particularly preferred sulfonated poly(arylene ether sulfone) polymer (A) formed from the above repeating units is known as sulfonated polyphenylene sulfone (PPSU) (Formula Ig).

[0160] In another particularly preferred embodiment, Ar = 1,4-phenylene, t = 1, q = 0, T = C (CH3) 2 and Y = SO2. Particularly preferred sulfonated poly (arylene ether sulfone) polymers (A) formed from the above repeating units are known as sulfonated polysulfones (PSU) (Formula Ia).

[0161] In another particularly preferred embodiment, Ar = 1,4-phenylene, t = 1, q = 0, T = Y = SO2. A particularly preferred sulfonated poly(arylene ether sulfone) polymer (A) formed from the above repeating units is known as sulfonated poly(ether sulfone) (PESU) (Formula Ik).

[0162] In the context of the present invention, abbreviations such as PPSU, PESU and PSU correspond to DIN EN ISO 1043-1 (Plastics - Symbols and abbreviated terms - Part 1: Base polymers and their special characteristics (ISO 1043-1:2001); German version EN ISO 1043-1:2002).

[0163] In a preferred embodiment, the sulfonated poly(arylene ether sulfone) polymer (sP) according to component (A) is a copolymer formed from poly(ether sulfone) (PESU) units and poly(phenylene sulfone) (PPSU) units, wherein at least one unit comprises an arylene group substituted with at least one -SO2X group, wherein X is selected from Cl and O in combination with a cation equivalent. - The group consisting of cations whose equivalent is H + , Li + 、Na + , K + Mg 2+ , Ca 2+ or NH4 + The copolymer may be, for example, a random copolymer or a block copolymer. Preferred are random copolymers formed from poly(ether sulfone) (PESU) and poly(phenylene sulfone) (PPSU) because a more homogeneous material is obtained which shows little or no phase separation in the dissolved or solid state.

[0164] In the case where the sulfonated poly(arylene ether sulfone) polymer (sP) according to component (A) is a copolymer formed from poly(ethersulfone) (PESU) units and poly(phenylene sulfone) (PPSU) units, the sulfonated poly(arylene ether sulfone) polymer (sP) comprises in the range of 1 mol % to 20 mol % of poly(phenylene sulfone) (PPSU) units and in the range of 80 mol % to 99 mol % of poly(ethersulfone) (PESU) units, based in each case on the sum of all repeating units of component (A).

[0165] In a particularly preferred embodiment, the sulfonated poly(arylene ether sulfone) polymer (sP) comprises formula (III)

[0166]

[0167] and / or units of formula (IV)

[0168]

[0169] Therefore, another object of the present invention is a process wherein the sulfonated poly(arylene ether sulfone) polymer (sP) comprises units of formula (III)

[0170]

[0171] and / or units of formula (IV)

[0172]

[0173] In a preferred embodiment, the sulfonated poly(arylene ether sulfone) polymer (sP) comprises units of formula (V)

[0174]

[0175] i) having a number average molecular weight (M) of 10000 g / mol to 35000 g / mol N ), and / or

[0176] ii) comprises an arylene group substituted with at least one -SO3X group, wherein X is selected from H + , Li + 、Na + , K + Mg 2+ , Ca 2+ or NH4 + The group of cationic equivalents

[0177] iii) x is in the range of 0.01 to 1, preferably in the range of 0.02 to 0.5, more preferably in the range of 0.04 to 0.4 and x+k is 1.

[0178] The sum of "x" and "k" equals 1.

[0179] In another particularly preferred embodiment, the sulfonated poly(arylene ether sulfone) polymer (sP) comprises units of formula (V)

[0180]

[0181] Therefore, another object of the present invention is a process wherein the sulfonated poly(arylene ether sulfone) polymer (sP) comprises units of formula (V)

[0182]

[0183] The sulfonated poly(arylene ether sulfone) polymer (sP) may also comprise units of formula (III) and / or formula (IV) and / or formula (V).

[0184] The sulfonated poly(arylene ether sulfone) polymer (sP) preferably has a number average molecular weight (M) of 10000 g / mol to 35000 g / mol. N ), which was determined by gel permeation chromatography in dimethylacetamide as solvent relative to narrow distribution polymethyl methacrylate as standard.

[0185] Therefore, another object of the present invention is a process, wherein the sulfonated poly(arylene ether sulfone) polymer (sP) has a number average molecular weight (M) of 10000 g / mol to 35000 g / mol. N ).

[0186] Furthermore, the sulfonated poly(arylene ether sulfone) polymer (sP) preferably has a free acid content of less than 3 mg KOH / g sulfonated poly(arylene ether sulfone) polymer (sP) as determined by titration with 0.1 mol / l tetrabutylammonium hydroxide solution (TBAH in methanol / toluene) against a Solvotrode 30 electrode (Metrohm).

[0187] Therefore, another object of the present invention is a process, wherein the sulfonated poly(arylene ether sulfone) polymer (sP) has a free acid content of less than 3 mg KOH / g sulfonated poly(arylene ether sulfone) polymer (sP).

[0188] The sulfonated poly(arylene ether sulfone) polymer (sP) can be prepared by any method known to those skilled in the art.

[0189] Preferably, the sulfonated poly(arylene ether sulfone) polymer (sP) is prepared by treating a non-sulfonated poly(arylene ether sulfone) polymer with at least one sulfonating agent. The at least one sulfonating agent is suitably any compound known to those skilled in the art that is capable of introducing at least one SO2X group into the aromatic ring of the non-sulfonated poly(arylene ether sulfone) polymer, wherein X is Cl or O in combination with one cation equivalent. - , where the cation equivalent is H + , Li + 、Na + , K + Mg 2+ , Ca 2+ or NH4 + The SO2X group is preferably a sulfonic acid group (-SO3H) or a group that can react with water to form a sulfonic acid group. This type of group is known to those skilled in the art and includes, for example, a chlorosulfonyl group (-SO2Cl). Therefore, the SO2X group is more preferably a sulfonic acid group (-SO3H) or a chlorosulfonyl group (-SO2Cl), and most preferably the SO2X group is a sulfonic acid group (-SO3H).

[0190] The reaction of the non-sulfonated poly(arylene ether sulfone) polymer with the at least one sulfonating agent preferably at least partially sulfonates at least one of the aromatic rings of the non-sulfonated poly(arylene ether sulfone) polymer.

[0191] The mechanism of the sulfonation reaction is known per se to the person skilled in the art. Thus, it is particularly preferred for the sulfonation reaction to replace the hydrogen atoms of the aromatic ring with sulfonic acid groups (-SO3H).

[0192] Typically, 0.001 to 1, preferably 0.005 to 0.1, and more preferably 0.01 to 0.08 SO2X groups are introduced into the non-sulfonated poly(arylene ether sulfone) polymer per aromatic ring. Therefore, the sulfonated poly(arylene ether sulfone) polymer (sP) typically has 0.001 to 1, preferably 0.005 to 0.1, and more preferably 0.01 to 0.08 sulfonic acid groups per aromatic ring.

[0193] The number of SO2X groups per aromatic ring is determined by dividing the average by all aromatic rings of the sulfonated poly(arylene ether sulfone) polymer (sP). To this end, the number of SO2X groups in the sulfonated poly(arylene ether sulfone) polymer (sP) is divided by the number of aromatic rings in the sulfonated poly(arylene ether sulfone) polymer (sP). Methods for determining the number of SO2X groups and the number of aromatic rings in the sulfonated poly(arylene ether sulfone) polymer (sP) are known to those skilled in the art. The determination can be performed, for example, by acid-base titration or by spectroscopic methods such as H 1 The number of SO2X groups can be determined by NMR spectroscopy or IR spectroscopy (infrared spectroscopy). Sulfonated aromatic polymers with SO2X groups on the aromatic rings show characteristic peaks and bands, making it possible to determine the number of SO2X groups per aromatic ring in the sulfonated poly(arylene ether sulfone) polymer (sP). These methods, in particular by H 1 NMR spectroscopy was used to determine the ratio of sulfonated to non-sulfonated aromatic rings.

[0194] When the non-sulfonated poly(arylene ether sulfone) polymers have aromatic rings whose degree of substitution differs, it is therefore generally the case that the most nucleophilic aromatic ring is preferentially sulfonated.

[0195] Component (B)

[0196] The solution (S) includes a non-sulfonated poly(arylene sulfone) polymer (P) as component (B). In this case, the terms "non-sulfonated poly(arylene sulfone) polymer (P)" and "component (B)" are used synonymously and thus have the same meaning.

[0197] In this case, the term "non-sulfonated poly(arylene sulfone) polymer (P)" is understood to mean exactly one non-sulfonated poly(arylene sulfone) polymer (P) and also mixtures of two or more non-sulfonated poly(arylene sulfone) polymers (P).

[0198] In the context of the present invention, "non-sulfonated" means that the non-sulfonated poly(arylene sulfone) polymer (P) does not include any -SO2X groups, wherein X is selected from Cl and O in combination with one cation equivalent. - Composed of groups.

[0199] In the context of the present invention, "a cation equivalent" means a cation of a single positive charge or a charge equivalent of a cation with two or more positive charges, for example H + , Li + 、Na + , K + Mg 2+ , Ca 2+ or NH4 + .

[0200] Preferably, the non-sulfonated poly(arylene sulfone) polymer (P) comprises units of formula (II)

[0201]

[0202] in

[0203] t and q: each independently 0, 1, 2 or 3,

[0204] Q, T and Y: each independently a chemical bond or selected from -O-, -S-, -SO2-, -(S=O)-, -(C=O)-, -N=N- and -CR a R b - a group in which R a and R b are independently a hydrogen atom or a C1-C 12 -alkyl, C1-C 12 -alkoxy or C6-C 18 -aryl group, and wherein at least one of Q, T and Y is -SO2- and

[0205] Ar, Ar 1 : are each independently an arylene group having 6 to 18 carbon atoms.

[0206] Therefore, another object of the present invention is a process in which the non-sulfonated poly(arylene sulfone) polymer (P) comprises units of formula (II)

[0207]

[0208] in

[0209] t and q: each independently 0, 1, 2 or 3,

[0210] Q, T and Y: each independently a chemical bond or selected from -O-, -S-, -SO2-, -(S=O)-, -(C=O)-, -N=N- and -CR a R b - a group in which R a and R bare independently a hydrogen atom or a C1-C 12 -alkyl, C1-C 12 -alkoxy or C6-C 18 -aryl group, and wherein at least one of Q, T and Y is -SO2- and

[0211] Ar, Ar 1 : are each independently an arylene group having 6 to 18 carbon atoms.

[0212] Among the above conditions, if Q, T or Y is a chemical bond, this should be understood to mean that the adjacent group on the left and the adjacent group on the right are directly bonded to each other via a chemical bond. However, preferably, Q, T and Y in formula (II) are each independently selected from -O and -SO2-, provided that at least one of the group consisting of Q, T and Y is -SO2-.

[0213] If Q, T or Y is -CR a R b -, then R a and R b are independently a hydrogen atom or a C1-C 12 -alkyl, C1-C 12 -alkoxy or C6-C 18 - an aryl group.

[0214] Preferred C1-C 12 -Alkyl groups include straight-chain and branched saturated alkyl groups having 1 to 12 carbon atoms. The following radicals should be mentioned in particular: C1-C6-alkyl radicals such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, 2- or 3-methylpentyl, and longer chain radicals such as unbranched heptyl, octyl, nonyl, decyl, undecyl, lauryl and their mono- or poly-branched analogs.

[0215] Available C1-C above 12 The alkyl radicals that can be used in the -alkoxy group include the alkyl radicals having 1 to 12 carbon atoms as defined above. The cycloalkyl radicals that can be preferably used include in particular C3-C 12 -cycloalkyl radicals, for example cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclopropylmethyl, cyclopropylethyl, cyclopropylpropyl, cyclobutylmethyl, cyclobutylethyl, cyclopentylethyl, -propyl, -butyl, -pentyl, -hexyl, cyclohexylmethyl, -dimethyl and -trimethyl.

[0216] Ar and Ar 1 Each independently is C6-C 18-arylene group. Ar is preferably derived from an electron-rich aromatic substance susceptible to electrophilic attack, preferably selected from the group consisting of hydroquinone, resorcinol, dihydroxynaphthalene, especially 2,7-dihydroxynaphthalene and 4,4'-bisphenol. Preferably, Ar 1 is unsubstituted C6- or C 12 -Arylene group.

[0217] Available C6-C 18 -Arylene groups Ar and Ar 1 Particularly included are phenylene groups such as 1,2-, 1,3- and 1,4-phenylene, naphthylene groups such as 1,6-, 1,7-, 2,6- and 2,7-naphthylene, and arylene groups derived from anthracene, phenanthrene and naphthacene.

[0218] Preferably, in a preferred embodiment, Ar and Ar of formula (II) 1 Each is independently selected from the group consisting of 1,4-phenylene, 1,3-phenylene, naphthylene, especially 2,7-dihydroxynaphthylene and 4,4'-biphenylene.

[0219] Preferred non-sulfonated poly(arylene sulfone) polymers (P) are those comprising as recurring structural unit at least one of the units la to lo as defined above.

[0220] In addition to the preferred units Ia to Io, preference is also given to those units in which one or more 1,4-phenylene units derived from hydroquinone are replaced by 1,3-phenylene units derived from resorcinol or by naphthylene units derived from dihydroxynaphthalene.

[0221] Particularly preferred units of the general formula (II) are units Ia, Ig and Ik. It is also particularly preferred that the non-sulfonated poly(arylene sulfone) polymer (P) of component (B) consists essentially of one unit of the units of the general formula (II), in particular of units selected from the group consisting of Ia, Ig and Ik.

[0222] In a particularly preferred embodiment, Ar = 1,4-phenylene, t = 1, q = 0, T is a chemical bond and Y = SO2. A particularly preferred non-sulfonated poly(arylene sulfone) polymer (B) formed from the above repeating units is known as poly(phenylene sulfone) (PPSU) (Formula Ig).

[0223] In another particularly preferred embodiment, Ar = 1,4-phenylene, t = 1, q = 0, T = C (CH3) 2 and Y = SO2. Particularly preferred non-sulfonated poly (arylene sulfone) polymers (B) formed from the above repeating units are known as polysulfones (PSU) (Formula Ia).

[0224] In another particularly preferred embodiment, Ar = 1,4-phenylene, t = 1, q = 0, T = Y = SO2. A particularly preferred non-sulfonated poly(arylene sulfone) polymer (B) formed from the above repeating units is known as poly(ether sulfone) (PESU) (Formula Ik).

[0225] Therefore, another object of the present invention is a process wherein the non-sulfonated poly(arylene sulfone) polymer (P) is

[0226] i) poly(ethersulfone) and comprising units of formula (1k)

[0227] or

[0228] ii) polysulfone and comprising units of formula (Ia)

[0229] or

[0230] iii) polyphenylene sulfone and comprising units of formula (Ig)

[0231]

[0232] The non-sulfonated poly(arylene ether sulfone) polymer preferably has a weight average molecular weight M of 10000 g / mol to 150000 g / mol, especially 15000 g / mol to 120000 g / mol, more preferably 18000 g / mol to 100000 g / mol. w , was determined using gel permeation chromatography in dimethylacetamide solvent relative to narrow distribution polymethyl methacrylate as a standard.

[0233] The preparation processes for obtaining the above-mentioned non-sulfonated poly(arylene sulfone) polymers are known per se to the person skilled in the art and are described, for example, in Herman F. Mark, “Encyclopedia of Polymer Science and Technology”, 3rd edition, volume 4, 2003, chapter “Polysulfones”, pages 2 to 8 and in Hans R. Kricheldorf, “Aromatic Polyethers” in Handbook of Polymer Synthesis, 2nd edition, 2005, pages 427 to 443.

[0234] Particularly preferred is the reaction of at least one aromatic compound having two halogen substituents with at least one aromatic compound having two functional groups reactive toward the above halogen substituents in an aprotic polar solvent in the presence of anhydrous alkali metal carbonates, in particular sodium carbonate, potassium carbonate or calcium carbonate or mixtures thereof, very particularly preferably potassium carbonate. A particularly suitable combination is N-methyl-2-pyrrolidone as solvent and potassium carbonate as base.

[0235] The present invention is more particularly illustrated by the following examples without being restricted thereto. Example

[0236] Components used

[0237] Sulfonated poly(arylene ether sulfone) polymer :

[0238] Synthesis of sulfonated polyethersulfone-polyphenylsulfone copolymer: sP1 (component (A1)) :

[0239] 1) Synthesis of polyethersulfone-polyphenylsulfone copolymer

[0240] In a 4-liter glass reactor equipped with a thermometer, an air inlet and a Dean-Stark separator, 574.34 g (2.0 mol) of 4,4′-dichlorodiphenyl sulfone (DCDPS) with a volume average particle size of 33.2 μm, 475.53 g (1.90 mol) of 4,4′-dihydroxydiphenyl sulfone (DHDPS), 18.621 g (0.10 mol) of 4,4′-bisphenol and 297.15 g (2.15 mol) of potassium carbonate were suspended in a nitrogen atmosphere in 1050 mL of NMP (N-methyl-2-pyrrolidone; CAS 872-50-4). The mixture was heated to 190° C. within one hour. In the following, the reaction time is understood to be the time during which the reaction mixture is kept at 190° C. The water formed in the reaction is continuously removed by distillation. The evaporated solvent is replaced. After a reaction time of 7 hours, the reaction is stopped by adding 1950 mL of NMP and cooling to room temperature (within one hour). The potassium chloride formed in the reaction was removed by filtration. The poly(ethersulfone) solution obtained was then precipitated in water, the resulting poly(ethersulfone) beads were isolated and then extracted with hot water (85° C.) for 20 h. The beads were then dried at 120° C. under reduced pressure (<100 mbar) for 24 h.

[0241] The presence of 4,4′-bisphenol-derived units in the copolymer was confirmed by 1H-NMR spectroscopy. The obtained poly(ether phenylene sulfone) had a glass transition temperature (T G ), viscosity number of 82.1mL / g, molecular weight M of 74450g / mol w(GPC in THF, PS standard) and a polydispersity of 3.6 MW / M N .

[0242] 2) Synthesis of sulfonated polyethersulfone-polyphenylenesulfone copolymer

[0243] Sulfuric acid (96%) is provided from a reservoir to the reaction vessel in an amount required to provide a solution with a target sulfonated poly(ether sulfone) concentration of 8 wt%. The temperature of the sulfuric acid is set to the sulfonation temperature. 50 kg of the poly(ether sulfone) obtained above is dosed to the mixture within 10 to 30 minutes. The reaction mixture is stirred for an additional 90 minutes to completely dissolve the poly(ether sulfone). The reaction mixture is then stirred for an additional 90 minutes. In a reservoir equipped with an agitator and having a wall temperature of 15°C, liquid L1 is prepared from 3125 L of deionized water and nitric acid so that the concentration of nitric acid in liquid L1 is 0.27 wt%, based on liquid L1.

[0244] As a dynamic in-line mixing device, a single-stage rotor-stator gear disperser with a concave rotor ( CD1010 with conical mixing system; Verfahrenstechnik v. Hagen & Funke GmbH, Germany ). The dynamic inline mixing device is used as a pump because it is operated at a maximum rotational speed of up to 12000 rpm. It draws liquid L1 from the reservoir, whereby the inline mixing device operates in a recirculation loop operation. While the three-way valve is set to the sulfuric acid reservoir, the gear pump is started to pump sulfuric acid to the dynamic inline mixer and flush the pipeline while doing so. After the connecting pipeline is cleaned with sulfuric acid, the corresponding sulfonated poly(ether sulfone) solution is fed to the dynamic inline mixing device by the following operation: the three-way valve is opened toward the reaction vessel containing the sulfonated poly(ether sulfone) solution and pumped into the dynamic inline mixer. After the corresponding sulfonated poly(ether sulfone) solution is contacted with liquid L1, a suspension is obtained. The suspension is recycled into the reservoir of liquid L1, whereby its solid content is continuously increased. In order to avoid sedimentation, the suspension is stirred in the reservoir. Liquid L1 and the suspension are respectively passed through the dynamic inline mixing device in an amount of about 75 L / min. The temperature of the suspension in the reservoir is monitored. During this process, the temperature of the suspension rises by 30° C. to 35° C. The suspension is recirculated until the corresponding sulfonated poly(ethersulfone) solution is used up. The pipes are then rinsed with sulfuric acid.

[0245] The suspension is filtered through a Nutsche, whereby a pressure of 1 bar is applied. A filter with a nominal pore size of 10 μm is used. The filter cake is washed with about 800 L of deionized water, wherein a temperature of about 40° C. is used for each wash. The washing is interrupted as soon as the filtrate water has a pH of 4 or higher. Typically, no more than six washes are performed. The corresponding sulfonated poly(ether sulfone) obtained is then dried under vacuum at 55° C. to 60° C. in a Nutsche before a residual water content of less than 2% by weight, based on the weight of the sulfonated poly(ether sulfone) is obtained.

[0246] The sulfonated polyethersulfone polymer has a viscosity number of 86.3 mL / g, a molecular weight Mw of 72400 g / mol (GPC in THF, PS standard), MW / M N =3.6 polydispersity and ion exchange capacity IEC of 0.210 meq / g.

[0247] Synthesis of sulfonated polyphenylene sulfone: sP2 (component (A2)) :

[0248] In a 4-liter glass reactor equipped with a thermometer, an inlet tube and a Dean-Stark water separator, 557.09 g (1.94 mol) of 4,4′-dichlorodiphenyl sulfone (DCDPS; CAS 80-07-9), 372.42 g (2.00 mol) of 4,4′-dihydroxydiphenyl sulfone (DHDPS; CAS 92-88-6), 70.15 g (0.1428 mol) of bis-(4-chloro-3-sulfophenyl)-sulfone disodium salt (sDCDPS; CAS 51698-33-0) and 317.83 g (2.3 mol) of potassium carbonate (volume average particle size of 33.2 μm) were suspended in 1250 mL of NMP (N-methyl-2-pyrrolidone; CAS 872-50-4) in a nitrogen atmosphere. The mixture was heated to 190° C. in one hour. Hereinafter, the reaction time is understood to be the time during which the reaction mixture is maintained at 190°C. The water formed in the reaction is continuously removed by distillation. The evaporated solvent is replaced. After a reaction time of 7 hours, the reaction is stopped by adding 500 mL of NMP and cooling to room temperature (within one hour). The potassium chloride formed in the reaction is removed by filtration. The sulfonated poly(phenylene sulfone) solution obtained is then precipitated in water, the resulting sPPSU beads are separated, and then extracted with hot water (85°C) for 20 hours. The beads are then dried at 120°C for 24 hours under reduced pressure (<100 mbar).

[0249] The presence of 5.3 mol% of sulfonated units derived from disodium-bis-(4-chloro-3-sulfophenyl)-sulfone units (x=0.053) in the copolymer was confirmed by 1H-NMR spectroscopy. The obtained sulfonated polyphenylene sulfone had a viscosity number of 62.7 mL / g and a calculated ion exchange capacity IEC of 0.260 meq / g.

[0250] P(component (B)) :

[0251] Non-sulfonated poly(arylene sulfone) polymers :

[0252] Poly(ethersulfone)

[0253] E 6020P; BASF SE; Viscosity number: 81cm 3 / g (determined according to ISO 307; in 0.01 g / mL phenol / 1,2-o-dichlorobenzene 1:1 solution); glass transition temperature T G : 225°C (determined according to ISO 11357-1 / -2, DSC, 10°C / min); molecular weight Mw: 75000 g / mol (determined by GPC in THF, PS standard); polydispersity MW / M N :3.4

[0254] Pore-forming additive (component (C1)) :

[0255] Poly(vinyl pyrrolidone)

[0256] K90; BASF SE; molecular weight Mw>900000 g / mol; solution viscosity is characterized by a K value of 90 (determined according to the method of Fikentscher (Fikentscher, Cellulosechemie 13, 1932 (58)))

[0257] Pore-forming additive (component (C2)) :

[0258] Glycerol; Propane-1,2,3-triol [CAS 56-81-5]

[0259] Solvent (component (D)) :

[0260] NMP; N-methyl-2-pyrrolidone [CAS 872-50-4]

[0261] General Procedures

[0262] Pure Water Permeability (PWP)

[0263] The pure water permeability (PWP) of the membrane was tested using ultrapure water (no salt water, filtered through a Millipore UF system) at 23°C and 1 bar water pressure using a pressure cell with a diameter of 74 mm. The pure water permeability (PWP) was calculated as follows (Formula 1):

[0264]

[0265] PWP: Pure water permeability [kg / bar h m2]

[0266] m: Mass of permeate water [kg]

[0267] A: membrane area [m2]

[0268] P: Pressure [bar]

[0269] t: time of penetration experiment [h].

[0270] More than 50kg / hm 2 A high PWP of bar allows for high flow rates and is desirable.

[0271] MWCO (Molecular Weight Cut-off)

[0272] In subsequent tests, solutions of polyethylene oxide standards with increasing molecular weight were used as feed to filter through the membrane at a pressure of 0.15 bar. The molecular weight of the permeate for each polyethylene oxide standard used was determined by gel permeation chromatography (GPC) measurement of the feed and the permeate. The membrane's weight average molecular weight cut-off (Mw) was 1.3 wt % (MW) and the ... w ) (MWCO) is the molecular weight of a first polyethylene oxide standard of which at least 90% is retained by the membrane. For example, a MWCO of 18400 means that polyethylene oxides of molecular weight 18400 g / mol and above are retained at least 90%. It is desirable to have a MWCO in the range of 5 kDa to 100 kDa.

[0273] Viscosity

[0274] The polymer solution viscosity was measured with a Brookfield viscometer DV-I Prime (Brookfield Engineering Laboratories, Inc., Middleboro, USA) using an RV 6 spindle at 60°C and 20 rpm.

[0275] Turbidity

[0276] The polymer solution turbidity was measured with a turbidimeter 2100AN (Hach Lange GmbH, Düsseldorf, Germany) using an 860 nm filter at 60° C. and expressed in nephelometric turbidity units (NTU). Low NTU values ​​are preferred.

[0277] PVP 总 and PVP 表面

[0278] The poly(vinyl pyrrolidone) content (PVP) of the films was determined by dissolving the film sample in N,N-dimethylformamide (DMF) and casting the solution as a thin film on a thallium bromide KRS-5 window. 总 The films were dried at 160 °C and analyzed using a Nicolet 6700 FT-IR spectrometer (Thermo Fischer Scientific, Waltham, MA, USA). Together with calibration samples of known poly(vinyl pyrrolidone) content, 1680 cm -1 The adsorption band at is used to determine the total poly(vinyl pyrrolidone) content of the membrane sample. The poly(vinyl pyrrolidone) content (PVP 表面 ) was estimated by attenuated infrared spectroscopy (ATR) and a reference sample using the same absorption band.

[0279] Membrane preparation

[0280] Comparative Example C1-M

[0281] As shown in Table 1, 19 g of non-sulfonated polyethersulfone (component (B)), 6 g of poly(vinyl pyrrolidone) (component (C1)), 10 g of glycerol (component (C2)) and 65 g of NMP (component (D)) were added to a three-necked flask equipped with a magnetic stirrer. The mixture was heated at 60° C. under gentle agitation until a uniform, clear, viscous solution (S) was obtained. The solution (S) was degassed overnight at room temperature. Then, the solution (S) was reheated at 60° C. for 2 hours and cast onto a glass plate with a casting knife (300 microns) at 60° C. using an Erichsen coater (Coatmaster 510, Erichsen GmbH & Co KG, Heimer, Germany) operating at a speed of 5 mm / s to obtain a film of the solution (S). The film of the solution (S) was left to stand for 30 seconds and then immersed in a 25° C. water-based coagulation bath (60 wt % water / 40 wt % NMP) for 10 minutes to obtain a membrane (M1). After the film (M1) was detached from the glass plate, the film (M1) was transferred to a bath containing 2000 ppm NaOCl at 60°C and pH 9.5 for 2 hours. Subsequently, the film (M1) was washed with water at 60°C to obtain a film (M), and washed once with a 0.5 wt% sodium bisulfite solution to remove active chlorine.

[0282] Embodiments I2-M to I5-M of the present invention

[0283] A sulfonated poly(ethersulfone) polymer (component (A1)) and a non-sulfonated poly(ethersulfone) (component (B)) in the amounts given in Table 1, 6 g of poly(vinylpyrrolidone) (component (C1)), 10 g of glycerol (component (C2)) and 65 g of NMP (component (D)) were added to a three-necked flask equipped with a magnetic stirrer. The mixture was heated at 60° C. with gentle agitation until a uniform, clear, viscous solution (S) was obtained (step a)). The solution (S) was degassed overnight at room temperature. Then, the solution (S) was heated at 60° C. for another 2 hours and cast onto a glass plate using an Erichsen coater (Coatmaster 510, Erichsen GmbH & CoKG, Heimer, Germany) operating at a speed of 5 mm / s with a casting knife (300 microns) at 60° C. to obtain a thin film of the solution (S) (step b-1)). The film of solution (S) was left to stand for 30 seconds and then immersed in a 25°C water-based coagulation bath (60 wt% water / 40 wt% NMP) for 10 minutes to obtain a membrane (M1) (step b-2)). After the membrane (M1) was detached from the glass plate, the membrane (M1) was transferred to a bath containing 2000 ppm NaOCl at 60°C and pH 9.5 for 2 hours. Subsequently, the membrane (M1) was washed with water at 60°C to obtain a membrane (M) (step b-3)), and washed once with a 0.5 wt% sodium bisulfite solution to remove active chlorine.

[0284] The compositions and properties of the solutions (S) and the prepared membranes (M) are shown in Table 1.

[0285] Table 1

[0286]

[0287] As can be seen from Table 1, the membranes (M) (I2-M to I5-M) of the present invention all show a 50 kg / hm 2 bar to 600kg / hm 2 bar and a MWCO of 11.2 kDa to 30 kDa. As the content of sulfonated poly(ethersulfone) polymer (component (A)) increases, the membrane (M) of the present invention exhibits an increased PVP content (PVP 总 and PVP 表面 ), which means that the membrane (M) of the present invention retains PVP in the membrane matrix and thus prevents PVP from leaching out of the membrane matrix.

[0288] Figure 1 shows a cross section of a membrane of Example I2-M of the invention, and Figure 2 shows a cross section of a membrane of Comparative Example C1-M (magnified 1500 times). As can be seen from the figures, the membrane according to the invention shows a well-constructed nanoporous filtration layer without defects or macropores. The membrane according to Comparative Example C1-M shows many macropores and defects that can partially penetrate the top filtration layer.

[0289] Embodiments I6-M to I8-M of the present invention

[0290] A sulfonated poly(phenylene sulfone) polymer (component (A2)) and a non-sulfonated poly(ether sulfone) (component (B)) in the amounts given in Table 2, 6 g of poly(vinyl pyrrolidone) (component (C1)), 10 g of glycerol (component (C2)) and 65 g of NMP (component (D)) were added to a three-necked flask equipped with a magnetic stirrer. The mixture was heated at 60° C. with gentle agitation until a uniform, clear, viscous solution (S) was obtained (step a)). The solution (S) was degassed overnight at room temperature. Then, the solution (S) was heated at 60° C. for another 2 hours and cast onto a glass plate using an Erichsen coater (Coatmaster 510, Erichsen GmbH & CoKG, Heimer, Germany) operating at a speed of 5 mm / s with a casting knife (300 microns) at 60° C. to obtain a thin film of the solution (S) (step b-1)). The film of solution (S) was left to stand for 30 seconds and then immersed in a 25°C water-based coagulation bath (60 wt% water / 40 wt% NMP) for 10 minutes to obtain a membrane (M1) (step b-2)). After the membrane (M1) was detached from the glass plate, the membrane (M1) was transferred to a bath containing 2000 ppm NaOCl at 60°C and pH 9.5 for 2 hours. Subsequently, the membrane (M1) was washed with water at 60°C to obtain a membrane (M) (step b-3)), and washed once with a 0.5 wt% sodium bisulfite solution to remove active chlorine.

[0291] The compositions and properties of the solutions (S) and the prepared membranes (M) are shown in Table 2.

[0292] Table 2

[0293]

[0294] As can be seen from Table 2, the membranes (M) (I6-M to I10-M) of the present invention all show a 50 kg / hm 2 bar to 600kg / hm 2 bar and a MWCO of 10.7 kDa to 28 kDa. With the increase of the content of sulfonated poly(phenylene ether sulfone) polymer (component (A2)), the membrane (M) of the present invention shows an increased PVP content (PVP 总 and PVP表面 ), which means that the membrane (M) of the present invention retains PVP in the membrane matrix and thus prevents PVP from leaching out of the membrane matrix.

Claims

1. A method for preparing a film (M), the film (M) comprising (A) sulfonated poly(arylene ether sulfone) polymer (sP) and (B) a non-sulfonated poly(arylene sulfone) polymer (P), The method comprises at least steps a) and b): a) providing a solution (S), said solution (S) comprising said sulfonated poly(arylene ether sulfone) polymer (sP) according to component (A), said non-sulfonated poly(arylene sulfone) polymer (P) according to component (B), at least one pore-forming additive (C) and at least one solvent (D), wherein said at least one pore-forming additive (C) comprises poly(vinyl pyrrolidone); and b) separating said at least one pore-forming additive (C) and said at least one solvent (D) from said solution (S) to obtain said membrane (M), wherein the solution (S) in step a) comprises 0.5 to 20 wt.-% of the sulfonated poly(arylene ether sulfone) polymer (sP), 0.5 to 20 wt.-% of the non-sulfonated poly(arylene sulfone) polymer (P), 3 to 20 wt.-% of the at least one pore-forming additive (C) and 40 to 96 wt.-% of the at least one solvent (D), in each case based on the total weight of the solution (S).

2. The method according to claim 1, wherein the sulfonated poly(arylene ether sulfone) polymer (sP) comprises units of formula (I) in t and q: each independently 0, 1, 2 or 3, Q, T and Y: each independently a chemical bond or selected from -O-, -S-, -SO2-, -S(=O)-, -(C=O)-, -N=N- and -CR a R b -, wherein Ra and Rb are each independently a hydrogen atom or a C1-C 12 Alkyl, C1-C 12 Alkoxy or C6-C 18 An aryl group, and wherein at least one of Q, T and Y is -SO2- and Ar and Ar1: each independently an arylene group having 6 to 18 carbon atoms And among them At least one unit (I) comprises an arylene group substituted with at least one -SO2X group, wherein X is selected from Cl and O in combination with a cation equivalent. - The group consisting of wherein the cation equivalent is H + , Li + 、Na + , K + Mg 2+ , Ca 2+ or NH4 + .

3. The method according to claim 1 or 2, wherein the sulfonated poly(arylene ether sulfone) polymer (sP) i) comprising a unit of formula (III) and / or units of formula (IV) and / or ii) having a number average molecular weight (M) of 10000 g / mol to 35000 g / mol N ), and / or iii) Sulfonated poly(arylene ether sulfone) polymers (sP) having a free acid content of less than 3 mg KOH / g.

4. The method according to claim 1 or 2, wherein the sulfonated poly(arylene ether sulfone) polymer (sP) comprises units of formula (V) i) having a number average molecular weight (M) of 10000 g / mol to 35000 g / mol N ), and / or ii) comprises an arylene group substituted with at least one -SO3X group, wherein X is selected from H + , Li + 、Na + , K + Mg 2+ , Ca 2+ or NH4 + The group of cationic equivalents iii) x is in the range of 0.01 to 1 and x+k is 1.

5. The method according to any one of claims 1 to 4, wherein the non-sulfonated poly(arylene sulfone) polymer (P) comprises units of formula (II) in t and q: each independently 0, 1, 2 or 3, Q, T and Y: each independently a chemical bond or selected from -O-, -S-, -SO2-, -(S=O)-, -(C=O)-, -N=N- and -CR a R b - a group in which R a and R b are independently a hydrogen atom or a C1-C 12 -alkyl, C1-C 12 -alkoxy or C6-C 18 -aryl group, and wherein at least one of Q, T and Y is -SO2- and Ar, Ar 1 : are each independently an arylene group having 6 to 18 carbon atoms.

6. The method according to claim 5, wherein the non-sulfonated poly(arylene sulfone) polymer (P) is i) poly(ethersulfone) and comprising units of formula (1k) or ii) polysulfone and comprising units of formula (Ia) or iii) polyphenylene sulfone and comprising units of formula (Ig) 7. The process according to any one of claims 1 to 6, wherein the at least one solvent (D) is selected from the group consisting of N-alkyl-2-pyrrolidone, preferably N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-butyl-2-pyrrolidone and N-tert-butyl-2-pyrrolidone, 2-pyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, dimethylformamide, N,N-dimethyl-2-hydroxypropaneamide, N,N-diethyl-2-hydroxypropaneamide, γ-valerolactone, dihydrolevoglucose ketone, 5-(dimethylamino)-2-methyl-5-oxopentanoic acid methyl ester and sulfolane.

8. The method according to any one of claims 1 to 7, wherein the at least one pore-forming additive (C) further comprises at least one alcohol, preferably glycerol.

9. The method according to any one of claims 1 to 7, wherein the at least one pore-forming additive (C) consists of poly(vinylpyrrolidone).

10. The method according to any one of claims 1 to 9, wherein step b) comprises the following steps: b-1) casting the solution (S) provided in step a) to obtain a thin film of the solution (S), b-2) immersing the thin film of the solution (S) into at least one protic polar solvent, wherein the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P) included in the thin film of the solution (S) are at least partially separated from the at least one pore-forming additive (C) and the at least one solvent (D) included in the thin film of the solution (S) to obtain a membrane (M1) in the form of a thin film, and b-3) washing the membrane (M1) with water, wherein the sulfonated poly(arylene ether sulfone) polymer (sP) and the non-sulfonated poly(arylene sulfone) polymer (P) included in the membrane (M1) are completely separated from the at least one pore-forming additive (C) and the at least one solvent (D) included in the membrane (M1) to obtain the membrane (M).

11. The method of claim 10, wherein the at least one protic polar solvent is a water-based coagulation bath.

12. The method according to claim 10 or 11, wherein step b-1) is carried out at a temperature ranging from 40°C to 80°C.

13. A film produced by the method according to any one of claims 1 to 12.

14. The film (M) according to claim 13, wherein the film (M) i) is a porous membrane (M), and / or ii) has a molecular weight cut-off in the range of 10 kDa to 30 kDa, and / or iii) has a capacity of >50 kg / (hm 2 bar) and / or iv) is asymmetric, and / or v) having a poly(vinylpyrrolidone) content PVP in the range of 0.8 wt.-% to 5 wt.-%, based on the total weight of the film (M) 总 .

15. The membrane (M) according to claim 13 or 14, wherein the membrane (M) comprises 5 to 90 wt.-% of the sulfonated poly(arylene ether sulfone) polymer (sP), based on the total weight of the membrane (M).